Preparation method of iron-based amorphous / nanocrystalline stress detection magnetic core based on wire cutting and its products

Through the preparation method of iron-based amorphous/nano-crystalline alloy magnetic core based on wire cutting, the crystallization problem caused by high temperature or strong strain in traditional processing methods is solved, and a high-precision and high-stability magnetic stress detection magnetic core is achieved. Preparation significantly improves the performance and applicability of the magnetic core.

CN115083717BActive Publication Date: 2024-11-15CHINA UNIV OF MINING & TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210797643.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-08
Publication Date
2024-11-15
Estimated Expiration
2042-07-08

AI Technical Summary

Technical Problem

During the processing process, existing iron-based amorphous alloys are prone to rapid relaxation and crystallization due to high temperature or strong strain, resulting in the disappearance of original excellent characteristics. It is difficult for traditional processing methods to effectively realize high-precision and high-stability magnetic stress detection. Core preparation.

Method used

Using the iron-based amorphous/nanocrystal stress detection magnetic core preparation method based on wire cutting, the amorphous/nanocrystal alloy strips are cut into thin sheets, stacked and applied pressure, and low vacuum impregnation and high temperature curing are carried out, combined with CAD drawings Wire cutting avoids the risk of temperature rise and oxidation caused by laser cutting, and retains the original excellent properties of the material.

Benefits of technology

It effectively avoids the risks of crystallization and oxidation, reduces processing costs, improves the integrity and performance of the magnetic core, significantly improves the saturation magnetization and coercivity, and has wide applicability, and is suitable for non-destructive detection of high-frequency magnetic stress.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115083717B_ABST
    Figure CN115083717B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing an iron-based amorphous / nanocrystalline stress detection magnetic core based on wire cutting and a product thereof, and relates to the technical field of stress magnetic anisotropy detection magnetic core preparation. The method comprises the following steps: cutting an amorphous / nanocrystalline alloy strip into amorphous / nanocrystalline alloy sheets with required shape and size, stacking to required number, fixing, and applying pressure in the stacking direction to obtain a sheet stack, and sequentially performing a low vacuum impregnation process and a high temperature curing process to obtain an amorphous / nanocrystalline alloy block; using CAD to draw a structural diagram of the required magnetic core, removing excess glue on the amorphous / nanocrystalline alloy block, correcting edges and corners, and performing wire cutting according to the structural diagram drawn by CAD; the invention can guarantee the original excellent performance of the iron-based amorphous nanocrystalline alloy to the greatest extent, thereby solving the problem of rapid tool loss caused by the high hardness of the iron-based amorphous nanocrystalline alloy in the traditional processing method, and reducing the processing cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of stress magnetic anisotropy detection magnetic core preparation, and in particular to a wire-cutting-based iron-based amorphous / nanocrystalline stress detection magnetic core preparation method and a product thereof. Background Art

[0002] With the development of science and technology, components made of ferromagnetic materials such as steel are increasingly used in bridges, buildings, aerospace and other fields. Real-time and non-destructive monitoring of their stress and working status is particularly important. Timely and accurate understanding of the internal stress change law of ferromagnetic components before an accident occurs and the development of stress non-destructive testing sensor cores are of great significance for reducing and preventing accidents.

[0003] At present, the sensors for stress testing are mainly resistance strain gauges, which are favored due to their small size, light weight and low price. However, resistance strain gauges are easily affected by the environment and have a short lifespan. Before use, the bracket must be rust-free, polished, and bonded, which is not only time-consuming and labor-intensive, but also depends on the operator's proficiency, the type of adhesive, the firmness of the bond, and other factors. These uncertainties greatly affect the reliability of the test results, making it difficult to monitor the internal stress of ferromagnetic components in a timely and accurate manner. The magnetic method for stress testing has great advantages: low price; small equipment, easy to carry, flexible testing; fast information acquisition speed; no surface treatment required; both contact measurement and non-contact and online measurement are possible. The use of magnetic methods for stress testing is also a hot topic in current research and has received widespread attention from engineering and technical personnel.

[0004] So far, the most commonly used sensor core is a four-level sensor core made of electrical pure iron, but the low magnetic permeability, high loss and poor measurement stability of electrical pure iron seriously restrict the accuracy of magnetic stress detection. For this reason, it is necessary to develop a sensor core with better performance. Iron-based amorphous alloy is a new type of soft magnetic alloy material, whose atomic arrangement has the characteristics of short-range order and long-range disorder. In addition, the ultra-fine grain structure of iron-based nanocrystals gives it the advantages of high initial magnetic permeability, low core loss rate and high stability. It is expected to replace traditional silicon steel, ferrite and other materials and be widely used in electronic products and devices with high precision and high stability requirements. Especially with the increase of frequency (>800 Hz), the low magnetic loss advantage of soft magnetic amorphous alloy compared with silicon steel is more obvious. Therefore, soft magnetic amorphous alloy is more suitable for use in magnetic stress non-destructive detection cores, thereby greatly reducing energy loss and improving detection accuracy.

[0005] It is difficult to effectively process amorphous alloys using traditional processing methods because amorphous alloys are metastable materials that will undergo rapid relaxation or even crystallization under high temperatures or strong strains, causing their original excellent properties to disappear.

[0006] Thermoplastic forming or blow molding can be used to process amorphous alloys, but these methods have very high requirements on material-related properties and require the material to have a wide supercooled liquid phase region. Therefore, the types of amorphous alloy materials that can be processed and formed by this method are limited, and the long forming time causes the material to have a high risk of oxidation and crystallization during the process. Summary of the invention

[0007] The purpose of the present invention is to provide a method for preparing an iron-based amorphous / nanocrystalline (iron-based amorphous or nanocrystalline) stress detection magnetic core based on wire cutting and its product, so as to solve the problems existing in the above-mentioned prior art.

[0008] To achieve the above object, the present invention provides the following solutions:

[0009] The present invention provides a method for preparing an iron-based amorphous / nanocrystalline stress detection magnetic core based on wire cutting, comprising the following steps:

[0010] (1) cutting the amorphous / nanocrystalline alloy strip into amorphous / nanocrystalline alloy sheets with desired shape and size;

[0011] (2) stacking the amorphous / nanocrystalline alloy sheets to a desired number, fixing them, and applying an adjustable pressure in the stacking direction to obtain a sheet stack;

[0012] (3) performing a low vacuum impregnation process and a high temperature curing process on the stack of thin sheets in sequence to obtain an amorphous / nanocrystalline alloy block;

[0013] (4) Using CAD to draw the structure diagram of the required magnetic core, removing excess glue on the amorphous / nanocrystalline alloy block, correcting the corners, and then performing wire cutting according to the structure diagram drawn by CAD to obtain an iron-based amorphous / nanocrystalline stress detection magnetic core based on wire cutting.

[0014] Furthermore, the composition of the amorphous / nanocrystalline alloy strip in step (1) is Fe 79 Si8B 13 Amorphous alloy or Fe 73.5 Si 13.5 B9Cu1Nb3 nanocrystalline alloy.

[0015] Furthermore, the thickness of the amorphous / nanocrystalline alloy strip in step (1) is 10 to 30 μm, preferably 20 μm, which is reasonable and easy to design.

[0016] Furthermore, the number of amorphous / nanocrystalline alloy sheets stacked in step (2) is 100 to 500 sheets, preferably 200 sheets, 400 sheets and 500 sheets.

[0017] Furthermore, the adjustable pressure applied in the stacking direction in step (2) is 10 to 200 MPa, which is highly flexible and can meet the actual pressure requirements.

[0018] Furthermore, the vacuum degree of the low vacuum dipping process in step (3) is less than 190 Pa, which is more conducive to the infiltration of the glue liquid; the curing temperature of the high temperature curing process is 150-170°C, and the curing time is 120-150 minutes.

[0019] Furthermore, the glue used in the low vacuum dipping process of step (3) is epoxy resin glue with the brand name E1228MR; it has good bonding effect, high impact strength, firmness and flexibility, and good solvent resistance.

[0020] Furthermore, in step (4), a wire cutting machine is used for wire cutting. The model of the wire cutting machine is JW7S-DK7735 cutting machine, which is small in size, safe and easy to operate.

[0021] The present invention also provides an iron-based amorphous / nanocrystalline stress detection magnetic core prepared by the preparation method based on wire cutting.

[0022] The magnetic core prepared by the method of the present invention has good integrity, a smooth and round cut surface and excellent comprehensive performance.

[0023] The present invention discloses the following technical effects:

[0024] The present invention rationally selects iron-based amorphous / nanocrystalline alloys and combines them with wire cutting to prepare magnetic cores, which can effectively avoid the risks of crystallization and oxidation of iron-based amorphous alloys in other cutting methods (for example, Fe 79 Si8B 13 The crystallization temperature of amorphous alloy is about 500℃, and the temperature of laser cutting is above 1200℃, so laser cutting can easily cause Fe 79 Si8B 13 Amorphous alloys will be amorphized, and rising temperatures will also lead to surface oxidation), which can maximize the original excellent performance of iron-based amorphous nanocrystalline alloys, thereby solving the problem of rapid tool loss caused by the high hardness of iron-based amorphous nanocrystalline alloys in traditional processing methods, reducing processing costs, and has high processing efficiency and wide applicability, which is conducive to widespread promotion and application.

[0025] Fe 79 Si8B 13 The magnetic core made of amorphous alloy has a smooth and round cutting surface, good integrity, and a saturation magnetization intensity of up to 1.63T; the coercive force is low, at 3A / m, and the overall performance is good.

[0026] Fe 73.5 Si 13.5The magnetic core made of B9Cu1Nb3 nanocrystalline alloy has a smooth and round cutting surface, good integrity, and a saturation magnetization intensity of up to 1.24T; the coercive force is low, at 0.58A / m, and the overall performance is good. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0028] Figure 1 is a flow chart of the preparation method of the present invention;

[0029] Figure 2 It is a structural schematic diagram of the magnetic core product of the present invention;

[0030] Figure 3 Fe prepared in Example 1 of the present invention 79 Si8B 13 Saturation magnetization intensity curve of amorphous alloy core;

[0031] Figure 4 Fe prepared in Example 1 of the present invention 79 Si8B 13 Coercivity curve of amorphous alloy core;

[0032] Figure 5 Fe prepared in Example 2 of the present invention 73.5 Si 13.5 Saturation magnetization curve of B9Cu1Nb3 nanocrystalline alloy;

[0033] Figure 6 Fe prepared in Example 2 of the present invention 73.5 Si 13.5 Coercivity curve of B9Cu1Nb3 nanocrystalline alloy. DETAILED DESCRIPTION

[0034] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0035] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0036] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0037] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0038] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0039] The present invention provides a method for preparing an iron-based amorphous / nanocrystalline stress detection magnetic core based on wire cutting, comprising the following steps:

[0040] (1) cutting the amorphous / nanocrystalline alloy strip into amorphous / nanocrystalline alloy sheets with desired shape and size;

[0041] (2) stacking amorphous / nanocrystalline alloy sheets to a desired number, fixing them, and applying an adjustable pressure in the stacking direction to obtain a sheet stack;

[0042] (3) performing a low vacuum impregnation process and a high temperature curing process on the stack of thin sheets in sequence to obtain an amorphous / nanocrystalline alloy block;

[0043] (4) Using a computer to perform CAD drawing, draw a structural diagram of the required sensor core, remove excess glue on the amorphous / nanocrystalline alloy block, correct the corners, and then perform wire cutting according to the structural diagram drawn by CAD to obtain an iron-based amorphous / nanocrystalline stress detection core based on wire cutting.

[0044] Theoretically, 3D printed magnetic cores can be made into any shape, but the powder needs to be prepared first during the printing process, and then printed using laser selective melting stereo molding technology. The printed magnetic cores have serious crystallization, thermal stress and residual stress, which makes its soft magnetic properties deteriorate sharply, and cracks and holes are difficult to avoid. It is still in the research stage and cannot be used in practice. Wire cutting is a subtractive manufacturing technology, while 3D printing is the opposite. It is additive manufacturing. Through different technical processes, the processed parts are stacked layer by layer to complete the processing. Compared with 3D printing, wire cutting does not have a heat-affected zone, and will not cause annealing and crystallization during the preparation of iron-based amorphous nanocrystalline alloys. It can well retain the original properties of iron-based amorphous and nanocrystalline, and has the advantages of low cost and mass production.

[0045] The preparation method of the present invention comprises the following steps: (1) the composition of the amorphous / nanocrystalline alloy strip is Fe 79 Si8B 13 Amorphous alloy and Fe 73.5 Si 13.5 B9Cu1Nb3 nanocrystalline alloy.

[0046] The thickness of the amorphous / nanocrystalline alloy strip in step (1) of the preparation method of the present invention is 10 to 30 μm, preferably 20 μm, which is reasonable and easy to design.

[0047] In the preparation method of the present invention, the number of amorphous / nanocrystalline alloy sheets stacked in step (2) is 100 to 500 sheets, preferably 200 sheets, 400 sheets and 500 sheets.

[0048] In the preparation method step (2) of the present invention, an adjustable pressure of 10 to 200 MPa is applied in the stacking direction, which has high flexibility and meets the pressure application requirements in practice.

[0049] The vacuum degree of the low vacuum dipping process in step (3) of the preparation method of the present invention is less than 190Pa, which is more conducive to the infiltration of the glue liquid; the curing temperature of the high temperature curing process is 150-170°C, and the curing time is 120-150min. After curing, the adhesive film has good toughness, high impact strength, good anti-vibration effect, low expansion coefficient, and high temperature resistance.

[0050] The glue used in the low vacuum dipping process of step (3) of the preparation method of the present invention is epoxy resin glue with the brand E1228MR; it has good bonding effect, high impact strength, firmness and flexibility, and good solvent resistance.

[0051] In step (4) of the preparation method of the present invention, a wire cutting machine is used for wire cutting. The model of the wire cutting machine is a JW7S-DK7735 cutting machine, which is small in size, safe, and easy to operate.

[0052] The present invention also provides an iron-based amorphous / nanocrystalline stress detection magnetic core prepared by the preparation method based on wire cutting.

[0053] The magnetic core prepared by the method of the present invention has good integrity, a smooth and round cut surface and excellent comprehensive performance.

[0054] The surface smoothing method in the embodiment of the present invention is a conventional technical means in the art and is not the focus of the present invention, so it will not be described in detail here.

[0055] The method of using CAD to draw the structural diagram of the required magnetic core in the embodiment of the present invention is a conventional technical means in the art, and is not the focus of the present invention, and will not be described in detail here.

[0056] The preparation method flow chart of the present invention is shown in Figure 1 , the structural schematic diagram of the magnetic core product of the present invention is shown in Figure 2 .

[0057] Example 1 Preparation of Fe 79 Si8B 13 Amorphous alloy core:

[0058] (1) Select Fe with a saturation magnetization of 1.63T, a coercive force of 3A / m, and a thickness of 20μm 79 Si8B 13 A roll of amorphous alloy is cut into thin sheets with a width of 20cm×20cm;

[0059] (2) After selecting 500 pieces and stacking them, put them into low vacuum dipping (vacuum degree less than 190Pa) using epoxy resin glue with brand E1228MR;

[0060] (3) Apply an adjustable pressure of 100 to 200 MPa in the stacking direction, set the curing temperature to 160°C, and the curing time to 150 min;

[0061] (4) Use CAD to draw Figure 2 The model diagram shown,

[0062] The core dimensions are:

[0063] Base radius 12mm;

[0064] Base thickness 10.6877mm;

[0065] The radius of the base hole is 2mm;

[0066] Probe height 25.4437mm;

[0067] The inner diameter of the quadruped is 6.8593mm;

[0068] The central angle of the four legs is 45 degrees;

[0069] (5) Use the wire cutting machine model JW7S-DK7735 to cut according to the CAD drawing, and then smooth the surface after cutting to obtain Fe 79 Si8B 13 Amorphous alloy core, Fe 79 Si8B 13 The saturation magnetization intensity curve of amorphous alloy core is shown in Figure 3 , Fe 79 Si8B 13 The coercivity curve of amorphous alloy core is shown in Figure 4 Its saturation magnetization can reach 1.63T; its coercive force is low, at 3A / m, and its comprehensive performance is good.

[0070] Example 2 Preparation of Fe 73.5 Si 13.5 B9Cu1Nb3 nanocrystalline alloy core

[0071] (1) Select Fe with a saturation magnetization of 1.24T, a coercive force of 0.58A / m, and a thickness of 25μm 73.5 Si 13.5 A roll of B9Cu1Nb3 nanocrystalline alloy was cut into thin sheets with a width of 20 cm × 20 cm;

[0072] (2) After selecting 400 pieces and stacking them, put them into low vacuum dipping (vacuum degree less than 190Pa) using epoxy resin glue with brand E1228MR;

[0073] (3) Apply a pressure of 180 MPa in the stacking direction, set the curing temperature to 160 °C, and the curing time to 150 min;

[0074] (4) Use CAD to draw Figure 2 The model diagram shown,

[0075] The core dimensions are:

[0076] Base radius 12mm;

[0077] Base thickness 10.6877mm;

[0078] The radius of the base hole is 2mm;

[0079] Probe height 25.4437mm;

[0080] The inner diameter of the quadruped is 6.8593mm;

[0081] The central angle of the four legs is 45 degrees.

[0082] (5) Use the wire cutting machine model JW7S-DK7735 to cut according to the CAD drawing, and then smooth the surface after cutting to obtain Fe 73.5 Si 13.5 B9Cu1Nb3 nanocrystalline alloy core, Fe 73.5 Si 13.5 The saturation magnetization curve of B9Cu1Nb3 nanocrystalline alloy is shown in Figure 5 , Fe 73.5 Si 13.5 The coercivity curve of B9Cu1Nb3 nanocrystalline alloy is shown in Figure 6 Its saturation magnetization can reach 1.24T; its coercive force is low, at 0.58A / m, and its comprehensive properties are excellent.

[0083] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing an iron-based amorphous / nanocrystalline stress detection magnetic core based on wire cutting, characterized in that: The following steps are involved: (1) cutting the amorphous / nanocrystalline alloy strip into amorphous / nanocrystalline alloy sheets with desired shape and size; (2) stacking the amorphous / nanocrystalline alloy sheets to a desired number, fixing them, and applying pressure in the stacking direction to obtain a sheet stack; (3) performing a low vacuum impregnation process and a high temperature curing process on the stack of thin sheets in sequence to obtain an amorphous / nanocrystalline alloy block; (4) using CAD to draw a structural diagram of the required magnetic core, removing excess glue from the amorphous / nanocrystalline alloy block, correcting the corners, and then performing wire cutting according to the structural diagram drawn by CAD to obtain an iron-based amorphous / nanocrystalline stress detection magnetic core based on wire cutting; The composition of the amorphous / nanocrystalline alloy strip in step (1) is Fe 79 Si8B 13 Amorphous alloy or Fe 73.5 Si 13.5 B9Cu1Nb3 nanocrystalline alloy; The pressure applied in the stacking direction in step (2) is 10 to 200 MPa; The vacuum degree of the low vacuum dipping process in step (3) is less than 190 Pa; the curing temperature of the high temperature curing process is 150-170° C., and the curing time is 120-150 min.

2. The preparation method according to claim 1, characterized in that: The thickness of the amorphous / nanocrystalline alloy strip in step (1) is 10 to 30 μm.

3. The preparation method according to claim 1, characterized in that: The number of amorphous / nanocrystalline alloy sheets stacked in step (2) is 100 to 500 sheets.

4. An iron-based amorphous / nanocrystalline stress detection magnetic core based on wire cutting, characterized in that: The compound is prepared by the preparation method according to any one of claims 1 to 3.