Method for preparing copper interconnect structure
By forming trenches on the surface of the copper layer and depositing a protective gas layer to prevent the entry of etching gas, the problem of hydrogen etching destroying the copper layer structure is solved and the stability of the copper layer performance is ensured.
Patent Information
- Application Number
- CN202210869989.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-22
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-07-22
AI Technical Summary
Hydrogen plasma destroys the crystal structure of the copper layer during the etching of the copper layer, resulting in void defects and degradation of performance.
The first etching is performed using a hard mask layer. After the trench is formed, a protective gas such as nitrogen is deposited to form a protective layer to prevent subsequent etching gas from entering the copper layer lattice structure, and the bottom wall of the trench is continued under the action of an electric field. Avoid etching gas destroying the copper layer structure.
The etching gas is effectively prevented from destroying the lattice structure of the copper layer, preventing the formation of hollow defects, and ensuring the performance of the copper layer.
Smart Images

Figure CN115036218B_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of semiconductor process technology, and specifically relates to a method for preparing a copper interconnect structure. Background Art
[0002] In the field of semiconductor technology, dry etching technology can not only meet the requirements of low dielectric constant thin film etching, but also avoid the defect problem caused by electroplating. In the related technology, hydrogen is used as the main etching gas to etch the copper layer. However, Figure 1 As shown in the figure, during the etching process using hydrogen plasma, due to the small atomic mass of hydrogen, hydrogen atoms will enter the crystal structure of the copper layer during the etching process, and the hydrogen atoms will react with the copper atoms to produce volatiles - copper hydride, and finally the copper layer will be formed. Figure 2 The lattice structure shown, therefore, the etching gas will destroy the crystal structure of the copper layer, which will cause void defects after a long period of accumulation and affect the performance of the copper layer. Summary of the invention
[0003] The purpose of the embodiments of the present application is to provide a method for preparing a copper interconnect structure, which can solve the problem in the related art that hydrogen destroys the crystal structure of the copper layer during the etching process of the copper layer, thereby affecting the performance of the copper layer.
[0004] The present application embodiment provides a method for preparing a copper interconnect structure, comprising a first etching step, a protective layer deposition step, and a second etching step, wherein:
[0005] The first etching step comprises: using the hard mask layer as a mask, etching the surface of the copper layer with an etching gas to form a groove on the surface of the copper layer until the groove reaches a first preset depth, and the etching gas includes hydrogen;
[0006] The protective layer deposition step comprises: depositing a protective gas on the sidewall surface and the bottom wall surface of the groove, so that the protective gas forms a protective layer on the sidewall surface and the bottom wall surface for blocking the etching gas, and the protective gas comprises nitrogen;
[0007] The second etching step is: continue to use the etching gas to etch the bottom wall surface of the groove until the groove reaches a second preset depth, and the second preset depth is greater than the first preset depth.
[0008] In the embodiment of the present application, a protective layer is formed on the sidewall and bottom wall of the groove by using a protective gas, and the protective layer can prevent the plasma of the etching gas for subsequent etching from entering the lattice structure of the copper layer. At the same time, since the protective layer is relatively thin relative to the copper layer, under the action of the electric field, the etching gas can continue to etch the bottom wall of the groove without affecting the subsequent etching process. In this way, the protective layer is used to prevent the etching gas from destroying the lattice structure of the copper layer, avoid causing void defects, and ensure the performance of the copper layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 is a schematic diagram of the lattice structure of the etching gas atoms entering the copper layer disclosed in the related art;
[0010] Figure 2 is a schematic diagram of the lattice structure of the damaged area of the copper layer disclosed in the related art;
[0011] Figure 3 is a flow chart of a method for preparing a copper interconnect structure disclosed in an embodiment of the present application;
[0012] Figure 4 is a cross-sectional view of the copper layer, the hard mask layer and the etching barrier layer disclosed in the embodiment of the present application during the etching process;
[0013] Figure 5 It is a schematic diagram of the side wall surface of the groove disclosed in the embodiment of the present application during the etching process.
[0014] Description of reference numerals:
[0015] 100-copper layer, 110-groove, 111-side wall surface, 112-bottom wall surface,
[0016] 200-protective layer,
[0017] 300-hard mask layer,
[0018] 400-etching stop layer,
[0019] 500-Photoresist layer. DETAILED DESCRIPTION
[0020] The following will be combined with the drawings in the embodiments of the present application to clearly describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all the embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments in the present application belong to the scope of protection of this application.
[0021] The terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable under appropriate circumstances, so that the embodiments of the present application can be implemented in an order other than those illustrated or described here, and the objects distinguished by "first", "second", etc. are generally of one type, and the number of objects is not limited. For example, the first object can be one or more. In addition, "and / or" in the specification and claims represents at least one of the connected objects, and the character " / " generally indicates that the objects associated with each other are in an "or" relationship.
[0022] The following describes in detail the method for preparing the copper interconnect structure provided by the embodiment of the present application through specific embodiments and application scenarios in conjunction with the accompanying drawings.
[0023] Please refer to Figure 3-Figure 5 The method for preparing a copper interconnect structure disclosed in the embodiment of the present application includes a first etching step, a protective layer deposition step and a second etching step.
[0024] S100, the first etching step is: using the hard mask layer 300 as a mask, etching the surface of the copper layer 100 with an etching gas to form a groove 110 on the surface of the copper layer 100 until the groove 110 reaches a first preset depth. The first preset depth is the depth of the groove 110 in the thickness direction of the copper layer 100, and the formed groove 110 can be a regular shape, such as Figure 4 The rectangular groove shown; the groove 110 formed can also be an irregular groove. This step is the basis for the protective layer deposition step and creates conditions for the protective layer deposition step. Optionally, Figure 4 The structure (b) can be formed into the structure (c) by adopting this step, and the first preset depth can be the depth of the groove 110 shown in the structure (c) and the structure (d).
[0025] Optionally, the hard mask layer 300 may be Figure 4 In the structure shown in structure (b), the hard mask layer 300 is provided with an opening, and the etching gas etches the groove 110 on the surface of the copper layer 100 through the opening, so the opening is opposite to the groove 110; the etching gas may include hydrogen. In the embodiment of etching the copper layer using hydrogen plasma, hydrogen ions react with copper to generate a volatile product-copper hydride.
[0026] S200, the protective layer deposition step is: depositing protective gas on the side wall surface 111 and the bottom wall surface 112 of the groove 110, so that the protective gas forms a protective layer 200 for blocking the etching gas on the side wall surface 111 and the bottom wall surface 112 of the groove 110, wherein the protective gas includes nitrogen. Optionally, the protective gas may also include at least one of oxygen and argon. When nitrogen is deposited on the side wall surface 111 and the bottom wall surface 112 of the groove 110, the nitrogen ions react with the copper ions to generate Cu x N y , that is, the protective layer 200 is Cu x N y , the lattice constant is greater than that of copper, and because Cu x N y As a macromolecular byproduct, the lattice structure is relatively complex, so it is difficult for hydrogen atoms to enter the lattice structure of the protective layer 200, and the protective layer 200 has an obstructive effect on the etching gas. Figure 4 The structure (c) can be formed into the structure (d) by adopting this step.
[0027] S300, the second etching step is: continue to use the etching gas to etch the bottom wall surface 112 of the groove 110 until the groove 110 reaches a second preset depth, and the second preset depth is greater than the first preset depth. The second preset depth is the depth of the groove 110 in the thickness direction of the copper layer 100. In the process of etching the bottom wall surface 112 of the groove 110 by the etching gas, the etching gas inevitably contacts the side wall surface 111 of the groove 110, and the protective layer 200 can prevent the atoms of the etching gas in this step from entering the lattice structure of the copper layer 100 from the side wall surface 111 of the groove 110, thereby preventing the etching gas from changing the lattice structure of the copper layer 100, thereby avoiding affecting the performance of the copper layer 100. Optionally, Figure 4 The structure (d) can be formed into the structure (e) by adopting this step, and the second preset depth can be the depth of the groove 110 shown in the structure (e) and the structure (f).
[0028] In the embodiment of the present application, a protective layer 200 is formed on the side wall surface 111 and the bottom wall surface 112 of the groove 110 by using a protective gas. The protective layer 200 can prevent the plasma of the etching gas for subsequent etching from entering the lattice structure of the copper layer 100. At the same time, since the protective layer 200 is relatively thin relative to the copper layer 100, under the action of the electric field, the etching gas can continue to etch the bottom wall surface 112 of the groove 110 without affecting the subsequent etching process. In this way, the protective layer 200 is used to prevent the etching gas from destroying the lattice structure of the copper layer 100, avoid causing void defects, and ensure the performance of the copper layer 100.
[0029] In an optional embodiment, the method for preparing the copper interconnect structure further includes:
[0030] S400 , alternately performing a protective layer deposition step and a second etching step in sequence until the trench 110 reaches a third preset depth, wherein the third preset depth is greater than the second preset depth.
[0031] like Figure 4 As shown, structure (e) can form structure (f) by using a protective layer deposition step, and structure (f) can form structure (g) by using a second etching step, and the third preset depth can be the depth of the groove 110 shown in structure (g). In an optional embodiment, in the method for preparing a copper interconnect structure, the protective layer deposition step and the second etching step are alternated at least three times. Optionally, the third preset depth can be equal to the thickness of the copper layer 100. Specifically, the copper layer 100 is provided with a first surface and a second surface opposite to each other, the groove 110 is opened on the first surface, and the second surface of the copper layer 100 is provided with an etching barrier layer 400. When the etching gas contacts the etching barrier layer 400, it indicates that the depth of the groove 110 reaches the third preset depth. Among them, the etching barrier layer 400 can be a titanium nitride film layer.
[0032] By adopting this embodiment, the entire etching process is divided into a first etching step and at least two second etching steps, that is, divided into multiple etching steps, the etching time of each etching step is relatively short, and the side wall surface 111 and the bottom wall surface 112 of the groove 110 formed in each etching step will deposit protective gas to form a protective layer 200, which can maximize the area of the formed protective layer 200, thereby preventing the atoms of the etching gas in each second etching step from the side wall surface 111 and the bottom wall surface 112 of the groove 110 from entering the lattice structure of the copper layer 100, thereby improving the protection effect of the side wall surface 111 and the bottom wall surface 112 of the groove 110.
[0033] In an optional embodiment, in the next second etching step of the protective layer deposition step, although the etching gas needs to etch the bottom wall surface 112 of the groove 110 and etch away the protective layer 200 opposite to the bottom wall surface 112, the protective layer 200 opposite to the bottom wall surface 112 can also play a role in temporarily blocking the etching gas. Specifically, when the etching gas etches a local area of the bottom wall surface 112, the protective layer 200 at other areas of the bottom wall surface 112 can block the plasma of the etching gas from entering the lattice structure of the copper layer 100, thereby further ensuring the performance of the copper layer 100.
[0034] In an optional embodiment, before etching the surface of the copper layer 100 with the etching gas, the process further includes:
[0035] S500 , etching the hard mask layer 300 disposed on the surface of the copper layer 100 using an etching gas until the etching gas contacts the surface of the copper layer 100 .
[0036] Since the hard mask layer 300 is disposed on the surface of the copper layer 100, the hard mask layer 300 may be etched before etching the copper layer 100 to facilitate the subsequent etching process. Figure 4 As shown, structure (a) can be formed into structure (b) by adopting this step. Optionally, the hard mask layer 300 is an inorganic thin film material generated by chemical deposition, and the material of the hard mask layer can be silicon dioxide or silicon oxynitride. Figure 4 As shown in structure (a), a surface of the hard mask layer 300 facing away from the copper layer 100 may be provided with a patterned photoresist layer 500. In the process of etching the hard mask layer 300 by the etching gas, the photoresist layer 500 is used as a mask. The etching gas passes through the gaps in the photoresist layer 500, and then etches an opening in the hard mask layer 300 that is opposite to the subsequent groove 110.
[0037] In the etching step of the hard mask layer 300, the vacuum degree of the process chamber is 0-300 mTorr, the RF frequency of the upper electrode and the RF frequency of the lower electrode can both be 13.56 MHz, the RF power of the upper electrode is 50-3000 W, and the RF power of the lower electrode is 50-800 W. Under this process condition, the etching gas has a good etching condition so that the etching gas can effectively etch the mask layer 300.
[0038] In an optional embodiment, the etching time of the etching gas in the first etching step or the second etching step is the first time, and the deposition time of the protective gas in the next protective layer deposition step of the first etching step or the second etching step is the second time, and the first time is greater than the second time. This arrangement avoids the protective layer 200 being too thick due to the deposition time being too long, thereby affecting the etching process. Therefore, the first time and the second time meet the above conditions, which is conducive to ensuring the smooth progress of the etching process.
[0039] Optionally, the first duration is at least twice the second duration. In this embodiment, the first duration may be 10s-20s, and the second duration may be 5s-10s.
[0040] In an optional embodiment, the etching gas further includes at least one of helium and argon. In this embodiment, the etching gas is a mixed gas of hydrogen, helium and argon. In this arrangement, at least one of helium and argon is used as a dilution gas to remove byproducts formed during the etching process and improve the etching effect.
[0041] In an optional embodiment, in the first etching step and the second etching step, the vacuum degree of the process chamber is 0-300mTorr, the RF power of the upper electrode is 300-500W, the RF power of the lower electrode is 50-500W, the flow rate of the etching gas is 50sccm-200sccm, and the temperature of the wafer carrier is less than 10°C. Optionally, the vacuum degree of the process chamber can be 5-20mTorr, the RF frequency of the upper electrode and the RF frequency of the lower electrode can both be 13.56MHz; the wafer carrier is an electrostatic chuck, that is, the temperature of the electrostatic chuck is less than 10°C. The upper electrode and the lower electrode here jointly form an electric field, thereby providing etching conditions for the etching step, and the wafer carrier is used to carry the wafer to be etched.
[0042] With such configuration, under the process conditions, the etching gas has good etching conditions, so that the etching gas can effectively etch the copper layer 100 , which is beneficial to improving the etching efficiency.
[0043] In an optional embodiment, in the protective layer deposition step, the vacuum degree of the process chamber is 0-300mTorr, the RF power of the upper electrode is 50-3000W, the RF power of the lower electrode is 50-500W, the flow rate of the protective gas is 50sccm-200sccm, and the temperature of the wafer carrier is less than 10°C. Optionally, the vacuum degree of the process chamber can be 5-20mTorr, the RF frequency of the upper electrode and the RF frequency of the lower electrode can both be 13.56MHz; the RF power of the upper electrode can be 1000-2000W; the flow rate of the protective gas can be 50-100sccm; the wafer carrier is an electrostatic chuck, that is, the temperature of the electrostatic chuck is less than 10°C.
[0044] With such arrangement, under the process conditions, the protective gas has good deposition conditions, so that the protective gas can be effectively deposited on the side wall surface 111 and the bottom wall surface 112 of the groove 110 , which is beneficial to improving the deposition efficiency.
[0045] The embodiments of the present application are described above in conjunction with the accompanying drawings, but the present application is not limited to the above-mentioned specific implementation methods. The above-mentioned specific implementation methods are merely illustrative and not restrictive. Under the guidance of the present application, ordinary technicians in this field can also make many forms without departing from the purpose of the present application and the scope of protection of the claims, all of which are within the protection of the present application.
Claims
1. A method for preparing a copper interconnect structure, characterized in that: The method comprises a first etching step, a protective layer deposition step and a second etching step, wherein: The first etching step comprises: using the hard mask layer (300) as a mask and etching the surface of the copper layer (100) using an etching gas to form a groove (110) on the surface of the copper layer (100), until the groove (110) reaches a first preset depth, the etching gas comprising hydrogen; The protective layer deposition step comprises: depositing protective gas on the side wall surface (111) and the bottom wall surface (112) of the groove (110), so that the protective gas forms a protective layer (200) on the side wall surface (111) and the bottom wall surface (112) for blocking the etching gas, wherein the protective gas comprises nitrogen; The second etching step comprises: continuing to use the etching gas to etch the bottom wall surface (112) of the groove (110) until the groove (110) reaches a second preset depth, wherein the second preset depth is greater than the first preset depth.
2. The method for preparing a copper interconnect structure according to claim 1, characterized in that: The protective layer deposition step and the second etching step are performed alternately in sequence until the groove (110) reaches a third preset depth, wherein the third preset depth is greater than the second preset depth.
3. The method for preparing a copper interconnect structure according to claim 1, characterized in that: The etching time of the etching gas in the first etching step or the second etching step is a first time length, and the deposition time of the protective gas in the next protective layer deposition step of the first etching step or the second etching step is a second time length, and the first time length is greater than the second time length.
4. The method for preparing a copper interconnect structure according to claim 3, characterized in that: The first duration is at least twice as long as the second duration.
5. The method for preparing a copper interconnect structure according to claim 1, characterized in that: The protective gas further comprises at least one of oxygen and argon.
6. The method for preparing a copper interconnect structure according to claim 1, characterized in that: The etching gas further includes at least one of helium and argon.
7. The method for preparing a copper interconnect structure according to claim 1, characterized in that: Before etching the surface of the copper layer (100) with etching gas, the method further comprises: The hard mask layer (300) disposed on the surface of the copper layer (100) is etched using the etching gas until the etching gas contacts the surface of the copper layer (100).
8. The method for preparing a copper interconnect structure according to claim 1, characterized in that: In the first etching step and the second etching step, the vacuum degree of the process chamber is 0-300mTorr, the RF power of the upper electrode is 300-500W, the RF power of the lower electrode is 50-500W, the flow rate of the etching gas is 50sccm-200sccm, and the temperature of the wafer carrier is less than 10°C.
9. The method for preparing a copper interconnect structure according to claim 8, characterized in that: The vacuum degree of the process chamber is 5-20 mTorr.
10. The method for preparing a copper interconnect structure according to claim 1, characterized in that: In the protective layer deposition step, the vacuum degree of the process chamber is 0-300mTorr, the RF power of the upper electrode is 50-3000W, the RF power of the lower electrode is 50-500W, the flow rate of the protective gas is 50sccm-200sccm, and the temperature of the wafer carrier is less than 10°C.
11. The method for preparing a copper interconnect structure according to claim 10, characterized in that: The vacuum degree of the process chamber is 5-20 mTorr, the radio frequency power of the upper electrode is 1000-2000 W, and the flow rate of the protective gas is 50 sccm-100 sccm.
Citation Information
Patent Citations
Double-nested copper interconnection structure and fabrication method thereof
CN104112734A
Metal interconnection structure having porous dielectric layer
CN108376676A
Shallow trench isolation structure and preparation method thereof
CN110911342A
Manufacturing method of metal conductive structure
CN113690178A
Metal interconnect layer of semiconductor device and method for forming a metal interconnect layer
US20020050649A1