Method for manufacturing glass sheet

By using glass compound with low B2O3 content in an electric melting furnace and adjusting the cooling speed of the annealing process, the problem of difficult to reduce the heat shrinkage in the prior art is solved, and a glass plate with a heat shrinkage of less than 15 ppm is realized. At low temperature polysilicon TFT and organic EL display.

CN115043576BActive Publication Date: 2024-11-12NIPPON ELECTRIC GLASS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210807118.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2017-12-20
Filing Date
2018-12-14
Publication Date
2024-11-12
Estimated Expiration
2038-12-14

AI Technical Summary

Technical Problem

The prior art is difficult to manufacture a glass plate with a heat shrinkage rate of 15 ppm or less in a glass substrate for low-temperature polysilicon TFT and an organic EL display, and the deviation of the heat shrinkage rate is difficult to effectively suppress.

Method used

The glass compound with a content of B2O3 below 3% is melted in an electric melting furnace. The cooling rate of the glass plate is adjusted through the annealing process to control the heat shrinkage rate, ensuring that the β-OH value of the glass plate is less than 0.2/mm and the heat shrinkage rate is Below 15ppm.

Benefits of technology

A glass plate with a thermal shrinkage of less than 15 ppm and a small deviation is achieved, which improves the thermal dimensional stability of the glass plate and is suitable for low-temperature polysilicon TFTs and organic EL displays.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115043576B_ABST
    Figure CN115043576B_ABST
Patent Text Reader

Abstract

The technical problem of the present invention is to provide a method for manufacturing a glass plate that can make the thermal shrinkage rate less than 15 ppm and stably suppress the deviation of the thermal shrinkage rate. The method for manufacturing a glass plate of the present invention is characterized in that it includes the following steps: a melting step of melting a glass batch prepared in a manner to become glass with a B2O3 content of less than 3% by mass in an electric melting furnace (1); a forming step of forming the molten glass (Gm) into a plate glass; an annealing step of annealing the plate glass in an annealing furnace (12); and a cutting step of cutting the annealed plate glass (Gr) into a specified size to obtain a glass plate (Gs) having a β-OH value of less than 0.2 / mm and a thermal shrinkage rate of less than 15 ppm, and measuring the thermal shrinkage rate of the glass plate (Gs), and adjusting the cooling rate of the plate glass in the annealing step according to the deviation of the thermal shrinkage rate from the target value.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of application number: 201880065281.5, PCT application number: PCT / JP2018 / 046174, application date: 2018.12.14, invention name: "Method for manufacturing glass plate". Technical Field

[0002] The present invention relates to a method for manufacturing a glass plate capable of stably manufacturing a glass plate having a low heat shrinkage rate. Background Art

[0003] As a glass melting furnace for melting glass raw materials, a gas combustion furnace utilizing gas combustion is generally widely used.

[0004] The glass melting furnace using gas combustion is a furnace that always carries out gas combustion. Therefore, the water concentration of the molten glass is substantially dominated by the water content of the exhaust gas from the burner combustion, and is maintained at a high level. As a result, the water content (β-OH value) of the manufactured glass becomes higher, the strain point is lowered, and the thermal shrinkage rate of the display glass plate's thermal dimensional stability becomes higher. In the case of glass substrates for displays such as low-temperature polysilicon TFTs and organic ELs, if high-temperature heat treatment is performed and a glass plate with poor thermal dimensional stability is used, poor display of the display device is likely to occur. Therefore, glass plates with low thermal shrinkage rates and small deviations in thermal shrinkage rates are particularly required.

[0005] In view of this situation, it is proposed to reduce the deviation of the thermal shrinkage rate of the glass sheet by adjusting the glass raw materials (see Patent Documents 1 and 2). In addition, it is proposed to reduce the deviation of the thermal shrinkage rate of the glass sheet by lowering the air pressure of the outer space of the annealing furnace of the down draw forming device relative to the air pressure of the inner space of the annealing furnace (Patent Document 3).

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2014-88306

[0009] Patent Document 2: Japanese Patent Application No. 2017-530928

[0010] Patent Document 3: Japanese Patent Application Publication No. 2013-126946 Summary of the invention

[0011] Problems to be solved by the invention

[0012] Patent Document 1 controls the mixing ratio of glass raw materials and cullets to adjust the β-OH value of glass, and Patent Document 2 selects glass batch materials to adjust the β-OH value of glass.

[0013] In recent years, with the advancement of higher definition of display screens, glass substrates for displays such as low-temperature polysilicon TFTs and organic ELs have been required to have a lower thermal shrinkage rate. Specifically, a thermal shrinkage rate of 15 ppm or less has been required.

[0014] However, as in Patent Documents 1 and 2, if the mixing ratio of glass raw materials and cullet is changed or the glass batch material is selected to adjust the β-OH value of the glass, it is difficult to adjust the deviation at an extremely low level of 15 ppm or less of the thermal shrinkage of the glass plate. That is, when the target value of the thermal shrinkage of the glass plate is about 20 ppm, the β-OH value of the glass can be adjusted by changing the glass raw materials and cullet, but in order to make the thermal shrinkage of the glass plate below 15 ppm, the water content of the glass raw materials needs to be reduced to a near limit. Therefore, even if the thermal shrinkage of the glass plate exceeds 15 ppm due to changes in the melting conditions of the glass, it is difficult to adopt a countermeasure to further reduce the β-OH value of the glass by changing the glass raw materials, and it is difficult to achieve a reduction in the thermal shrinkage of the glass plate.

[0015] In addition, Patent Document 3 reduces the deviation of the thermal shrinkage rate in the width direction of the glass sheet by suppressing the deviation of the temperature inside the annealing furnace of the pull-down device, and does not intend to suppress the deviation of the thermal shrinkage rate between glass sheets produced at different times due to the change of the β-OH value of the glass. In addition, it does not envision reducing the β-OH value of the glass to reduce the thermal shrinkage rate to less than 15 ppm.

[0016] An object of the present invention is to provide a method for producing a glass plate in which the thermal shrinkage rate can be set to 15 ppm or less and in which the variation in the thermal shrinkage rate can be stably suppressed.

[0017] Means for solving problems

[0018] The manufacturing method of the glass plate of the present invention created to solve the above-mentioned problems is characterized in that it includes the following steps: a melting step of melting a glass batch prepared in a manner to obtain glass having a B2O3 content of 3% or less by mass in an electric melting furnace; a forming step of forming the molten glass into a plate-shaped glass; an annealing step of annealing the plate-shaped glass in an annealing furnace; and a cutting step of cutting the annealed plate-shaped glass into a specified size to obtain a glass plate having a β-OH value of less than 0.2 / mm and a thermal shrinkage of less than 15 ppm, and measuring the thermal shrinkage of the glass plate, and adjusting the cooling rate of the plate-shaped glass in the annealing step according to the deviation of the thermal shrinkage from the target value. Here, the glass batch is a general term for glass raw materials and cullet obtained by finely crushing glass articles.

[0019] According to the method of the present invention, the glass batch prepared in a manner to become glass with a B2O3 content of less than 3% by mass is melted in an electric melting furnace, thereby easily obtaining a glass plate with a β-OH value of less than 0.2 / mm and a thermal shrinkage of less than 15 ppm.

[0020] That is, the β-OH value of glass is easily affected by the water content contained in the glass batch put into the glass melting furnace, especially the glass raw material as a boron source is hygroscopic, and there is also a substance containing crystal water, so it is easy to introduce water into the glass. Therefore, the more the content of B2O3 in the glass is reduced, the lower the β-OH value of the glass is, and the easier it is to achieve the reduction of the thermal shrinkage of the glass sheet. In addition, if an electric melting furnace is used to melt the glass, the increase of the amount of water in the atmosphere caused by gas combustion in the melting furnace can be suppressed, so it is easy to reduce the amount of water in the molten glass compared with a gas combustion furnace. Therefore, the β-OH value of the glass manufactured by the electric melting furnace is reduced, and it is easy to obtain a glass sheet with a low thermal shrinkage. According to the above reasons, it is preferred that substantially no B2O3 is contained in the present invention. Here, substantially no B2O3 means that B2O3 is not intentionally contained as a raw material, and the mixing from impurities is not denied. Specifically, it refers to that the content of B2O3 is less than 0.1% by mass.

[0021] Generally, as the moisture content of the glass batch and the melting conditions of the glass change, the β-OH value of the glass changes, and the thermal shrinkage of the glass sheet changes. In the present invention, the thermal shrinkage of the glass sheet is measured, and the cooling rate of the plate glass in the annealing process is adjusted according to its deviation from the target value. Specifically, when the thermal shrinkage of the glass sheet deviates greatly from the target value, the annealing rate of the plate glass in the annealing process is adjusted, thereby correcting the deviation of the thermal shrinkage of the glass sheet from the target value. In this way, a glass sheet with a small deviation in thermal shrinkage can be stably manufactured. It is preferred to adjust the cooling rate in such a way that the deviation of the target value of the thermal shrinkage of the glass sheet is less than ±1ppm. Here, the deviation of the thermal shrinkage of the glass sheet from the target value is less than ±1ppm, which means that, for example, when the target value of the thermal shrinkage of the glass sheet is 10ppm, the thermal shrinkage is maintained within the range of 9ppm to 11ppm. In addition, the thermal shrinkage of the glass sheet does not need to be measured on all the produced glass sheets, and it is sufficient to perform sampling inspection on a part of the glass sheets.

[0022] In the present invention, the plate glass is slowly cooled while being moved in the annealing process, and the cooling rate is preferably an average cooling rate of 300°C / min to 1000°C / min in the temperature range from the annealing point to (annealing point-100°C). The thermal shrinkage rate of the glass plate varies depending on the cooling rate when the plate glass is annealed. That is, the thermal shrinkage rate of the glass plate cooled quickly is high, and conversely, the thermal shrinkage rate of the glass plate cooled slowly is low. Therefore, when the thermal shrinkage rate of the glass plate is measured and the thermal shrinkage rate is greater than the target value, the average cooling rate in the temperature range from the annealing point to (annealing point-100°C) is adjusted to be lower in the range of 300°C / min to 1000°C / min, and conversely, when it is less than the target value, the average cooling rate in the temperature range from the annealing point to (annealing point-100°C) is adjusted to be higher in the range of 300°C / min to 1000°C / min.

[0023] It should be noted that in the present invention, from the viewpoint of improving productivity, in the annealing process, the average cooling rate in the temperature range higher than the annealing point and the average cooling rate in the temperature range lower than (annealing point - 100 ° C) can be set to be larger than the average cooling rate in the temperature range from the annealing point to (annealing point - 100 ° C), and specifically, it is preferably set to be 1.1 to 20 times, and further 1.5 to 15 times, the average cooling rate in the temperature range from the annealing point to (annealing point - 100 ° C).

[0024] In the present invention, the heat shrinkage of the glass plate is preferably 12 ppm or less, 10 ppm or less, 9 ppm or less, 8 ppm or less, 7 ppm or less, 6 ppm or less, and particularly 5 ppm or less. However, in order to make the heat shrinkage of the glass plate 0 ppm, productivity will be significantly reduced, so it is preferably 1 ppm or more, 2 ppm or more, and particularly 3 ppm or more. In addition, the deviation of the heat shrinkage of the glass plate from the target value is preferably ±0.7 ppm or less, and particularly ±0.5 ppm or less. If the heat shrinkage of the glass plate is high, poor display of low-temperature polysilicon TFT and organic EL display devices is likely to occur. In addition, if the deviation of the heat shrinkage of the glass plate is large, it is impossible to stably produce display substrates.

[0025] The forming method of the present invention is not particularly limited. From the viewpoint of extending the annealing process, the floating method is preferred. From the viewpoint of improving the surface quality of the glass sheet or reducing its thickness, the down-draw method is preferred, and the overflow down-draw method is particularly preferred. In the overflow down-draw method, the surface of the glass substrate that should become the front and back surfaces does not contact the forming body, but is formed in a free surface state. Therefore, a glass sheet that is not ground and has excellent surface quality (small surface roughness and fluctuation) can be manufactured at a low cost.

[0026] In the present invention, when the down-draw method is adopted, the length (height difference) of the annealing furnace is preferably 3 m or more. The annealing process is a process for removing the strain of the glass sheet. The longer the annealing furnace is, the easier it is to adjust the cooling rate and the easier it is to reduce the thermal shrinkage of the glass sheet. Therefore, the length of the annealing furnace is preferably 5 m or more, 6 m or more, 7 m or more, 8 m or more, 9 m or more, and particularly 10 m or more.

[0027] In the present invention, the short side of the glass plate is preferably 1500 mm or more, and the long side is preferably 1850 mm or more. That is, the larger the size of the glass plate, the more glass substrates that can be produced from a single glass plate, and the higher the production efficiency of the glass substrate, but the thermal shrinkage rate of the glass plate is prone to deviation. However, according to the method of the present invention, even if a glass plate of a large size is manufactured, the deviation of the thermal shrinkage rate of the glass plate can be reliably suppressed, and low thermal shrinkage glass can be stably produced. The short side of the glass plate is preferably 1950 mm or more, 2200 mm or more, 2800 mm or more, and particularly 2950 mm or more, and the long side is preferably 2250 mm or more, 2500 mm or more, 3000 mm or more, and particularly 3400 mm or more.

[0028] In the present invention, the thickness of the glass plate is preferably 0.7 mm or less, 0.6 mm or less, 0.5 mm or less, and particularly 0.4 mm or less, which can reduce the weight of the glass plate and is suitable for a mobile display substrate.

[0029] Effects of the Invention

[0030] According to the present invention, a glass sheet having a heat shrinkage of 15 ppm or less and a small variation in the heat shrinkage can be stably manufactured. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is an explanatory diagram showing equipment used in the method for producing a glass plate of the present invention.

[0032] Figure 2 It is an explanatory diagram showing an overflow down-draw apparatus used in the method for producing a glass sheet of the present invention.

[0033] Figure 3 It is an explanatory diagram showing a method for measuring the thermal shrinkage rate of a glass plate. DETAILED DESCRIPTION

[0034] Hereinafter, one embodiment of the method for producing a glass plate of the present invention will be described with reference to the drawings.

[0035] Figure 1This is an explanatory diagram of the equipment used in the method for manufacturing a glass plate of the present invention, which includes, from the upstream side, an electric melting furnace 1, a clarification tank 2, a homogenization tank (stirring tank) 3, a tank 4 and a forming body 5, which are connected by transfer pipes 6 to 9.

[0036] The electric melting furnace 1 is provided with a raw material supply device 1a for supplying a glass batch prepared with glass raw materials and cullet. As the raw material supply device 1a, a screw feeder or a vibrating feeder can be used, and the glass batch is sequentially supplied to the glass liquid surface of the electric melting furnace 1. The electric melting furnace 1 has a structure equipped with a plurality of electrodes 1b containing molybdenum, platinum, tin, etc., and electricity is applied between these electrodes 1b, so that the molten glass is energized, and the glass is continuously melted by its Joule heat. It should be noted that radiation heating using a heater and a burner can also be used auxiliaryly, but the moisture generated by the combustion of the burner is introduced into the molten glass, and it is difficult to reduce the moisture concentration of the molten glass. Therefore, from the perspective of reducing the β-OH value of the glass, it is ideal to set it as a complete electric melting without using a burner.

[0037] As the electrode 1b, a molybdenum electrode is preferably used. Since the molybdenum electrode has a high degree of freedom in the configuration location and electrode shape, even for alkali-free glass that is difficult to be energized, the optimal electrode configuration and electrode shape can be adopted, and heating by energization is easy. The shape of the electrode 1b is preferably a rod shape. If it is a rod shape, the desired number of electrodes 1b can be arranged at any position on the side wall surface and the bottom wall surface of the electric melting furnace 1 while maintaining the desired distance between electrodes. The arrangement of the electrode 1b is preferably arranged on the wall surface (side wall surface, bottom wall surface, etc.) of the electric melting furnace 1, especially the bottom wall surface, shortening the distance between electrodes and arranging multiple pairs.

[0038] The glass batch supplied from the raw material supply device 1a to the glass liquid surface of the electric melting furnace 1 is melted due to Joule heat to form molten glass. When chloride is contained in the glass batch, the chloride decomposes and volatilizes to take away the moisture in the glass into the atmosphere, thereby reducing the β-OH value of the glass. In addition, polyvalent oxides such as tin compounds contained in the glass batch are dissolved in the molten glass and act as clarifiers. For example, the tin component releases oxygen bubbles during the heating process. The released oxygen bubbles expand and float the bubbles contained in the molten glass MG and are removed from the glass. In addition, the tin component absorbs oxygen bubbles during the cooling process, thereby eliminating the bubbles remaining in the glass.

[0039] The glass batch supplied to the electric melting furnace 1 can be any glass raw material formulation, and cullet can be used in addition to the glass raw material. When cullet is used, the greater the proportion of cullet used relative to the total amount of the glass batch formulated with the glass raw material and cullet, the more the meltability of the glass is improved, and thus it is preferably 1% by mass or more, 5% by mass or more, 10% by mass or more, and particularly 20% by mass or more. There is no upper limit to the proportion of cullet used, but it is preferably 50% by mass or less, 45% by mass or less, and particularly 40% by mass or less.

[0040] Glass raw materials and cullets should have as little water content as possible. In addition, these may absorb moisture from the atmosphere during storage, so it is preferred to supply dry air to the interior of each raw material silo used for weighing and supplying glass raw materials, and the furnace silo (not shown) used to supply the prepared glass batch to the melting furnace.

[0041] In the present invention, the water content of the glass batch is reduced as much as possible, and the glass is melted by the electric melting furnace 1, so that the glass with a β-OH value of less than 0.2 / mm can be manufactured. The lower the β-OH value of the glass, the higher the strain point of the glass becomes, and the lower the thermal shrinkage rate becomes, so the β-OH value is preferably less than 0.15 / mm, less than 0.1 / mm, less than 0.07 / mm, and particularly less than 0.05 / mm.

[0042] The glass melted in the electric melting furnace 1 is then sent to the clarification tank 2 via the transfer pipe 6. The molten glass is clarified (defoamed) by the action of a clarifier, etc. in the clarification tank 2. It should be noted that the clarification tank 2 is not necessarily provided, and the glass clarification process can also be performed on the downstream side of the electric melting furnace 1.

[0043] The molten glass thus clarified is sent to the homogenizing tank 3 via the transfer pipe 7. In the homogenizing tank 3, the molten glass is stirred by the stirring blades 3a and homogenized.

[0044] The molten glass homogenized in this manner is sent to the tank 4 via the transfer pipe 8. In the tank 4, the molten glass is adjusted to a state (viscosity, etc.) suitable for molding.

[0045] The molten glass in the tank 4 is sent to the forming body 5 via the transfer pipe 9. The forming body 5 of the present embodiment is formed into a plate shape by an overflow down-draw method to produce a glass plate.

[0046] The forming body 5 is made of a refractory material having a substantially wedge-shaped cross section, and an overflow trough (not shown) is formed at the top of the forming body 5. After the molten glass Gm is supplied to the overflow trough through the transfer pipe 9, the molten glass Gm overflows from the overflow trough and flows down along the side wall surfaces on both sides of the forming body 5. The molten glass Gm flowing down is fused at the lower top of the side wall surface and extends downward, thereby forming a plate-shaped glass.

[0047] It should be noted that the structure and material of the forming body 5 used in the overflow down-draw method are not particularly limited as long as the desired size and surface accuracy can be achieved. In addition, each transfer pipe 6 to 9 is composed of a cylindrical pipe containing platinum or a platinum alloy, for example, and transfers the molten glass Gm in the horizontal direction. Each transfer pipe 6 to 9 is electrically heated as needed.

[0048] Figure 2 1 is an explanatory diagram showing an overflow down-drawing device 10 used in the manufacturing method of the glass sheet of the present invention. As described above, an overflow trough is formed on the upper part of the forming body 5, an edge roller 11 is provided just below the forming body 5, and a plurality of heaters 13 and stretching rollers 14 are provided in the annealing furnace 12. These edge rollers 11 and stretching rollers 14 clamp both ends of the plate glass Gr and rotate, thereby stretching the plate glass Gr to a predetermined thickness while cooling. In addition, a plurality of heaters 13 in the annealing furnace 12 are installed in the height direction and width direction of the inner wall, and the atmosphere temperature can be controlled for each divided area in the annealing furnace 12, and the temperature of the heater 13 arranged on the downstream side is set lower. That is, the set temperature of the heater 13 is gradually reduced from the upstream side to the downstream side, thereby forming a temperature gradient in the height direction of the annealing furnace 12, so that the cooling rate of the plate glass Gr can be adjusted. The heater 13 may also form a temperature gradient in the width direction of the annealing furnace 12. For example, the set temperature of the heater located in the center of the plate glass may be lower than the set temperature of the heaters 13 located at both ends of the plate glass.

[0049] Each stretching roller 14 can adjust the rotation speed appropriately, and the method of applying force when stretching the plate-shaped glass Gr downward is not particularly limited. For example, a stretching method using a stretching roller having heat-resistant rollers in contact with the plate-shaped glass Gr near both ends; or a stretching method using a stretching roller having heat-resistant rollers separated into multiple pairs and in contact with the ends of the plate-shaped glass Gr can be adopted.

[0050] In the present invention, when the thermal shrinkage of the glass sheet is measured and the deviation of the thermal shrinkage from the target value becomes large, the cooling rate of the plate glass Gr can be appropriately adjusted by adjusting the temperature of each heater 13 in the annealing furnace 12 and the rotation speed of the stretching roller 14. It should be noted that the atmosphere temperature in the annealing furnace 12 is easily disturbed by the rising airflow, so it is ideal to adjust the air pressure inside and outside the furnace in a way that the rising airflow is as small as possible, or to set a mechanism to suppress the rising airflow from intruding into the furnace.

[0051] The plate glass Gr annealed in this manner is cooled in the cooling chamber 15. The cooling chamber 15 is not provided with a heater, and the plate glass Gr is naturally cooled in the cooling chamber 16. The length (height difference) of the cooling chamber 15 may be set to, for example, about 2 to 10 m.

[0052] After the cooling process in the cooling chamber 15, the plate glass Gr is cut into a predetermined size by the cutting device 16a in the cutting chamber 16 to form a glass plate Gs. The cutting device 16a preferably has, for example, a scribing mechanism and a breaking mechanism.

[0053] In the present invention, the glass plate is preferably an alkali-free glass plate containing, by mass%, 50% to 70% of SiO2, 10% to 25% of Al2O3, 0% to 3% of B2O3, 0% to 10% of MgO, 0% to 15% of CaO, 0% to 10% of SrO, 0% to 15% of BaO, 0% to 5% of ZnO, 0% to 5% of ZrO2, 0% to 5% of TiO2, 0% to 10% of P2O5, and 0% to 0.5% of SnO2, and substantially containing no alkali metal oxide. The reasons for specifying the content of each component as described above are explained below. It should be noted that the expression of % of each component below refers to mass % unless otherwise specified.

[0054] SiO2 is a component that forms the skeleton of glass. The content of SiO2 is preferably 50% or more, 55% or more, 58% or more, and particularly 60% or more. In addition, it is preferably 70% or less, 66% or less, 64% or less, 63% or less, and particularly 62% or less. If the content of SiO2 decreases, the density becomes too high and the acid resistance tends to decrease. On the other hand, if the content of SiO2 increases, the high-temperature viscosity increases, the solubility tends to decrease, and devitrified crystals such as cristobalite tend to precipitate, and the liquidus temperature tends to rise.

[0055] Al2O3 is also a component that forms the skeleton of glass, and is a component that improves strain point, Young's modulus and inhibits phase separation. The content of Al2O3 is preferably more than 10%, more than 12%, more than 13%, more than 14%, more than 15%, more than 16%, more than 17%, more than 18%, especially more than 19%. In addition, it is preferably less than 25%, less than 24%, less than 23%, less than 22%, especially less than 20%. If the content of Al2O3 decreases, strain point and Young's modulus are easy to reduce, and glass is easy to phase separate. On the other hand, if the content of Al2O3 increases, devitrified crystals such as mullite and calcium feldspar are easy to precipitate, and liquidus temperature is easy to rise.

[0056] B2O3 is a component that improves the melting property and the resistance to devitrification. If the content of B2O3 increases, the amount of water introduced from the glass raw materials increases, and the strain point and Young's modulus are easily reduced. The content of B2O3 is preferably 3% or less, less than 3%, 2.5% or less, 2% or less, 1.9% or less, 1.6% or less, 1.5% or less, 1% or less, 0.8% or less, 0.5% or less, and it is particularly preferred that it is substantially free of B2O3. Among them, in the case of giving priority to improving the melting property of the glass, it is preferred to contain 0.1% or more, 0.2% or more of B2O3, and it is further preferred to contain 0.3% or more of B2O3.

[0057] MgO is a component that reduces high temperature viscosity and improves solubility, and is a component that significantly improves Young's modulus among alkaline earth metal oxides. The content of MgO is preferably less than 10%, less than 9%, less than 8%, less than 6%, less than 5%, less than 4%, less than 3.5%, and particularly less than 3%. In addition, it is preferably more than 1%, more than 1.5%, and particularly more than 2%. If the content of MgO decreases, the solubility and Young's modulus tend to decrease. On the other hand, if the content of MgO increases, the resistance to devitrification and the strain point tend to decrease.

[0058] CaO is a component that does not lower the strain point and thus reduces high temperature viscosity and significantly improves solubility. It is also a component among alkaline earth metal oxides that reduces the cost of raw materials because the raw materials introduced are relatively cheap. The content of CaO is preferably less than 15%, less than 12%, less than 11%, less than 8%, less than 6%, and particularly less than 5%. In addition, it is preferably more than 1%, more than 2%, more than 3%, and particularly more than 4%. If the content of CaO decreases, it is difficult to enjoy the above-mentioned effects. On the other hand, if the content of CaO is too much, the glass is prone to devitrification and the thermal expansion coefficient is prone to increase.

[0059] SrO is a component that suppresses the phase separation of glass and improves the resistance to devitrification. Furthermore, it is a component that does not lower the strain point and reduces the high-temperature viscosity and improves the solubility, and suppresses the rise in liquidus temperature. The content of SrO is preferably less than 10%, less than 7%, less than 5%, less than 3.5%, and especially less than 3%. In addition, it is preferably more than 0.1%, more than 0.2%, more than 0.3%, more than 0.5%, more than 1.0%, and especially more than 1.5%. If the content of SrO decreases, it is difficult to enjoy the above-mentioned effects. On the other hand, if the content of SrO increases, strontium silicate-based devitrification crystals are likely to precipitate, and the resistance to devitrification is likely to decrease.

[0060] BaO is a component that significantly improves resistance to devitrification. The content of BaO is preferably less than 15%, less than 14%, less than 13%, less than 12%, less than 11%, less than 10.5%, less than 10%, less than 9.5%, and particularly less than 9%. In addition, it is preferably more than 1%, more than 3%, more than 4%, more than 5%, more than 6%, more than 7%, and particularly more than 8%. If the content of BaO decreases, it is difficult to enjoy the above-mentioned effects. On the other hand, if the content of BaO increases, the density becomes too high and the solubility tends to decrease. Moreover, devitrification crystals containing BaO are easily precipitated and the liquidus temperature tends to rise.

[0061] ZnO is a component that improves melting properties. However, if the content of ZnO increases, the glass is prone to devitrification and the strain point is prone to decrease. The content of ZnO is preferably 0% to 5%, 0% to 4%, 0% to 3%, 0% to 2%, 0% to 1%, and particularly 0% to 0.5%.

[0062] ZrO2 is a component that improves chemical durability, but if the content of ZrO2 increases, it is easy to produce devitrified products of ZrSiO4. The content of ZrO2 is preferably 0% to 5%, 0% to 4%, 0% to 3%, 0.1% to 2%, and particularly 0.1% to 0.5%.

[0063] TiO2 is a component that reduces high temperature viscosity and improves melting properties, and inhibits solarization. However, if the content of TiO2 increases, the glass will be colored and the transmittance will be easily reduced. The content of TiO2 is preferably 0% to 5%, 0% to 4%, 0% to 3%, 0% to 2%, and particularly 0% to 0.1%.

[0064] P2O5 is a component that increases the strain point and inhibits the precipitation of devitrified crystals of alkaline earth aluminosilicates such as calcium feldspar. However, if a large amount of P2O5 is contained, the glass is prone to phase separation. The content of P2O5 is preferably 0% to 10%, 0% to 9%, 0% to 8%, 0% to 7%, 0% to 6%, and particularly 0% to 5%.

[0065] SnO2 is a component that has a good clarification effect in a high temperature region, increases the strain point, and reduces the high temperature viscosity. In addition, in the case of an electric melting furnace using a molybdenum electrode, it has the advantage of not corroding the electrode. The content of SnO2 is preferably 0% to 0.5%, 0.001% to 0.5%, 0.001% to 0.45%, 0.001% to 0.4%, 0.01% to 0.35%, 0.1% to 0.3%, and particularly 0.15% to 0.3%. If the content of SnO2 increases, devitrified crystals of SnO2 are easily precipitated, and it is easy to promote the precipitation of devitrified crystals of ZrO2. If the content of SnO2 is less than 0.001%, it is difficult to enjoy the above-mentioned effects.

[0066] In the present invention, in addition to the above-mentioned components, a total of 3% of Cl, F, SO3, C, CeO2 or metal powders such as Al and Si may be contained. From the perspective of the environment and prevention of electrode corrosion, it is ideal that As2O3 and Sb2O3 are substantially not contained.

[0067] In the present invention, substantially containing no alkali metal oxide means that Li2O, Na2O, and K2O are not intentionally contained in the raw materials, and specifically means that the content of the alkali metal oxide is 0.2% or less.

[0068] The alkali-free glass obtained by the method of the present invention preferably has a strain point of 710° C. or higher, 720° C. or higher, 730° C. or higher, 740° C. or higher, and particularly 750° C. or higher. However, the higher the strain point is, the higher the temperature during melting and forming becomes, and the production cost of the glass sheet increases, so it is preferred that the strain point be 800° C. or lower.

[0069] The alkali-free glass obtained by the method of the present invention is preferably 4 The temperature corresponding to dPa·s is 1380°C or lower, 1370°C or lower, and particularly 1360°C or lower. 4 When the dPa·s equivalent temperature increases, the temperature during molding becomes too high, and the manufacturing yield is likely to decrease.

[0070] The alkali-free glass obtained by the method of the present invention is preferably 2.5 dPa·s is equivalent to a temperature of 1670°C or less, 1660°C or less, and particularly 1650°C or less. 2.5 As the temperature corresponding to dPa·s increases, glass becomes difficult to melt, defects such as bubbles increase, and the manufacturing yield tends to decrease.

[0071] The alkali-free glass obtained by the method of the present invention preferably has an annealing point of 750°C or higher, 780°C or higher, 800°C or higher, 810°C or higher, and particularly 820°C or higher.

[0072] The alkali-free glass obtained by the method of the present invention preferably has a liquidus temperature of less than 1250°C, less than 1240°C, less than 1230°C, and particularly less than 1220°C. If so, devitrified crystals are not easily produced during glass manufacturing. In addition, it is easy to form using the overflow down-draw method, thereby improving the surface quality of the glass sheet and suppressing the decline in the manufacturing yield rate. Here, from the perspective of the large-scale glass substrates and the high-precision displays in recent years, in order to suppress devitrification products that will become surface defects as much as possible, it is also very meaningful to improve the resistance to devitrification.

[0073] The alkali-free glass obtained by the method of the present invention preferably has a viscosity of 10 4.9 dPa·s or more, 10 5.1 dPa·s or more, 10 5.2 dPa·s or more, especially 10 5.3 dPa·s or more. If so, devitrification is less likely to occur during forming, so it is easy to form a glass sheet using the overflow down-draw method, and the surface quality of the glass sheet can be improved. It should be noted that the viscosity at the liquidus temperature is an indicator of formability, and the higher the viscosity at the liquidus temperature, the better the formability.

[0074] Example

[0075] (Example 1)

[0076] Tables 1 and 2 show glasses of Examples (Sample Nos. 1 to 9) that can be used in the present invention.

[0077] [Table 1]

[0078]

[0079] [Table 2]

[0080]

[0081] The glass samples in Tables 1 and 2 were prepared as follows. First, a glass batch prepared with glass raw materials in the form of the composition in the table was added to a platinum crucible and melted at 1600°C to 1650°C for 24 hours. When the glass batch was melted, it was stirred with a platinum stirring rod to homogenize it. Next, the molten glass was poured onto a carbon plate and formed into a plate shape, and then annealed at a temperature near the annealing point for 30 minutes. For each sample obtained in this way, the density, Young's modulus, strain point, annealing point, and 10 4 dPa·s equivalent temperature, and 10 2.5 dPa·s equivalent temperature, liquidus temperature TL, viscosity at liquidus temperature Log 10 ηTL.

[0082] In addition, the density was measured by the well-known Archimedean method.

[0083] Young's modulus was measured by a bending resonance method.

[0084] The strain point and the annealing point were measured by the method of ASTM C336.

[0085] With high temperature viscosity 10 4 dPa·s, 10 2.5 The temperature equivalent to dPa·s was measured by a platinum ball pulling method.

[0086] The liquidus temperature TL is obtained by placing glass powder that passes through a 30-mesh standard sieve (500 μm) and remains on a 50-mesh (300 μm) sieve into a platinum boat, and keeping it in a temperature gradient furnace set at 1100°C to 1350°C for 24 hours. The platinum boat is then taken out and the temperature at which devitrification (crystalline foreign matter) is confirmed in the glass is measured.

[0087] Viscosity at liquidus temperature Log 10 ηTL measures the viscosity of glass at liquidus temperature using the platinum ball pulling method.

[0088] As can be seen from the table, the strain points of each sample No. 1 to 9 are above 735°C and the annealing points are above 785°C, so it is easy to reduce the thermal shrinkage of the glass. In addition, the liquidus temperature is below 1230°C and the viscosity at the liquidus temperature is 10 4.9 dPa·s or more, so devitrification is less likely to occur during molding. In particular, the viscosity of each sample No. 1, 2, 6 to 9 at the liquidus temperature is 10 5.2 dPa·s or more, and thus it is easy to form by the overflow down-draw method.

[0089] (Example 2)

[0090] A glass batch was prepared in such a manner as to become the glass of sample No. 6 in Table 1. Next, the glass batch was put into an electric melting furnace, melted at 1650°C, clarified and homogenized the molten glass in a clarification tank and a homogenization tank, and then adjusted to a viscosity suitable for forming in a tank. Next, the molten glass was formed into a plate shape by an overflow down-draw device and annealed in an annealing furnace. Thereafter, a glass plate having a size of 1500×1850×0.7 mm was produced by cutting the plate-shaped glass.

[0091] The length of the annealing furnace of the overflow down-drawing device was set to 5 m, and the temperatures of the multiple heaters arranged on the inner wall of the annealing furnace were appropriately adjusted, and the pulling speed of the plate glass was set to 350 cm / min, thereby setting the average cooling rate in the temperature range from the annealing point to (annealing point-100°C) to 385°C / min. The β-OH value of the glass plate obtained in this manner was 0.1 / mm, and the thermal shrinkage was 10 ppm.

[0092] Secondly, the melting conditions of the glass (temperature, time, etc.) were changed, and a glass plate was produced without changing the plate pulling speed and the average cooling rate. As a result, the β-OH value was 0.18 / mm and the thermal shrinkage rate exceeded 11ppm. The thermal shrinkage rate was restored to 10ppm by changing the plate pulling speed to 250cm / min and the average cooling rate in the temperature range from the annealing point to (annealing point - 100°C) to 275°C / min.

[0093] It should be noted that the drawing speed in the present invention refers to the speed at which the central part of the continuously formed plate-shaped glass in the plate width direction passes through the annealing zone. In this embodiment, the measurement is performed by making the measuring roller contact the middle point of the annealing zone in the central part in the plate width direction (a position corresponding to a temperature equivalent to the annealing point - 50°C). In addition, the average cooling speed refers to the speed calculated by calculating the time for the plate-shaped glass to pass through the area (annealing zone) corresponding to the temperature range from the annealing point to (annealing point - 100°C), and dividing the temperature difference in the annealing zone in the central part or the end by the passing time.

[0094] The β-OH value of glass was determined by measuring the transmittance of glass using FT-IR and using the following formula.

[0095] β-OH value = (1 / X)log(T1 / T2)

[0096] X: Glass wall thickness (mm)

[0097] T1: Reference wavelength 3846cm -1 Transmittance under (%)

[0098] T2: Hydroxyl absorption wavelength 3600cm -1 Minimum transmittance near (%)

[0099] In addition, the thermal shrinkage of the glass plate is measured by the following method. Figure 3 As shown in (a), a 160 mm × 30 mm short strip sample G is prepared as a glass plate sample. A mark M is formed at the two ends of the long side direction of the short strip sample G using #1000 water-resistant abrasive paper at a position 20 to 40 mm away from the edge. Then, as Figure 3As shown in (b), a short strip sample G with a mark M formed thereon is folded into two pieces along a direction perpendicular to the mark M to produce sample pieces Ga and Gb. Then, only one sample piece Gb is subjected to a heat treatment of increasing the temperature from room temperature to 500°C at 5°C / min, maintaining it at 500°C for 1 hour, and then cooling it at 5°C / min. After the above heat treatment, Figure 3 As shown in (c), when the unheat-treated sample Ga and the heat-treated sample Gb are arranged side by side, the displacement (ΔL1, ΔL2) of the marks M of the two sample pieces Ga and Gb is read by a laser microscope, and the thermal shrinkage rate is calculated by the following formula. It should be noted that l0 in the formula is the initial distance between the marks M.

[0100] Thermal shrinkage (ppm) = [{ΔL1 (μm) + ΔL2 (μm)} × 10 3 ] / l0(mm)

[0101] Based on the results of Example 2, it can be understood that when the thermal shrinkage of the glass plate is below 15 ppm and the thermal shrinkage deviation from the target value becomes larger, the thermal shrinkage of the glass plate can be corrected by adjusting the cooling rate of the plate glass in the annealing process without adjusting the β-OH value of the glass.

[0102] Description of Reference Numerals

[0103] 1 Electric melting furnace

[0104] 1a Raw material supply device

[0105] 1b Electrode

[0106] 2 Clarification tank

[0107] 3. Homogenization tank (mixing tank)

[0108] 3a Stirring wings

[0109] 4 cans

[0110] 5 formed body

[0111] 6~9 Transfer pipe

[0112] 10 Overflow pull-down device

[0113] 11 Edge Roller

[0114] 12 Annealing furnace

[0115] 13 Heater

[0116] 14 stretching roller

[0117] 15 Cooling Chamber

[0118] 16 Cutting Room

[0119] 16a Cutting device

[0120] Gm Molten glass

[0121] Gr Plate Glass

[0122] Gs Glass Plate

Claims

1. A method for manufacturing a glass plate, characterized in that: Including the following processes: A melting step of melting a glass batch prepared in such a way as to obtain a glass containing 3% by mass or less of B2O3 in an electric melting furnace; A forming step of forming the molten glass into a sheet of glass; an annealing step of annealing the plate glass in an annealing furnace; and The cutting step is to cut the annealed plate-shaped glass into a predetermined size to obtain a glass plate having a β-OH value of less than 0.2 / mm and a heat shrinkage of less than 15 ppm. The thermal shrinkage of the glass plate is measured. When the thermal shrinkage is greater than a target value, the annealing process is adjusted so that the average cooling rate in the temperature range from the annealing point to the annealing point-100°C is lowered within a range of 300°C / minute to 1000°C / minute. Conversely, when the thermal shrinkage is less than the target value, the annealing process is adjusted so that the average cooling rate in the temperature range from the annealing point to the annealing point-100°C is higher within a range of 300°C / minute to 1000°C / minute, thereby correcting the deviation of the thermal shrinkage from the target value.

2. The method for manufacturing a glass plate according to claim 1, wherein: It contains virtually no B2O3.

3. The method for manufacturing a glass plate according to claim 1 or 2, characterized in that: The cooling rate in the annealing step was adjusted so that the deviation of the thermal shrinkage ratio from the target value was ±1 ppm or less.

4. The method for manufacturing a glass plate according to claim 1 or 2, characterized in that: In the annealing step, the average cooling rate in the temperature range above the annealing point and the average cooling rate in the temperature range below the annealing point-100°C are 1.1 to 20 times the average cooling rate in the temperature range from the annealing point to the annealing point-100°C.

5. The method for manufacturing a glass plate according to claim 1 or 2, characterized in that: The forming process is draw-down forming, and the length of the annealing furnace is more than 3 m.

6. The method for manufacturing a glass plate according to claim 1 or 2, characterized in that: The glass plate has a size that the short side is 1500 mm or more and the long side is 1850 mm or more.

7. The method for manufacturing a glass plate according to claim 1 or 2, characterized in that: The glass plate has a thickness of 0.7 mm or less.