Method for preparing wide titanium alloy plates by titanium-steel joint mode
Through the hot rolling process of titanium steel combined mode and steel-titanium-clad structure, the problems of difficult and high cost of wide-frame TA5 titanium alloy sheets in the existing technology are solved, efficient production is achieved and the risk of surface cracks is reduced, and the market is met Demand for wider products.
Patent Information
- Application Number
- CN202210771741.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-06-30
AI Technical Summary
The prior art is difficult to effectively produce TA5 titanium alloy sheets with a width of 4-10mm and a width of 1200-1600mm, resulting in high production difficulty, high cost and low material yield, and easy to widen the heat-affected zone during welding and Corrosion problem.
Using the titanium steel joint model, the steel titanium clad structure is made, and the hot rolling and thermal correction process is performed using the steel mill 3800mm rolling mill, gaps and pores are set to reduce deformation resistance and oxide layer formation, and the steel plate is removed after treatment to obtain the target product.
The production of TA5 titanium alloy sheets with wider and thinner specifications has been achieved, which reduces the incidence of surface cracks, increases the yield rate, reduces manufacturing costs, and meets the market's demand for wider products.
Smart Images

Figure CN115041523B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of titanium alloy plate preparation, and in particular to a method for preparing a wide-width titanium alloy plate by adopting a titanium-steel joint mode. Background Art
[0002] Titanium alloys are light (the density of titanium alloys is about half that of steel and other alloys), have high specific strength and excellent corrosion resistance, making them an ideal choice for metal structural materials for ships, and are increasingly used in fields such as marine engineering. With the increasing demand for titanium materials in the shipbuilding field, TA5 titanium alloy (nominal composition is Ti-4Al-0.005B), as a medium-strength α-type titanium alloy, has excellent welding performance, oxidation resistance, high temperature strength and corrosion resistance, and is a good material for ship structures.
[0003] However, due to its good high-temperature strength, TA5 titanium alloy has high deformation resistance during hot rolling and poor processing plasticity. It is very easy to crack during rolling, and even serious cracks may appear on the surface, making it extremely difficult to roll.
[0004] At present, the methods available on the market for producing titanium alloy plates are mainly limited as follows: using the "titanium-steel joint" production model, only titanium alloy plate products with a thickness of more than 10.0 mm can be produced using equipment such as the steel plant's 3800mm rolling mill, and the thickness below 10 mm is limited and cannot be produced; for titanium alloy medium and thick plate products with a thickness of 3-10 mm, hot-rolled plates produced using equipment such as the titanium industry's 1800mm rolling mill can only produce titanium alloy plate products with a width of less than 1200 mm, and the width size is limited.
[0005] Since titanium alloy plate products with narrow width often require a lot of welding in the process of processing into large equipment and parts, not only is the welding process complicated, but also the heat concentration per unit volume during welding will cause the heat affected zone to become wider and the structure and performance to be unstable. At the same time, the weld often becomes a source of corrosion and fracture, which greatly affects the safety and life of the parts. Therefore, the market demand for TA5 titanium alloy medium and thick plate products with wider width and thinner thickness for marine engineering is increasing.
[0006] Currently, there are few equipments on the market that can produce wide-width titanium alloy plate products for marine engineering with a size range of (4-10)*(1200-1600)*Lmm. It is extremely difficult to produce products with wider specifications such as (4-10)*(1200-1600)*Lmm, and surface cracks, edge cracks and other problems are very likely to occur during the rolling process.
[0007] For titanium alloy plate products with a thickness of 4-10mm (except pure titanium products), the current mainstream width specification on the market is 800-1200mm, and the market demand for wider products is becoming more and more vigorous (in the past two years, especially in the military field).
[0008] To achieve wide TA5 titanium alloy sheet products with a size range of (4-10)*(1200-1600)*L mm, the main limitation is related equipment, which increases the difficulty of production. Specifically, during the hot rolling production process, the deformation resistance is large, and serious problems such as surface cracks and cracked edges are very likely to occur, which reduces the yield rate of the product, and the grinding of surface cracks increases its production cycle. Therefore, in order to obtain wide TA5 titanium alloy sheet products with a size of (4-10)*(1200-1600)*L mm, it is urgent to develop a method for preparing wide titanium alloy sheets using a titanium-steel joint mode. Summary of the invention
[0009] The purpose of the present invention is to provide a method for preparing wide-width titanium alloy plates by using a titanium-steel joint mode, which is used to solve the problems of high production difficulty, high cost and low yield rate in the existing process for preparing wide-width titanium alloy plates. The specific technical scheme is as follows:
[0010] A method for preparing a wide titanium alloy plate using a titanium-steel joint mode comprises the following steps:
[0011] Step S1: Making a steel-titanium clad structure
[0012] The lower steel plate that has undergone the first pretreatment is horizontally arranged, the first steel bars are symmetrically arranged in the two long sides of the lower steel plate, and the second steel bars are symmetrically arranged in the two wide sides of the lower steel plate, and the lower steel plate, the first steel bars and the second steel bars form a receiving space;
[0013] The upper titanium alloy plate and the lower titanium alloy plate which have been pretreated for the second time are stacked up and down to form a titanium alloy composite plate, and the plate is arranged in the accommodation space;
[0014] The upper steel plate that has undergone the first pretreatment is arranged opposite to the lower steel plate, covers the accommodation space, and is connected with the first steel bar and the second steel bar to form a steel-titanium clad structure;
[0015] A first gap is provided between the first steel bar and the titanium alloy composite plate, and a second gap is provided between the second steel bar and the titanium alloy composite plate; an air hole is left at one end adjacent to the first steel bar and the second steel bar;
[0016] Step S2, subjecting the steel-titanium clad structure to heating, hot rolling and hot straightening processes in sequence to obtain a pre-finished product;
[0017] Step S3, post-processing the pre-finished product to obtain the target product.
[0018] In some embodiments, in step S1, the first pretreatment includes first grinding, chamfering and first brushing, wherein the first grinding is to grind and polish the surfaces of the upper steel plate and the lower steel plate located in the accommodation space respectively; the chamfering is to chamfer the edges of the surfaces of the upper steel plate and the lower steel plate located in the accommodation space respectively; the first brushing is to brush the isolation agent on the surfaces of the upper steel plate and the lower steel plate respectively in contact with the titanium alloy composite plate to form a first coating;
[0019] The second pretreatment includes a second grinding and a second brushing, wherein the second grinding is to grind and polish the upper and lower surfaces of the upper titanium alloy plate and the upper and lower surfaces of the lower titanium alloy plate respectively, and the grinding direction is the direction of reversing rolling of the upper titanium alloy plate and the lower titanium alloy plate; the second brushing is to brush the isolation agent on the upper and lower surfaces of the upper titanium alloy plate and the upper and lower surfaces of the lower titanium alloy plate respectively to form a second coating.
[0020] In some embodiments, the first coating layer and the second coating layer have the same thickness, which is 0.1-0.2 mm.
[0021] In some embodiments, the width of the first gap is 3-5 mm; in the rolling direction, the width of the second gap at the front end of the steel-titanium cladding structure is 3-5 mm, and the width of the second gap at the rear end of the steel-titanium cladding structure is 20-30 mm; the width of the pores is 30-50 mm.
[0022] In some embodiments, the first steel bar and the second steel bar have the same thickness, and both are 0-0.2 mm thinner than the thickness of the titanium alloy composite plate.
[0023] In some embodiments, step S1 further includes spot welding and full welding. First, the upper surface and the lower surface of the steel-titanium cladding structure are respectively pressed by a pressing mechanism; then, the positions where the first steel bar contacts the upper steel plate and the lower steel plate are spot welded, and the positions where the second steel bar contacts the upper steel plate and the lower steel plate are spot welded; finally, the positions where the first steel bar contacts the upper steel plate and the lower steel plate are full welded, and the positions where the second steel bar contacts the upper steel plate and the lower steel plate are full welded;
[0024] The upper titanium alloy plate and the lower titanium alloy plate are both made of TA5 titanium alloy.
[0025] In some embodiments, in step S2, the heating process conditions used for the steel-titanium clad structure are: the heating temperature is 20-30°C below the phase transition point temperature of TA5 titanium alloy, the insulation time is 1.2-1.4min / mm times the thickness of the steel-titanium clad structure, and the furnace is loaded when the temperature reaches 1.2-1.4min / mm.
[0026] In some embodiments, in step S2, the hot rolling process conditions used for the steel-titanium clad structure are: after being taken out of the furnace, the steel-titanium clad structure is hot rolled within 1 minute; the equipment used for the hot rolling includes a 3800mm four-roll reversible hot rolling mill in a steel plant;
[0027] During the hot rolling process, the starting rolling temperature is controlled at 900-920°C, the hot rolling passes are controlled not to exceed 10 passes, the reduction in the initial pass is controlled to be 8-12mm, and the reduction rate is controlled to be 9.1%-10.7%; in the middle pass, the reduction is controlled to increase first and then decrease, with a range of 2-12mm, and the control reduction is controlled to increase first and then decrease, with a range of 5.2%-16.7%; in the final pass, the reduction is controlled to be 1-2mm, and the reduction rate is controlled to be 2.8%-3.6%; the rolling speed is controlled to be 2-4.5m / s;
[0028] After hot rolling, hot straightening is directly performed using a hot straightening machine to obtain a pre-finished product;
[0029] The hot straightening is to perform straightening treatment on the plate obtained by hot rolling, and the hot straightening temperature is greater than or equal to 700°C.
[0030] In some embodiments, in step S3, the post-processing includes trimming, lifting, annealing, shaping, surface treatment, sizing, and pickling and whitening; wherein,
[0031] The trimming and lifting plate is used to trim the pre-finished product after straightening, and the first steel bar and the second steel bar at the edge of the pre-finished product are cut off; then the upper steel plate and the lower steel plate are lifted off, and the upper titanium alloy plate and the lower titanium alloy plate are taken out;
[0032] The annealing is to heat and air-cool the upper titanium alloy plate and the lower titanium alloy plate respectively, wherein the heating temperature is 700-750°C, and after keeping the temperature for 30-60 minutes, the upper titanium alloy plate and the lower titanium alloy plate are respectively air-cooled;
[0033] The shape correction is to use a leveling device to level the upper titanium alloy plate and the lower titanium alloy plate after air cooling respectively;
[0034] The surface treatment is to perform surface grinding treatment on the leveling upper titanium alloy plate and the lower titanium alloy plate respectively;
[0035] The sizing is to determine the sizes of the upper titanium alloy plate and the lower titanium alloy plate after surface treatment respectively to obtain the target product;
[0036] The pickling and whitening is a surface decontamination treatment for the target product.
[0037] In some embodiments, the target product is a wide TA5 titanium alloy plate product with a target size of (4-10mm)*(1200-1600mm)*L.
[0038] The application of the technical solution of the present invention has at least the following beneficial effects:
[0039] (1) The present invention adopts a method for preparing a wide titanium alloy plate using a titanium-steel joint mode. Through the steel-titanium cladding structure, the titanium alloy composite plate is prevented from directly contacting the air and the rollers during the hot rolling process. In this way, the problem of surface cracks due to a sharp increase in the deformation resistance of the titanium alloy material caused by too fast a temperature drop is not caused, and the possibility of a thicker oxide layer being generated on the surface of the titanium alloy composite plate in contact with the atmosphere is reduced. In addition, the titanium alloy composite plate is coated with an upper steel plate and a lower steel plate, so that the thickness of the steel-titanium cladding structure after rolling in the steel plant meets its equipment requirements (i.e., a thickness of more than 10 mm), ensuring the lower limit thickness of the steel plant equipment rolling; the upper steel plate and the lower steel plate are removed by post-processing to obtain the target product. In addition, the upper steel plate and the lower steel plate are used to make the material selection price cheap and reduce the manufacturing cost. The first gap and the second gap are set to provide deformation extension space for the titanium alloy composite plate during the hot rolling process; the pores are set to ensure that the gas generated by the titanium alloy composite plate during the hot rolling process is released in time, so that the hot rolling process proceeds smoothly. The target product is a wide-width TA5 titanium alloy plate product with a target size of (4-10)*(1200-1600)*L mm, which has high market competitiveness.
[0040] (2) The method of preparing wide-width titanium alloy plates by using a titanium-steel joint mode in the present invention relies on the steel plant's 3800mm rolling mill and other equipment to achieve the production of wide-width TA5 alloy plates, meeting the current market demand for wider and thinner TA5 titanium alloy plates, and also getting rid of the limitation that only equipment from individual manufacturers can be used to produce these specifications of products; it is also a new method and process for preparing wide-width titanium alloy plates by coating using a new titanium-steel joint production mode. In addition, the titanium-steel joint production mode adopted in the present invention also reduces the generation of cracks on the surface of the TA5 titanium alloy and thus reduces the amount of grinding on the surface of the titanium alloy plate, improves the yield rate, and reduces the manufacturing cost.
[0041] In addition to the above-described objects, features and advantages, the present invention has other objects, features and advantages. The present invention will be further described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] The drawings constituting a part of this application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0043] Figure 1 This is the metallographic structure diagram of the 5 mm thick and wide TA5 alloy target product obtained in Example 1 of the present invention after annealing;
[0044] Figure 2 This is the metallographic structure diagram of the TA5 alloy target product with a thickness of 8 mm and a width obtained in Example 2 of the present invention after annealing. DETAILED DESCRIPTION
[0045] The following will be combined with the accompanying drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.
[0046] Embodiment 1:
[0047] A method for preparing a wide titanium alloy plate using a titanium-steel joint mode comprises the following steps:
[0048] Step S1: Making a steel-titanium clad structure
[0049] The lower steel plate that has undergone the first pretreatment is horizontally arranged, the first steel bars are symmetrically arranged in the two long sides of the lower steel plate, and the second steel bars are symmetrically arranged in the two wide sides of the lower steel plate, and the lower steel plate, the first steel bars and the second steel bars form a receiving space;
[0050] The upper titanium alloy plate and the lower titanium alloy plate which have been pretreated for the second time are stacked up and down to form a titanium alloy composite plate, and the plate is arranged in the accommodation space;
[0051] The upper steel plate that has undergone the first pretreatment is arranged opposite to the lower steel plate, covers the accommodation space, and is connected with the first steel bar and the second steel bar to form a steel-titanium clad structure;
[0052] A first gap is provided between the first steel bar and the titanium alloy composite plate, and a second gap is provided between the second steel bar and the titanium alloy composite plate; an air hole is left on one end adjacent to the first steel bar and the second steel bar. The first steel bar, the second steel bar, the upper steel plate and the lower steel plate are all made of Q345R.
[0053] See Table 1 for the initial conditions and rolling plans of the upper steel plate, the lower steel plate, the upper titanium alloy plate, the lower titanium alloy plate, the first steel bar and the second steel bar used in step S1.
[0054] Table 1
[0055]
[0056] The design in Table 1 is as follows: 45mm is reserved on all four sides of the lower steel plate and the upper steel plate without coating. After the first steel bar and the second steel bar are placed in this 45mm area, the remaining area 25mm away from the edge and the chamfers of the lower steel plate and the upper steel plate are convenient for subsequent welding; the size of the two second steel bars at the head and tail is determined by calculation to be 27.8*20*1600mm. After deducting the welding area and the thickness of the steel bar, the size of the two symmetrical ventilation holes at the head and tail is guaranteed to be 30mm.
[0057] Step S2, subjecting the steel-titanium clad structure to heating, hot rolling and hot straightening processes in sequence to obtain a pre-finished product;
[0058] Step S3, post-processing the pre-finished product to obtain the target product.
[0059] In step S1, the first pretreatment includes first grinding, chamfering and first brushing, wherein the first grinding is to grind and polish the surfaces of the upper steel plate and the lower steel plate located in the accommodation space respectively, and the surface crack defects are cleaned, wherein the direction of the first grinding and polishing is the rolling direction, specifically the long side direction of the steel-titanium cladding structure; chamfering is to chamfer the edges of the surfaces of the upper steel plate and the lower steel plate located in the accommodation space respectively, specifically, the surfaces of the upper steel plate and the lower steel plate located in the accommodation space are chamfered on one side, and the chamfer size is 4mm*45°, which is convenient for welding with a welding gun; the first brushing is to brush the isolation agent on the surfaces of the upper steel plate and the lower steel plate that are in contact with the titanium alloy composite plate respectively, to form a first coating; the upper steel plate and the lower steel plate are both made of Q345R steel;
[0060] The second pretreatment includes a second grinding and a second brushing, wherein the second grinding is to grind and polish the upper and lower surfaces of the upper titanium alloy plate and the upper and lower surfaces of the lower titanium alloy plate respectively, and the grinding direction is the direction of subsequent reversing rolling of the upper titanium alloy plate and the lower titanium alloy plate, and the purpose of reversing rolling is to make the anisotropy of the final finished titanium alloy plate smaller; the second grinding can be used to clean the surface crack defects of the upper titanium alloy plate and the lower titanium alloy plate; the second brushing is to brush the upper and lower surfaces of the upper titanium alloy plate and the upper and lower surfaces of the lower titanium alloy plate with an isolation agent to form a second coating.
[0061] The thickness of the first coating layer and the second coating layer is the same, both of which are 0.1 mm.
[0062] The width of the first gap is 5 mm; in the rolling direction, the width of the second gap located at the front end of the steel-titanium cladding structure is 5 mm, and the width of the second gap located at the rear end of the steel-titanium cladding structure is 30 mm; the number of the pores is four, and they are symmetrically arranged, and the width of each pore is 30 mm.
[0063] The first steel bar and the second steel bar have the same thickness, and are both 0.2 mm thinner than the thickness of the titanium alloy composite plate, to ensure that the internal titanium alloy composite plate is compressed during subsequent welding and assembly, to avoid movement of the titanium alloy composite plate and affect subsequent rolling.
[0064] In step S1, it also includes the use of robot automatic welding processing, namely spot welding processing and full welding processing. First, the upper surface and the lower surface of the steel-titanium cladding structure are respectively pressed by a hydraulic press clamping mechanism; then, the positions where the first steel bar contacts the upper steel plate and the lower steel plate are spot welded, and the positions where the second steel bar contacts the upper steel plate and the lower steel plate are spot welded; the spot welding process ensures that the titanium alloy composite plate is pressed by the upper steel plate and the lower steel plate; finally, the positions where the first steel bar contacts the upper steel plate and the lower steel plate are full welded, and the positions where the second steel bar contacts the upper steel plate and the lower steel plate are full welded; the full welding process ensures that the titanium alloy composite plate is firmly pressed by the upper steel plate and the lower steel plate, thereby ensuring the smooth progress of step S2. It should be noted that during the spot welding and full welding processes, the pores need to be sealed with thermal insulation cotton first to prevent welding slag from entering the accommodation space and affecting the surface quality of the titanium alloy composite plate; after welding is completed, the thermal insulation cotton is removed to ensure that the gas generated by the titanium alloy composite plate during the hot rolling process is released in time, so that the hot rolling process proceeds smoothly.
[0065] The sequence of the above processing process of step S1 can be summarized as shown in Table 2.
[0066] Table 2
[0067]
[0068]
[0069] The upper titanium alloy plate and the lower titanium alloy plate are both made of TA5 titanium alloy.
[0070] In step S2, the heating process conditions used for the steel-titanium clad structure are: the heating temperature is 980°C and the holding time is 105 minutes, and the furnace is loaded at temperature (that is, the steel-titanium clad structure is loaded into the furnace after the actual temperature of the heating furnace reaches the required heating temperature, and the holding time is calculated). In step S2, the hot rolling process conditions used for the steel-titanium clad structure are: after being taken out of the furnace, the steel-titanium clad structure is hot rolled within 1 minute; the equipment used for hot rolling is a 3800mm four-roll reversible hot rolling mill in a steel plant;
[0071] In the hot rolling process, the starting temperature is controlled at 920°C, and the rolling is carried out with a width of 1750 mm. The hot rolling passes are controlled to be no more than 10 passes, and the reduction in the initial pass is controlled to be 8-12 mm, and the reduction rate is controlled to be 9.1%-10.7%; in the middle pass, the reduction is controlled to increase first and then decrease, and the range is 2-12 mm, and the control reduction is controlled to increase first and then decrease, and the range is 5.2%-16.7%; in the final pass, the reduction is controlled to be 1-2 mm, and the reduction rate is controlled to be 2.8%-3.6%, see Table 3 for details. In the hot rolling process, the rolling speed is controlled to be 2-4.5 m / s.
[0072] Table 3 (Note: The negative sign in some rolling speeds in Table 3 indicates that the rolling direction is reverse)
[0073] path Roller gap setting mm Press down amount (mm) Reduction rate % Rolling speed m / s 1 80 8 9.1% 2.11 2 70 10 12.5% -2.23 3 60 10 14.3% 2.35 4 50 10 16.7% -2.47 5 42 8 16.0% 3.42 6 38 4 9.5% -3.82 7 36 2 5.2% 4.23 8 34 1 2.8% -4.43
[0074] After hot rolling, hot straightening machine is used to perform hot straightening treatment directly. The hot straightening temperature is ≥700℃. After hot straightening, pre-finished products are obtained.
[0075] In step S3, the post-processing includes trimming, lifting, annealing, shaping, surface treatment, sizing and pickling and whitening; wherein,
[0076] The trimming and lifting plate is used to trim the pre-finished product after straightening, and the first steel bar and the second steel bar at the edge of the pre-finished product are cut off; then the upper steel plate and the lower steel plate are lifted off, and the upper titanium alloy plate and the lower titanium alloy plate are taken out;
[0077] The annealing process is 700°C / 40min / AC. Specifically, the annealing is to heat and air-cool the upper titanium alloy plate and the lower titanium alloy plate respectively. The heating temperature is 700°C. After keeping warm for 40 minutes, the upper titanium alloy plate and the lower titanium alloy plate are air-cooled respectively.
[0078] The shape correction is to use a leveling device to level the upper titanium alloy plate and the lower titanium alloy plate after air cooling respectively;
[0079] The surface treatment is to perform surface grinding treatment on the leveling upper titanium alloy plate and the lower titanium alloy plate respectively;
[0080] The sizing is to determine the sizes of the upper titanium alloy plate and the lower titanium alloy plate after surface treatment respectively to obtain the target product;
[0081] The pickling and whitening is a surface decontamination treatment for the target product.
[0082] The target product obtained in Example 1 is a wide-width TA5 titanium alloy plate product with a target size of 5mm*1600mm*4000mm, and its dimensional accuracy, plate shape, surface quality, organization and performance indicators can meet the requirements of GJB 944A-2018 standard.
[0083] Depend on Figure 1 It is known that the target product can effectively improve the uniformity of the structure and achieve equiaxed structure after heating, hot rolling and hot straightening, and obtain a metallographic structure mainly composed of equiaxed α phase, which meets the organizational characteristics of annealed state TA5.
[0084] According to the provisions of GB / T 228.1-228, the room temperature tensile properties of wide TA5 alloy plates of different specifications were tested, and the sampling directions were longitudinal and transverse. Table 4 below shows the room temperature tensile properties test results of the corresponding materials. From the test data, the tensile performance indicators can meet the requirements of GJB 944A-2018 standard.
[0085] Table 4 Tensile properties of finished TA5 alloy plates with a thickness of 5 mm and a width of 5 mm
[0086]
[0087] Embodiment 2:
[0088] Different from Example 1,
[0089] In step S1: the initial conditions and rolling plan conditions shown in Table 1 are adjusted to Table 4.
[0090] Table 4
[0091]
[0092] In step S2: In step S2, the heating process conditions adopted for the steel-titanium cladding structure are: the heating temperature is 960°C and the holding time is 135 minutes;
[0093] During the hot rolling process, the starting rolling temperature was controlled at 900°C, and the rolling was carried out with a width of 1650 mm. The specific conditions for controlling the hot rolling passes are shown in Table 5.
[0094] Table 5 (Note: The negative sign in some rolling speeds in Table 5 indicates that the rolling direction is reverse)
[0095] path Roller gap setting mm Press down amount (mm) Reduction rate % Rolling speed m / s 1 100 12 10.7% 2.32 2 88 12 12% -2.56 3 74 14 15.9% 2.90 4 64 10 13.5% -3.20 5 58 6 9.4% 3.82 6 55 3 5.2% -4.03 7 53 2 3.6% 4.30
[0096] In step S3: the annealing process is 750℃ / 40min / AC. Specifically, the annealing is to heat and air-cool the upper titanium alloy plate and the lower titanium alloy plate respectively. The heating temperature is 750℃. After keeping warm for 40min, the upper titanium alloy plate and the lower titanium alloy plate are air-cooled respectively.
[0097] The target product obtained by Example 2 is a wide-width TA5 titanium alloy plate product with a target size of 8*1500*4000mm, and its dimensional accuracy, plate shape, surface quality, organization and performance indicators can meet the requirements of GJB 944A-2018 standard.
[0098] Depend on Figure 2 It is known that the target product can effectively improve the uniformity of the structure and achieve equiaxed structure after heating, hot rolling and hot straightening, and obtain a metallographic structure mainly composed of equiaxed α phase, which meets the organizational characteristics of annealed state TA5.
[0099] According to the provisions of GB / T 228.1-228, the room temperature tensile properties of wide TA5 alloy plates of different specifications were tested, and the sampling directions were longitudinal and transverse. Table 5 below shows the room temperature tensile properties test results of the corresponding materials. From the test data, the tensile performance indicators can meet the requirements of GJB 944A-2018 standard.
[0100] Table 5 Tensile properties of finished TA5 alloy plates with a thickness of 8 mm and a width of 8 mm
[0101]
[0102]
[0103] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing wide titanium alloy plates using a titanium-steel joint mode, characterized in that: The following steps are involved: Step S1: Making a steel-titanium clad structure The lower steel plate that has undergone the first pretreatment is horizontally arranged, the first steel bars are symmetrically arranged in the two long sides of the lower steel plate, and the second steel bars are symmetrically arranged in the two wide sides of the lower steel plate, and the lower steel plate, the first steel bars and the second steel bars form a receiving space; The upper titanium alloy plate and the lower titanium alloy plate which have been pretreated for the second time are stacked up and down to form a titanium alloy composite plate, and the plate is arranged in the accommodation space; The upper steel plate that has undergone the first pretreatment is arranged opposite to the lower steel plate, covers the accommodation space, and is connected with the first steel bar and the second steel bar to form a steel-titanium clad structure; A first gap is provided between the first steel bar and the titanium alloy composite plate, and a second gap is provided between the second steel bar and the titanium alloy composite plate; an air hole is left at one end adjacent to the first steel bar and the second steel bar; Step S2, the steel-titanium clad structure is subjected to heating, hot rolling and hot straightening processes in sequence to obtain a pre-finished product; during the hot rolling process, the starting rolling temperature is controlled at 900-920°C, the hot rolling passes are controlled to be no more than 10 passes, the reduction in the initial pass is controlled to be 8-12 mm, and the reduction rate is controlled to be 9.1%-10.7%; in the intermediate passes, the reduction is controlled to increase first and then decrease, with a range of 2-12 mm, and the reduction is controlled to increase first and then decrease, with a range of 5.2%-16.7%; in the final pass, the reduction is controlled to be 1-2 mm, and the reduction rate is controlled to be 2.8%-3.6%; the rolling speed is controlled to be 2-4.5 m / s; Step S3, obtaining a target product by post-processing the pre-finished product; the target product is a wide TA5 titanium alloy plate product with a target size of (4-10)*(1200-1600)*Lmm.
2. The method for preparing wide-width titanium alloy plates using a titanium-steel joint mode according to claim 1 is characterized in that: In step S1, the first pretreatment includes first grinding, chamfering and first painting, wherein the first grinding is to grind and polish the surfaces of the upper steel plate and the lower steel plate located in the accommodation space respectively; the chamfering is to chamfer the edges of the surfaces of the upper steel plate and the lower steel plate located in the accommodation space respectively; the first painting is to apply a release agent to the surfaces of the upper steel plate and the lower steel plate respectively in contact with the titanium alloy composite plate to form a first coating; The second pretreatment includes a second grinding and a second brushing, wherein the second grinding is to grind and polish the upper and lower surfaces of the upper titanium alloy plate and the upper and lower surfaces of the lower titanium alloy plate respectively, and the grinding direction is the direction of reversing rolling of the upper titanium alloy plate and the lower titanium alloy plate; the second brushing is to brush the isolation agent on the upper and lower surfaces of the upper titanium alloy plate and the upper and lower surfaces of the lower titanium alloy plate respectively to form a second coating.
3. The method for preparing wide-width titanium alloy sheet using titanium-steel joint mode according to claim 2 is characterized in that: The thickness of the first coating layer and the second coating layer is the same, which is 0.1-0.2 mm.
4. The method for preparing wide-width titanium alloy sheet using titanium-steel joint mode according to claim 1, characterized in that: The width of the first gap is 3-5mm; in the rolling direction, the width of the second gap at the front end of the steel-titanium cladding structure is 3-5mm, while the width of the second gap at the rear end of the steel-titanium cladding structure is 20-30mm; the width of the pores is 30-50mm.
5. The method for preparing wide-width titanium alloy plates using a titanium-steel joint mode according to claim 1, characterized in that: The thickness of the first steel bar and the second steel bar is the same, and both are 0-0.2 mm smaller than the thickness of the titanium alloy composite plate.
6. The method for preparing wide-width titanium alloy plates by using a titanium-steel joint mode according to any one of claims 1 to 5, characterized in that: In step S1, spot welding and full welding are also included. First, the upper surface and the lower surface of the steel-titanium cladding structure are respectively pressed by a pressing mechanism; then, the positions where the first steel bar contacts the upper steel plate and the lower steel plate are spot welded, and the positions where the second steel bar contacts the upper steel plate and the lower steel plate are spot welded; finally, the positions where the first steel bar contacts the upper steel plate and the lower steel plate are full welded, and the positions where the second steel bar contacts the upper steel plate and the lower steel plate are full welded; The upper titanium alloy plate and the lower titanium alloy plate are both made of TA5 titanium alloy.
7. The method for preparing wide-width titanium alloy plates using a titanium-steel joint mode according to claim 6, characterized in that: In step S2, the heating process conditions used for the steel-titanium cladding structure are: the heating temperature is 20-30°C below the phase transition point temperature of TA5 titanium alloy, the insulation time is 1.2-1.4min / mm times the thickness of the steel-titanium cladding structure, and the furnace is loaded when the temperature reaches 100°C.
8. The method for preparing wide-width titanium alloy plates using a titanium-steel joint mode according to claim 7, characterized in that: In step S2, the hot rolling process conditions used for the steel-titanium clad structure are: after being taken out of the furnace, the steel-titanium clad structure is hot rolled within 1 minute; the equipment used for the hot rolling includes a 3800mm four-roll reversible hot rolling mill of the steel plant; After hot rolling, hot straightening is directly performed using a hot straightening machine to obtain a pre-finished product; The hot straightening is to perform straightening treatment on the plate obtained by hot rolling, and the hot straightening temperature is greater than or equal to 700°C.
9. The method for preparing wide-width titanium alloy plates using a titanium-steel joint mode according to claim 8, characterized in that: In step S3, the post-processing includes trimming, lifting, annealing, shaping, surface treatment, sizing and pickling and whitening; wherein, The trimming and lifting plate is used to trim the pre-finished product after straightening, and the first steel bar and the second steel bar at the edge of the pre-finished product are cut off; then the upper steel plate and the lower steel plate are lifted off, and the upper titanium alloy plate and the lower titanium alloy plate are taken out; The annealing is to heat and air-cool the upper titanium alloy plate and the lower titanium alloy plate respectively, wherein the heating temperature is 700-750°C, and after keeping the temperature for 30-60 minutes, the upper titanium alloy plate and the lower titanium alloy plate are respectively air-cooled; The shape correction is to use a leveling device to level the upper titanium alloy plate and the lower titanium alloy plate after air cooling respectively; The surface treatment is to perform surface grinding treatment on the leveling upper titanium alloy plate and the lower titanium alloy plate respectively; The sizing is to determine the sizes of the upper titanium alloy plate and the lower titanium alloy plate after surface treatment respectively to obtain the target product; The pickling and whitening is a surface decontamination treatment for the target product.
Citation Information
Patent Citations
A method for preparing titanium alloy thin plates by steel plate cladding and rolling
CN102274851A
Preparation method for titanium alloy wide sheet
CN102489507A
Method for preparing titanium alloy wide and thick plate through steel mill rolling mill
CN110695085A
Assembly of rolling composite sheet of titanium steel
CN206652853U
Manufacture of titanium clad steel sheet by continuous hot rolling
JP1994155050A