A P-type solar cell and its manufacturing method, battery assembly and photovoltaic system

By providing a doped polysilicon layer on the first side of the solar cell and an aluminum oxide layer on the second side, and using laser scanning to form the boron doped layer and slotting, the double-sided radiation resistance effect of the solar cell is achieved and the problem is solved Attenuation problems in high UV radiation environments, reducing costs and improving photoelectric conversion efficiency.

CN115084299BActive Publication Date: 2024-10-01GUANGDONG AIKO SOLAR ENERGY TECH CO LTD +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210716869.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-23
Publication Date
2024-10-01
Estimated Expiration
2042-06-23

AI Technical Summary

Technical Problem

Existing solar cells have high attenuation in high ultraviolet radiation environments and insufficient radiation resistance.

Method used

The production method of P-type solar cells is adopted, which includes providing a doped polysilicon layer on the first side of the solar cell, an aluminum oxide layer on the second side, and forming a boron doped layer and slotting through laser scanning to form a double-sided resistor. irradiate the structure while repairing the lattice damage introduced by the laser.

Benefits of technology

The radiation resistance of the solar cell is improved, the attenuation caused by radiation is reduced, the cost is lower, and the photoelectric conversion efficiency is higher.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115084299B_ABST
    Figure CN115084299B_ABST
Patent Text Reader

Abstract

The present application is applicable to the field of solar cell technology, and provides a P-type solar cell and its manufacturing method, a battery assembly and a photovoltaic system. The manufacturing method of a P-type solar cell includes: providing a P-type silicon wafer; etching and cleaning the P-type silicon wafer; preparing a tunneling oxide layer on the first side of the P-type silicon wafer; preparing a doped polysilicon layer on the tunneling oxide layer; preparing an aluminum oxide layer on the second side of the P-type silicon wafer; preparing a first passivation layer on the doped polysilicon layer; preparing a second passivation layer on the aluminum oxide layer; locally covering a boron source layer on the second passivation layer; using a laser to scan the boron source layer to form a boron doped layer, and simultaneously forming a laser groove; cleaning the boron doped layer; forming a first electrode on the first side, the first electrode passes through the first passivation layer to contact the doped polysilicon layer; forming a second electrode on the second side, the second electrode contacts the boron doped layer through the grooved area. In this way, double-sided radiation resistance and repair of laser-induced lattice damage can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of solar cells, and in particular relates to a P-type solar cell and a manufacturing method thereof, a cell assembly and a photovoltaic system. Background Art

[0002] Solar cell power generation is a sustainable source of clean energy. It uses the photovoltaic effect of semiconductor pn junction to convert sunlight into electrical energy.

[0003] In the related art, a silicon nitride layer is usually set on the solar cell, or a silicon oxide layer and a silicon nitride layer are set on the solar cell to reduce the reflection of sunlight. However, this causes the solar cell to attenuate too much in an environment with strong ultraviolet radiation such as plateaus, sea surfaces or space, resulting in a high risk of failure.

[0004] Based on this, how to improve the radiation resistance of solar cells has become an urgent problem to be solved. Summary of the invention

[0005] The present application provides a P-type solar cell and a manufacturing method thereof, a battery assembly and a photovoltaic system, aiming to solve the problem of how to improve the radiation resistance effect of solar cells.

[0006] In a first aspect, the present application provides a method for manufacturing a P-type solar cell, comprising:

[0007] Provide P-type silicon wafers;

[0008] Etching and cleaning the P-type silicon wafer;

[0009] Preparing a tunneling oxide layer on the first surface of the P-type silicon wafer;

[0010] preparing a doped polysilicon layer on the tunnel oxide layer;

[0011] preparing an aluminum oxide layer on the second surface of the P-type silicon wafer;

[0012] preparing a first passivation layer on the doped polysilicon layer;

[0013] preparing a second passivation layer on the aluminum oxide layer;

[0014] locally covering the second passivation layer with a boron source layer;

[0015] Scanning a boron source layer using a laser to form a boron doped layer and simultaneously forming a laser groove;

[0016] cleaning the boron-doped layer;

[0017] forming a first electrode on the first surface, wherein the first electrode passes through the first passivation layer and contacts the doped polysilicon layer;

[0018] A second electrode is formed on the second surface, and the second electrode contacts the boron doped layer through the groove region.

[0019] Optionally, before the step of forming the first electrode on the first surface, the manufacturing method includes:

[0020] Performing laser film opening on the first passivation layer;

[0021] Forming a first electrode on the first surface includes:

[0022] forming the first electrode by copper electroplating;

[0023] A second electrode is formed on the second surface, comprising:

[0024] The second electrode is formed by copper electroplating.

[0025] Optionally, forming a first electrode on the first surface includes:

[0026] forming the first electrode on the first surface using silver paste;

[0027] Forming a second electrode on the second surface includes:

[0028] The second electrode is formed by copper electroplating.

[0029] Optionally, forming a first electrode on the first surface includes:

[0030] forming the first electrode on the first surface using silver paste;

[0031] Forming a second electrode on the second surface includes:

[0032] The second electrode is formed on the second surface using aluminum paste.

[0033] Optionally, the second electrode includes a fine grid, a main grid and a pad, the fine grid is an aluminum conductor, and the second electrode is formed on the second surface using aluminum paste, including:

[0034] Using aluminum paste to form the aluminum conductor on the second surface;

[0035] The main grid and the pad are formed on the aluminum conductor, wherein the main grid includes a first silver conductive portion, and / or the pad includes a second silver conductive portion.

[0036] Optionally, the second electrode includes an aluminum fine grid and a silver fine grid, and the second electrode is formed on the second surface using an aluminum paste, comprising:

[0037] Using aluminum paste to form the aluminum fine grid on the second surface, wherein the aluminum fine grid is in contact with the P-type silicon wafer through the grooved area;

[0038] The silver fine grid is formed on the aluminum fine grid, and the aluminum fine grid and the silver fine grid form a composite fine grid.

[0039] Optionally, forming the silver fine grid on the aluminum fine grid comprises:

[0040] The silver fine grid covers the top and side surfaces of the aluminum fine grid.

[0041] Optionally, the aluminum fine grid is covered to a thickness less than 1 / 2 of the thickness of the silver fine grid.

[0042] Optionally, the difference between the width of the silver fine grid and the width of the aluminum fine grid is 5 μm-20 μm.

[0043] Optionally, the thickness of the silver fine grid is 5 μm-10 μm.

[0044] Optionally, the aluminum fine grid has a thickness of 10 μm-40 μm.

[0045] In a second aspect, the P-type solar cell provided in the present application is manufactured using any of the above-mentioned methods for manufacturing a P-type solar cell.

[0046] In a third aspect, the present application provides a P-type solar cell, comprising:

[0047] P-type silicon wafer;

[0048] A tunneling oxide layer, a doped polysilicon layer, a first passivation layer and a first electrode are sequentially stacked on the first surface of the P-type silicon wafer, wherein the first electrode passes through the first passivation layer and contacts the doped polysilicon;

[0049] An aluminum oxide layer, a second passivation layer and a second electrode are sequentially stacked on the second surface of the P-type silicon wafer, the aluminum oxide layer and the second passivation layer are provided with a grooved area, a boron-doped layer is formed in the grooved area, and the second electrode contacts the boron-doped layer through the grooved area.

[0050] Optionally, both the first electrode and the second electrode are electroplated copper electrodes.

[0051] Optionally, the first electrode is a silver electrode, and the second electrode is an electroplated copper electrode.

[0052] Optionally, the first electrode is a silver electrode, and the second electrode includes an aluminum electrode.

[0053] Optionally, the second electrode is a composite fine gate, the composite fine gate includes an aluminum fine gate and a silver fine gate, the aluminum fine gate is in contact with the P-type silicon wafer through a grooved area, and the silver fine gate is arranged on a side of the aluminum fine gate away from the P-type silicon wafer.

[0054] Optionally, the silver fine grid covers the top surface and side surfaces of the aluminum fine grid.

[0055] Optionally, the difference between the width of the silver fine grid and the width of the aluminum fine grid is 5 μm-20 μm.

[0056] Optionally, the thickness of the silver fine grid is 5 μm-10 μm.

[0057] Optionally, the aluminum fine grid has a thickness of 10 μm-40 μm.

[0058] In a third aspect, the battery assembly provided by the present application includes any of the above-mentioned P-type solar cells.

[0059] In a fourth aspect, the photovoltaic system provided in the present application includes the above-mentioned battery assembly.

[0060] The P-type solar cell and its manufacturing method, battery assembly and photovoltaic system provided by the present application have a doped polysilicon layer on the first side and an aluminum oxide layer on the second side, so the manufactured P-type solar cell can be radiation-resistant on both sides, thereby reducing the attenuation caused by radiation. At the same time, laser grooving and laser doping will cause certain damage to the battery cell, and the process of forming the electrode will repair the lattice damage introduced by the laser. In this way, the cost of manufacturing P-type solar cells is low and the photoelectric conversion efficiency is high. BRIEF DESCRIPTION OF THE DRAWINGS

[0061] Figure 1 is a schematic flow chart of a method for manufacturing a P-type solar cell according to an embodiment of the present application;

[0062] Figure 2 is a schematic structural diagram of a P-type solar cell according to an embodiment of the present application;

[0063] Figure 3 is a schematic flow chart of a method for manufacturing a P-type solar cell according to an embodiment of the present application;

[0064] Figure 4 is a schematic flow chart of a method for manufacturing a P-type solar cell according to an embodiment of the present application;

[0065] Figure 5 is a schematic flow chart of a method for manufacturing a P-type solar cell according to an embodiment of the present application;

[0066] Figure 6 is a schematic flow chart of a method for manufacturing a P-type solar cell according to an embodiment of the present application;

[0067] Figure 7 is a schematic flow chart of a method for manufacturing a P-type solar cell according to an embodiment of the present application;

[0068] Figure 8 is a schematic structural diagram of a P-type solar cell according to an embodiment of the present application;

[0069] Description of main component symbols:

[0070] P-type solar cell 10, P-type silicon wafer 101, tunneling oxide layer 11, doped polysilicon layer 12, first passivation layer 13, first electrode 14, aluminum oxide layer 15, second passivation layer 16, second electrode 17, aluminum fine gate 171, silver fine gate 172, boron doped layer 189. DETAILED DESCRIPTION

[0071] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0072] The radiation resistance of solar cells in the related art is poor. Since the present application is provided with a doped polysilicon layer and an aluminum oxide layer, it can be double-sided and radiation-resistant, thereby reducing the attenuation caused by radiation. At the same time, laser grooving and laser doping will cause certain damage to the cell. The process of forming the electrode will repair the lattice damage introduced by the laser. In this way, the cost of making P-type solar cells is low and the photoelectric conversion efficiency is high.

[0073] Embodiment 1

[0074] See also Figure 1 and Figure 2 The method for manufacturing the P-type solar cell 10 of this embodiment includes:

[0075] Step S11: providing a P-type silicon wafer 101;

[0076] Step S12: etching and cleaning the P-type silicon wafer 101;

[0077] Step S13: preparing a tunneling oxide layer 11 on the first surface of the P-type silicon wafer 101;

[0078] Step S14: preparing a doped polysilicon layer 12 on the tunneling oxide layer 11;

[0079] Step S15: preparing an aluminum oxide layer 15 on the second surface of the P-type silicon wafer 101;

[0080] Step S16: preparing a first passivation layer 13 on the doped polysilicon layer 12;

[0081] Step S17: preparing a second passivation layer 16 on the aluminum oxide layer 15;

[0082] Step S18: locally covering the second passivation layer 16 with a boron source layer;

[0083] Step S19: using laser scanning to form a boron doped layer 189 on the boron source layer, and simultaneously forming a laser groove;

[0084] Step S20: cleaning the boron doped layer 189;

[0085] Step S22: forming a first electrode 14 on the first surface, wherein the first electrode 14 passes through the first passivation layer 13 and contacts the doped polysilicon layer 12;

[0086] Step S23: forming a second electrode 17 on the second surface, wherein the second electrode 17 contacts the boron doped layer 189 through the grooved region.

[0087] In the manufacturing method of the P-type solar cell 10 of the embodiment of the present application, since the first surface is provided with a doped polysilicon layer 12 and the second surface is provided with an aluminum oxide layer 15, the manufactured P-type solar cell 10 can be radiation-resistant on both sides, thereby reducing the attenuation caused by radiation. At the same time, laser grooving and laser doping cause certain damage to the cell, and the process of forming the electrode will repair the lattice damage introduced by the laser. In this way, the cost of manufacturing the P-type solar cell 10 is low and the photoelectric conversion efficiency is high.

[0088] Specifically, in step S12, the first surface can be flattened by etching and cleaning, so that the doped polysilicon layer 12 has better passivation. The light-facing surface can also be textured by etching and cleaning to achieve a light trapping effect and reduce the reflection loss of sunlight. The light-facing surface can be the first surface and / or the second surface.

[0089] Specifically, in step S13, the tunnel oxide layer 11 can be formed by thermal oxidation, chemical oxidation, PECVD or ALD. The thickness of the tunnel oxide layer 11 is 0.5nm-5nm. For example, 0.5nm, 1nm, 3nm, 4nm, 5nm. The thickness of the tunnel oxide layer 11 is preferably 0.7nm-1.5nm. For example, 0.7nm, 1nm, 1.2nm, 1.5nm.

[0090] Specifically, in step S13, the tunneling oxide layer 11 includes one or more of a silicon oxide layer and an aluminum oxide layer 15. Preferably, the tunneling oxide layer 11 is a silicon oxide layer.

[0091] Furthermore, the tunnel oxide layer 11 can be prepared by thermal oxidation and solution oxidation. Furthermore, in the case of preparing the tunnel oxide layer 11 by thermal oxidation, oxygen and nitrogen can be introduced at 500-800° C. for thermal oxidation for 5-60 minutes, thereby forming a silicon oxide layer on the P-type silicon wafer 101. In the case of preparing the tunnel oxide layer 11 by solution oxidation, a solution ratio of 4:1 to 1:4 can be used. 2 SO 4 With H 2 O 2 The mixed solution of the solutions is oxidized to form a silicon oxide layer on the P-type silicon wafer 101 .

[0092] Furthermore, the tunnel oxide layer 11 may also be prepared by PECVD.

[0093] Specifically, in step S14, the thickness of the doped polysilicon layer 12 is 20nm-400nm, such as 20nm, 50nm, 100nm, 300nm, 400nm. The thickness of the doped polysilicon layer 12 is preferably 80nm-180nm, such as 80nm, 100nm, 120nm, 150nm, 180nm.

[0094] Specifically, in step S14, the tunneling layer may be entirely covered with a doped polysilicon layer 12, and when the P-type silicon wafer 101 is sintered, the first electrode 14 burns through the first passivation layer 13 to contact the doped polysilicon layer 12. In this way, the doped polysilicon layer 12 is entirely covered, and the electrode does not pass through, so the radiation resistance effect is better. Moreover, since the first electrode 14 is in contact with the polysilicon, the passivation effect is better.

[0095] It can be understood that in other embodiments, the doped polysilicon layer 12 may also cover a portion of the tunneling layer.

[0096] Specifically, in step S14, the doped polysilicon layer 12 may be a phosphorus-doped single crystal silicon layer with a square resistance of less than 60 ohm / squ. In this way, fewer first electrodes 14 may be used, thereby saving costs.

[0097] Specifically, in step S14, a doped polysilicon layer 12 can be prepared on the tunnel oxide layer 11 using a PECVD (Plasma Enhanced Chemical Vapor Deposition) device or a LPCVD (Low Pressure Chemical Vapor Deposition) device or a PVD (Physical Vapor Deposition) device. In this way, the temperature required for deposition using PECVD equipment is relatively low, which can save energy and reduce the lifetime decay of minority carriers in silicon wafers caused by high temperatures. The LPCVD equipment has better step coverage, and the deposition rate and output are higher. PVD is a chain transmission, which has higher production capacity and lower cost when depositing thin films. This is conducive to improving the quality of batteries and reducing costs.

[0098] Specifically, in step S15, the thickness of the aluminum oxide layer 15 is 1 nm-30 nm, such as 1 nm, 2 nm, 10 nm, 15 nm, 28 nm, and 30 nm. The thickness of the aluminum oxide layer 15 is preferably 2 nm-6 nm, such as 2 nm, 3 nm, 4 nm, 5 nm, and 6 nm.

[0099] Specifically, in step S15, the aluminum oxide layer 15 can be prepared on the second surface of the P-type silicon wafer 101 using PECVD equipment, ALD (Atomic Layer Deposition) equipment or PVD equipment. In this way, the temperature required for deposition using PECVD equipment is relatively low, which can save energy and reduce the decay of minority carrier lifetime in the silicon wafer caused by high temperature. The film layer made by the ALD equipment has good uniformity, is dense and has no holes, and the thickness of the film is precisely controlled. In this way, it is beneficial to improve the quality of the battery and reduce the cost.

[0100] Please note that step S16 may be before or after step S15. The process in the figure is only an example and is not intended to limit the order of the steps. The order of the steps may be disrupted in a reasonable manner.

[0101] Specifically, in step S16, the first passivation layer 13 can be prepared by ALD, PECVD or PVD processes. The thickness of the first passivation layer 13 is 10nm-200nm. For example, 10nm, 50nm, 100nm, 150nm, 200nm. The thickness of the first passivation layer 13 is preferably 50nm-100nm. For example, 50nm, 60nm, 80nm, 100nm.

[0102] Specifically, in step S16 , the first passivation layer 13 includes a first silicon nitride layer. Step S16 includes: preparing the first silicon nitride layer on the doped polysilicon layer 12 by using PECVD equipment.

[0103] Specifically, in step S17, the second passivation layer 16 may be prepared by ALD, PECVD or PVD processes. The thickness of the second passivation layer 16 is 10 nm-200 nm, for example, 10 nm, 50 nm, 100 nm, 150 nm, 200 nm, preferably 50 nm-100 nm, for example, 50 nm, 60 nm, 80 nm, 100 nm.

[0104] Specifically, in step S17 , the second passivation layer 16 includes a second silicon nitride layer. Step S17 includes: preparing the second silicon nitride layer on the aluminum oxide layer 15 by using PECVD equipment.

[0105] In this way, by using the silicon nitride layer to reduce reflection, the loss of sunlight can be reduced, the utilization rate of sunlight can be increased, and thus the photoelectric conversion efficiency can be improved. At the same time, hydrogen ions will combine with dangling bonds, reduce recombination centers, and have a passivation effect. Moreover, the PECVD equipment makes the silicon nitride layer have fewer pinholes and is not easy to crack, which is conducive to improving the film quality of the silicon nitride layer.

[0106] Furthermore, the silicon nitride layer may be one layer or multiple layers. In the case where the silicon nitride layer is multiple layers, a refractive index gradient may be formed between two adjacent silicon nitride layers. In this way, gradient extinction is achieved through the refractive index gradient, further improving the utilization rate of sunlight.

[0107] Specifically, in step S18, the boron source may be covered on the area to be doped on the second passivation layer 16 by spin coating or screen printing and drying, or a boron source layer may be formed by CVD or PVD.

[0108] Specifically, in step S18, the thickness of the boron source layer is less than 10 μm, such as 10 μm, 9 μm, 8 μm, or 7 μm. Preferably, the thickness of the boron source layer is less than 3 μm, such as 3 μm, 2 μm, 1 μm, or 0.5 μm.

[0109] Specifically, in step S19, the pulse width of the laser is greater than 1ns or it is a continuous laser. The scanning speed is 5-70m / s. The energy density formed on the boron source is greater than 0.1μJ / cm 2 In this way, a boron doped layer 189 with a depth greater than 0.2 um is formed.

[0110] Specifically, in step S19, a laser may be used to open dot-shaped holes on the second passivation layer 16 and the aluminum oxide layer 15 of the P-type silicon wafer 101. Further, the diameter of the dot-shaped holes is 25μm-45μm. For example, 25μm, 27μm, 30μm, 32μm, 35μm, 40μm, 45μm. Further, the spacing between adjacent dot-shaped holes in the length direction of the fine gate is 400μm-800μm. For example, 400μm, 420μm, 500μm, 600μm, 700μm, 780μm, 800μm. Further, the spacing between adjacent dot-shaped holes in the width direction of the fine gate is 500μm-1000μm. For example, 500μm, 520μm, 600μm, 800μm, 980μm, 1000μm.

[0111] Specifically, in step S19, a laser may be used to open discontinuous linear grooves on the second passivation layer 16 and the aluminum oxide layer 15 of the P-type silicon wafer 101. Further, the length of the linear groove is 0.1mm-0.5mm. For example, 0.1mm, 0.2mm, 0.3mm, 0.4mm, 0.5mm. Further, the width of the linear groove is 25μm-45μm. For example, 25μm, 28μm, 30μm, 35μm, 38μm, 40μm, 45μm. Further, the spacing between adjacent linear grooves in the length direction of the fine gate is 0.2mm-1mm. For example, 0.2mm, 0.4mm, 0.8mm, 1mm. Further, the spacing between adjacent linear grooves in the width direction of the fine gate is 0.5mm-1mm. For example, 0.5mm, 0.6mm, 0.8mm, 1mm.

[0112] Specifically, in step S19, a laser may be used to open continuous linear grooves on the second passivation layer 16 and the aluminum oxide layer 15 of the P-type silicon wafer 101. Specifically, the groove width is 2 μm-100 μm. For example, 2 μm, 5 μm, 8 μm, 15 μm, 30 μm, 70 μm, 100 μm. Preferably, the groove area width is 10 μm-35 μm. For example, 10 μm, 12 μm, 15 μm, 20 μm, 28 μm, 30 μm, 35 μm.

[0113] Specifically, in step S20, an alkaline solution is used for cleaning. The alkaline solution is, for example, KOH solution, NaOH solution, TMAH solution, etc. Alkaline chemicals and hydrogen peroxide can also be used for cleaning. Specifically, in step S22, screen printing can be used to form the first electrode 14. In this way, the efficiency and accuracy of electrode production are higher, which is conducive to improving the quality of the battery. In other embodiments, the first electrode 14 can also be formed by processes such as electroplating copper, sputtering, and vacuum evaporation.

[0114] Specifically, in step S22, the width of the first electrode 14 is 2 μm-400 μm, such as 2 μm, 10 μm, 100 μm, 300 μm, 400 μm. The width of the first electrode 14 is preferably 10 μm-70 μm, such as 10 μm, 20 μm, 50 μm, 65 μm, 70 μm.

[0115] Specifically, in step S22, the thickness of the first electrode 14 is 2 μm-40 μm, such as 2 μm, 10 μm, 15 μm, 30 μm, 40 μm. The thickness of the first electrode 14 is preferably 5 μm-20 μm, such as 5 μm, 10 μm, 15 μm, 20 μm.

[0116] Specifically, in step S23, screen printing can be used to form the second electrode 17. In this way, the efficiency and accuracy of electrode manufacturing are higher, which is conducive to improving the quality of the battery. In other embodiments, the second electrode 17 can also be formed by electroplating copper, sputtering, vacuum evaporation and other processes.

[0117] Specifically, in step S23, the width of the second electrode 17 is 2 μm-400 μm, for example, 2 μm, 10 μm, 100 μm, 300 μm, 400 μm. The width of the second electrode 17 is preferably 10 μm-70 μm, for example, 10 μm, 20 μm, 50 μm, 65 μm, 70 μm.

[0118] Specifically, in step S23, the thickness of the second electrode 17 is 2 μm-40 μm, such as 2 μm, 10 μm, 15 μm, 30 μm, 40 μm. The thickness of the second electrode 17 is preferably 5 μm-20 μm, such as 5 μm, 10 μm, 15 μm, 20 μm.

[0119] Specifically,

[0120] See also Figure 3 Optionally, before step S22, the manufacturing method includes:

[0121] Step S21: laser opening the first passivation layer 13;

[0122] Step S22 includes:

[0123] Step S221: forming a first electrode 14 by copper electroplating;

[0124] Step S23 includes

[0125] Step S231: forming the second electrode 17 by copper electroplating.

[0126] In this way, copper electrodes are formed on both sides of the P-type silicon wafer 101 through the copper electroplating process, which has a better conductive effect and can reduce costs compared to using silver electrodes.

[0127] Specifically, nickel, chromium, titanium, or tungsten electrodes may be used as seed layers or protective layers for electroplating copper electrodes.

[0128] Specifically, step S21 can be performed simultaneously with step S19. In this way, double-sided grooving can be performed while laser doping is performed, which is more efficient. It is understood that step S21 can be performed separately from step S19.

[0129] Specifically, step S221 and step S231 can be performed simultaneously. In this way, double-sided copper electrodes can be prepared simultaneously, which is more efficient. It can be understood that step S221 and step S231 can also be performed in steps. The order of each step is not limited here.

[0130] See also Figure 4 Optionally, step S22 includes:

[0131] Step S222: forming a first electrode 14 on the first surface using silver paste;

[0132] Step S23 includes

[0133] Step S232: forming the second electrode 17 by copper electroplating.

[0134] In this way, the first electrode 14 is a silver electrode and the second electrode 17 is a copper electrode, which has a better conductive effect and can reduce the cost compared with double-sided silver electrodes.

[0135] Specifically, in step S222, silver paste may be screen printed to form the first electrode 14. In this way, the technical control difficulty of double-sided electroplating can be reduced to a certain extent. It can be understood that the silver paste is sintered to form the first electrode 14, burn through the first passivation layer 13, and contact the doped polysilicon layer 12.

[0136] Specifically, in step S232, nickel, chromium, titanium, or tungsten electrodes may be used as seed layers or protective layers for electroplating copper electrodes.

[0137] See also Figure 5 Optionally, step S22 includes:

[0138] Step S223: forming a first electrode 14 on the first surface using silver paste;

[0139] Step S23 includes

[0140] Step S233: forming a second electrode 17 on the second surface using aluminum paste.

[0141] In this way, the conductive effect is better and the cost can be reduced compared to double-sided silver electrodes.

[0142] Specifically, in step S223, silver paste may be screen-printed to form the first electrode 14. In this way, the efficiency and precision of manufacturing the first electrode 14 are higher.

[0143] Specifically, in step S233, aluminum paste may be screen-printed to form the second electrode 17. In this way, the efficiency and accuracy of manufacturing the second electrode 17 are higher.

[0144] It is understood that the first electrode 14 and the second electrode 17 may be formed by sintering after applying the slurry.

[0145] See also Figure 6 Optionally, the second electrode 17 includes a fine grid, a main grid and a pad, the fine grid is an aluminum conductor, and step S233 includes:

[0146] Step S2331: using aluminum paste to form an aluminum conductor on the second surface;

[0147] Step S2332: forming a main grid and a pad on the aluminum conductor, wherein the main grid includes a first silver conductive portion, and / or the pad includes a second silver conductive portion.

[0148] In this way, at least one of the main grid and the pad includes a silver conductive portion, which facilitates welding when manufacturing a battery assembly.

[0149] Specifically, in step S2331, the aluminum conductor may be formed by screen printing; the aluminum conductor may also be formed by sputtering, vacuum evaporation or other processes.

[0150] Specifically, in step S2332, the main grid may include the first silver conductive portion, and the pad may include the second silver conductive portion; the main grid may include the first silver conductive portion, and the pad may not include the second silver conductive portion; the main grid may not include the first silver conductive portion, and the pad may include the second silver conductive portion. Further, in the case where the main grid includes the first silver conductive portion, part of the main grid may be the first silver conductive portion, or the entire main grid may be the first silver conductive portion. In the case where the pad includes the second silver conductive portion, part of the pad may be the second silver conductive portion, or the entire pad may be the second silver conductive portion.

[0151] Specifically, in step S2332, the silver conductive portion may be formed by screen printing; the silver conductive portion may also be formed by sputtering, vacuum evaporation or other processes.

[0152] See also Figure 7 and Figure 8 Optionally, the second electrode 17 includes an aluminum fine grid 171 and a silver fine grid 172, and step S233 includes:

[0153] Step S2333: using aluminum paste to form an aluminum fine grid 171 on the second surface, and the aluminum fine grid 171 is in contact with the P-type silicon wafer 101 through the grooved area;

[0154] Step S2334: forming a silver fine grid 172 on the aluminum fine grid 171, and the aluminum fine grid 171 and the silver fine grid 172 form a composite fine grid.

[0155] In this way, the self-doping of the aluminum fine grid 171 forms an ohmic contact, and the strong conductivity of the silver fine grid 172 is used to efficiently conduct the current. In addition, since the aluminum fine grid 171 is used as a contact electrode, the thickness of the silver fine grid 172 can be thinner. In this way, while ensuring the photoelectric conversion efficiency, the cost of the composite fine grid is low and the process is simple.

[0156] Specifically, in step S2333, aluminum fine grid 171 can be formed on the second surface by screen printing using aluminum paste. In this way, the efficiency and precision of manufacturing aluminum fine grid 171 are higher, which is conducive to improving the quality of the battery. In other embodiments, aluminum fine grid 171 can also be formed by sputtering, vacuum evaporation and other processes.

[0157] Specifically, in step S2334, the silver fine grid 172 can be formed by screen printing. In this way, the efficiency and precision of making the silver fine grid 172 are higher, which is conducive to improving the quality of the battery. In other embodiments, the silver fine grid 172 can also be formed by sputtering, vacuum evaporation and other processes.

[0158] Optionally, step S2334 includes: covering the top and side surfaces of the aluminum fine grid 171 with the silver fine grid 172. In this way, the contact area between the silver fine grid 172 and the aluminum fine grid 171 is larger, so that the conductive effect between the silver fine grid 172 and the aluminum fine grid 171 is better.

[0159] It is understandable that in other embodiments, the silver fine grid 172 may only cover the top surface of the aluminum fine grid 171 but not the side surface of the aluminum fine grid 171 ; or the silver fine grid 172 may not cover the top surface of the aluminum fine grid 171 but only the side surface of the aluminum fine grid 171 .

[0160] Specifically, the silver fine grid 172 completely covers the top surface of the aluminum fine grid 171 and the side surface of the aluminum fine grid 171. In this way, the contact area between the silver fine grid 172 and the aluminum fine grid 171 is larger, so that the conductive effect between the silver fine grid 172 and the aluminum fine grid 171 is better.

[0161] It is understood that in other embodiments, the silver fine grid 172 may cover a portion of the top surface of the aluminum fine grid 171, or may cover a portion of the side surface of the aluminum fine grid 171. For example, the silver fine grid 172 may form a hollow area.

[0162] Optionally, the thickness of the aluminum fine grid 171 covered is less than 1 / 2 of the thickness of the silver fine grid 172. The thickness of the aluminum fine grid 171 covered is, for example, 1 / 3, 1 / 4, 1 / 5, or 1 / 6 of the thickness of the silver fine grid 172. In this way, the thickness ratio of the silver fine grid 172 to the aluminum fine grid 171 is within a suitable range, which can avoid poor overall conductivity caused by too small a thickness ratio, and can also avoid excessively high costs caused by too large a thickness ratio.

[0163] Optionally, the difference between the width of the silver fine grid 172 and the width of the aluminum fine grid 171 is 5 μm-20 μm. For example, 5 μm, 6 μm, 10 μm, 15 μm, 20 μm. In this way, the difference between the width of the silver fine grid 172 and the width of the aluminum fine grid 171 is within a suitable range, which can avoid the thinner silver fine grid 172 covering the side of the aluminum fine grid 171 due to the small width difference, thereby avoiding poor conductive effect, and can avoid the thicker silver fine grid 172 covering the side of the aluminum fine grid 171 due to the large width difference, thereby avoiding high cost.

[0164] Optionally, the thickness of the silver fine grid 172 is 5 μm-10 μm, for example 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm. In this way, the thickness of the silver fine grid 172 is within a suitable range, which can avoid the poor conductive effect caused by the silver fine grid 172 being too thin, and can also avoid the high cost caused by the silver fine grid 172 being too thick.

[0165] Optionally, the thickness of the aluminum fine grid 171 is 10 μm-40 μm, for example, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 40 μm. In this way, the thickness of the aluminum fine grid 171 is within a suitable range, so that the ohmic contact formed by the self-doping of the aluminum fine grid 171 is better, which is conducive to the efficient conduction of current.

[0166] In the related art, the reverse dark saturation current density (J0) of the front emitter of the PERC cell is 20fA / cm 2 , contact area J0 is 600fA / cm 2 , J0 of the back non-contact area is 3fA / cm 2 , contact area J0 is 500fA / cm 2 The front emitter J0 of the Topcont cell is 10fA / cm 2 , contact area J0 is 800fA / cm 2 , J0 of the back non-contact area is 2fA / cm 2 , contact area J0 is 50fA / cm 2 .

[0167] The P-type solar cell 10 manufactured by the manufacturing method of the P-type solar cell 10 of this embodiment has a first surface J0 of 2fA / cm 2, contact area J0 is 50fA / cm 2 , the second non-contact area J0 is 2fA / cm 2 , contact area J0 is 300fA / cm 2 .

[0168] If the contact area ratio is 2%, the J0 of the PERC cell in the related art is 43.54 fA / cm 2 The J0 of the P-type solar cell 10 manufactured by the manufacturing method of the P-type solar cell 10 of this embodiment is 10.92 fA / cm 2 Obviously, the P-type solar cell 10 manufactured by the manufacturing method of the P-type solar cell 10 of this embodiment has better electrical performance.

[0169] For other explanations and descriptions about this embodiment, please refer to other parts of this document. To avoid redundancy, they will not be repeated here.

[0170] Embodiment 2

[0171] The P-type solar cell 10 of the present embodiment is manufactured by using any of the manufacturing methods of the P-type solar cell 10 in the first embodiment.

[0172] The P-type solar cell 10 of the embodiment of the present application has a doped polysilicon layer 12 on the first side and an aluminum oxide layer 15 on the second side, so the manufactured P-type solar cell 10 can be radiation-resistant on both sides, thereby reducing the attenuation caused by radiation. At the same time, laser grooving and laser doping will cause certain damage to the cell, and the process of forming the electrode will repair the lattice damage introduced by the laser. In this way, the cost of manufacturing the P-type solar cell 10 is low and the photoelectric conversion efficiency is high.

[0173] For other explanations and descriptions about this embodiment, please refer to other parts of this document. To avoid redundancy, they will not be repeated here.

[0174] Embodiment 3

[0175] The P-type solar cell 10 of this embodiment includes:

[0176] P-type silicon wafer 101;

[0177] A tunneling oxide layer 11, a doped polysilicon layer 12, a first passivation layer 13 and a first electrode 14 are sequentially stacked on the first surface of the P-type silicon wafer 101, and the first electrode 14 passes through the first passivation layer 13 and contacts with the doped polysilicon;

[0178] An aluminum oxide layer 15, a second passivation layer 16 and a second electrode 17 are sequentially stacked on the second surface of the P-type silicon wafer 101. The aluminum oxide layer 15 and the second passivation layer 16 are provided with a grooved area, a boron-doped layer 189 is formed in the grooved area, and the second electrode 17 contacts the boron-doped layer 189 through the grooved area.

[0179] The P-type solar cell 10 of the embodiment of the present application has a doped polysilicon layer 12 on the first side and an aluminum oxide layer 15 on the second side, so the manufactured P-type solar cell 10 can be radiation-resistant on both sides, thereby reducing the attenuation caused by radiation. At the same time, laser grooving and laser doping will cause certain damage to the cell, and the process of forming the electrode will repair the lattice damage introduced by the laser. In this way, the cost of manufacturing the P-type solar cell 10 is low and the photoelectric conversion efficiency is high.

[0180] Optionally, the first electrode 14 and the second electrode 17 are both electroplated copper electrodes.

[0181] Optionally, the first electrode 14 is a silver electrode, and the second electrode 17 is an electroplated copper electrode.

[0182] Optionally, the first electrode 14 is a silver electrode, and the second electrode 17 includes an aluminum electrode.

[0183] Optionally, the second electrode 17 is a composite fine gate, which includes an aluminum fine gate 171 and a silver fine gate 172 . The aluminum fine gate 171 contacts the P-type silicon wafer 101 through the groove area, and the silver fine gate 172 is arranged on the side of the aluminum fine gate 171 away from the P-type silicon wafer 101 .

[0184] Optionally, the silver fine grid 172 covers the top surface and side surfaces of the aluminum fine grid 171 .

[0185] Optionally, the difference between the width of the silver fine grid 172 and the width of the aluminum fine grid 171 is 5 μm-20 μm.

[0186] Optionally, the thickness of the silver fine grid 172 is 5 μm-10 μm.

[0187] Optionally, the thickness of the aluminum fine grid 171 is 10 μm-40 μm.

[0188] For other explanations and descriptions of this embodiment, please refer to other parts of this document, especially Embodiment 1, which will not be repeated here to avoid redundancy.

[0189] Embodiment 4

[0190] The battery assembly of this embodiment includes the P-type solar cell 10 of the second embodiment or the third embodiment.

[0191] The battery assembly of the embodiment of the present application has a doped polysilicon layer 12 on the first side and an aluminum oxide layer 15 on the second side, so the manufactured P-type solar cell 10 can be radiation-resistant on both sides, thereby reducing the attenuation caused by radiation. At the same time, laser grooving and laser doping will cause certain damage to the battery cell, and the process of forming the electrode will repair the lattice damage introduced by the laser. In this way, the cost of manufacturing the P-type solar cell 10 is low and the photoelectric conversion efficiency is high.

[0192] For other explanations and descriptions about this embodiment, please refer to other parts of this document. To avoid redundancy, they will not be repeated here.

[0193] Embodiment 5

[0194] The photovoltaic system of this embodiment includes the battery assembly of the fourth embodiment.

[0195] In the photovoltaic system of the embodiment of the present application, since the first surface is provided with a doped polysilicon layer 12 and the second surface is provided with an aluminum oxide layer 15, the manufactured P-type solar cell 10 can be radiation-resistant on both sides, thereby reducing the attenuation caused by radiation. At the same time, laser grooving and laser doping will cause certain damage to the cell, and the process of forming the electrode will repair the lattice damage introduced by the laser. In this way, the cost of manufacturing the P-type solar cell 10 is low and the photoelectric conversion efficiency is high.

[0196] In this embodiment, the photovoltaic system can be applied to photovoltaic power stations, such as ground power stations, rooftop power stations, water power stations, etc., and can also be applied to equipment or devices that use solar energy to generate electricity, such as user solar power supplies, solar street lights, solar cars, solar buildings, etc. Of course, it can be understood that the application scenarios of the photovoltaic system are not limited to this, that is to say, the photovoltaic system can be applied in all fields that require solar energy to generate electricity. Taking the photovoltaic power generation system network as an example, the photovoltaic system may include a photovoltaic array, a junction box and an inverter. The photovoltaic array may be an array combination of multiple battery components. For example, multiple battery components can form multiple photovoltaic arrays. The photovoltaic array is connected to the junction box. The junction box can converge the current generated by the photovoltaic array. The converged current flows through the inverter and is converted into the alternating current required by the mains power grid, and then connected to the mains network to realize solar power supply.

[0197] For other explanations and descriptions about this embodiment, please refer to other parts of this document. To avoid redundancy, they will not be repeated here.

[0198] The above are only preferred embodiments of the present application and are not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application shall be included in the protection scope of the present application. Moreover, the specific features, structures, materials or characteristics described in the embodiments or examples of the present application may be combined in any one or more embodiments or examples in a suitable manner.

Claims

1. A method for manufacturing a P-type solar cell, It is characterized in that include: Provide P-type silicon wafers; Etching and cleaning the P-type silicon wafer; Preparing a tunneling oxide layer on the first surface of the P-type silicon wafer, wherein the tunneling oxide layer entirely covers the first surface; Preparing a doped polysilicon layer on the tunnel oxide layer, wherein the doped polysilicon layer entirely covers the tunnel oxide layer; preparing an aluminum oxide layer on the second surface of the P-type silicon wafer; preparing a first passivation layer on the doped polysilicon layer; preparing a second passivation layer on the aluminum oxide layer; locally covering the second passivation layer with a boron source layer; Scanning a boron source layer using a laser to form a boron doped layer and simultaneously forming a laser groove; cleaning the boron-doped layer; forming a first electrode on the first surface, wherein the first electrode passes through the first passivation layer and contacts the doped polysilicon layer; forming a second electrode on the second surface, wherein the second electrode contacts the boron-doped layer through a grooved region; Forming a first electrode on the first surface includes: forming the first electrode on the first surface using silver paste; forming a second electrode on the second surface includes: forming the second electrode on the second surface using aluminum paste; The second electrode comprises an aluminum fine grid and a silver fine grid, and the second electrode is formed on the second surface using aluminum paste, comprising: forming the aluminum fine grid on the second surface using aluminum paste, wherein the aluminum fine grid is in contact with the P-type silicon wafer through a grooved area; forming the silver fine grid on the aluminum fine grid, wherein the aluminum fine grid and the silver fine grid form a composite fine grid; The thickness of the aluminum fine grid covered by the silver fine grid is less than 1 / 2 of the thickness of the silver fine grid; the difference between the width of the silver fine grid and the width of the aluminum fine grid is 5 μm-20 μm.

2. The method for manufacturing a P-type solar cell according to claim 1, It is characterized in that Before the step of forming the first electrode on the first surface, the manufacturing method includes: Performing laser film opening on the first passivation layer; Forming a first electrode on the first surface includes: forming the first electrode by copper electroplating; A second electrode is formed on the second surface, comprising: The second electrode is formed by copper electroplating.

3. The method for manufacturing a P-type solar cell according to claim 1, It is characterized in that Forming a first electrode on the first surface includes: forming the first electrode on the first surface using silver paste; Forming a second electrode on the second surface includes: The second electrode is formed by copper electroplating.

4. The method for manufacturing a P-type solar cell according to claim 1, It is characterized in that The second electrode includes a fine grid, a main grid and a pad, the fine grid is an aluminum conductor, and the second electrode is formed on the second surface using aluminum paste, including: Using aluminum paste to form the aluminum conductor on the second surface; The main grid and the pad are formed on the aluminum conductor, wherein the main grid includes a first silver conductive portion, and / or the pad includes a second silver conductive portion.

5. The method for manufacturing a P-type solar cell according to claim 1, It is characterized in that The step of forming the silver fine grid on the aluminum fine grid comprises: The silver fine grid covers the top and side surfaces of the aluminum fine grid.

6. The method for manufacturing a P-type solar cell according to claim 1, It is characterized in that The thickness of the silver fine grid is 5 μm-10 μm.

7. The method for manufacturing a P-type solar cell according to claim 1, It is characterized in that The thickness of the aluminum fine grid is 10 μm-40 μm.

8. A P-type solar cell, It is characterized in that The P-type solar cell is manufactured by the manufacturing method of any one of claims 1 to 7.

9. A P-type solar cell, It is characterized in that include: P-type silicon wafer; A tunneling oxide layer, a doped polysilicon layer, a first passivation layer and a first electrode sequentially stacked on the first surface of the P-type silicon wafer, the first electrode passes through the first passivation layer and contacts the doped polysilicon, the tunneling oxide layer covers the first surface in its entirety, and the doped polysilicon layer covers the tunneling oxide layer in its entirety; An aluminum oxide layer, a second passivation layer, and a second electrode are sequentially stacked on the second surface of the P-type silicon wafer, wherein the aluminum oxide layer and the second passivation layer are provided with a grooved area, a boron-doped layer is formed in the grooved area, and the second electrode passes through the grooved area to contact the boron-doped layer; The first electrode is a silver electrode, and the second electrode includes an aluminum electrode; the second electrode is a composite fine grid, and the composite fine grid includes an aluminum fine grid and a silver fine grid, the aluminum fine grid forms contact with the P-type silicon wafer through a grooved area, and the silver fine grid is arranged on the side of the aluminum fine grid away from the P-type silicon wafer; the thickness of the aluminum fine grid covered by the silver fine grid is less than 1 / 2 of the thickness of the silver fine grid; the difference between the width of the silver fine grid and the width of the aluminum fine grid is 5μm-20μm.

10. The P-type solar cell according to claim 9, It is characterized in that The first electrode and the second electrode are both electroplated copper electrodes.

11. The P-type solar cell according to claim 9, It is characterized in that The first electrode is a silver electrode, and the second electrode is an electroplated copper electrode.

12. The P-type solar cell according to claim 9, It is characterized in that The silver fine grid covers the top surface and the side surfaces of the aluminum fine grid.

13. The P-type solar cell according to claim 9, It is characterized in that The thickness of the silver fine grid is 5 μm-10 μm.

14. The P-type solar cell according to claim 9, It is characterized in that The thickness of the aluminum fine grid is 10 μm-40 μm.

15. A battery assembly, It is characterized in that A P-type solar cell comprising claim 8 or any one of claims 9-14.

16. A photovoltaic system, It is characterized in that A battery assembly comprising the battery assembly of claim 15.