A lithium battery negative electrode composite material and preparation method thereof

By performing double-layer coating on the surface of the silicon oxide particles of the negative electrode material of the lithium-ion battery, combining porous materials and carbon nanotubes, the problems of high expansion rate and poor conductivity of the silicon oxygen/carbon-based negative electrode material are solved, and lithium ions are improved Battery performance and stability.

CN115084479BActive Publication Date: 2024-11-26ZHEJIANG GEELY HLDG GRP CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210846852.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-05
Publication Date
2024-11-26
Estimated Expiration
2042-07-05

AI Technical Summary

Technical Problem

The high expansion rate and conductivity deviation of silicon oxygen/carbon-based negative electrode materials limit their wide application in lithium-ion batteries.

Method used

Using double-layer coating treatment, the conductivity and stability of the material are improved by covering porous materials and carbon nanotubes on the surface of the silicon oxide particles and filling the graphene sheets with double-layer coated silicon oxide particles. .

Benefits of technology

It effectively reduces the expansion rate of the negative electrode material, improves the performance of lithium-ion batteries, enhances the conductivity and stability of the material, and prevents the relative displacement between the silicon oxide particles and graphene.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115084479B_ABST
    Figure CN115084479B_ABST
Patent Text Reader

Abstract

The present invention proposes a lithium battery negative electrode composite material and a preparation method, the composite material at least comprising: silicon dioxide particles; a first coating layer, the first coating layer is a porous material, and the first coating layer is coated on the surface of the silicon dioxide particles; a second coating layer, coated on the surface of the first coating layer, and the second coating layer is implanted with carbon nanotubes; and graphene, the double-layer coated silicon dioxide particles are filled between adjacent graphene sheets. The present invention provides a lithium battery negative electrode composite material and a preparation method, which can effectively reduce the expansion rate of the negative electrode material and improve the conductivity of the negative electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion battery materials, and in particular to a lithium battery negative electrode composite material and a preparation method thereof. Background Art

[0002] Lithium-ion batteries have the advantages of light weight, large energy storage, high power, no pollution, long life, and small automatic discharge coefficient. They are ideal vehicle batteries for electric bicycles, electric cars, etc.

[0003] As the market's requirements for lithium-ion battery energy density increase, the requirements for lithium-ion battery electrode materials are also increasing, and negative electrode materials are the key materials for lithium-ion batteries. Among them, silicon-oxygen / carbon-based negative electrode materials are valued for their high gram capacity and abundant resources, and are used in fields such as high specific energy density lithium-ion batteries. However, the high expansion rate and conductivity deviation of silicon-oxygen / carbon-based negative electrode materials restrict the widespread application of silicon-oxygen / carbon-based negative electrode materials. Summary of the invention

[0004] The present invention provides a lithium battery negative electrode composite material and a preparation method thereof, which can effectively reduce the expansion rate of the negative electrode material and improve the conductivity of the negative electrode material, thereby improving the performance of the lithium ion battery.

[0005] To solve the above technical problems, the present invention is achieved through the following technical solutions:

[0006] The present invention provides a lithium battery negative electrode composite material, comprising at least:

[0007] Silicon oxide particles;

[0008] A first coating layer, wherein the first coating layer is a porous material and the first coating layer is coated on the surface of the silicon oxide particles;

[0009] a second coating layer, coated on the surface of the first coating layer, wherein the second coating layer is implanted with carbon nanotubes; and

[0010] Graphene, wherein the adjacent graphene sheets are filled with double-layer coated silicon dioxide particles.

[0011] In one embodiment of the present invention, the first coating layer is a porous structure, and the porosity of the first coating layer is 30-60%.

[0012] In one embodiment of the present invention, the porous material includes one of a porous carbon material or a porous polymer material.

[0013] In one embodiment of the present invention, the particle size of the silicon oxide particles is 200 nm-5 μm.

[0014] In one embodiment of the present invention, the thickness of the first coating layer is 1 / 5-1 / 4 of the particle size of the silicon oxide particles.

[0015] The present invention also provides a method for preparing a lithium battery negative electrode composite material, the preparation method comprising the following steps:

[0016] Providing silicon dioxide particles;

[0017] Coating a layer of porous material on the surface of the silicon oxide particles to form a first coating layer;

[0018] Coating a second coating layer on the surface of the first coating layer;

[0019] Implanting carbon nanotubes in the second coating layer; and

[0020] The graphene is mixed with the double-layer coated silicon dioxide particles to form the lithium battery negative electrode composite material, wherein the double-layer coated silicon dioxide particles are filled between adjacent graphene sheets.

[0021] In one embodiment of the present invention, the step of preparing the first coating layer comprises:

[0022] soaking the silicon oxide particles in a polydiallyldimethylammonium chloride solution; and

[0023] An initiator is added to the polydiallyldimethylammonium chloride solution.

[0024] In one embodiment of the present invention, the initiator includes any one of azobisisoheptanenitrile, diisopropyl peroxydicarbonate or ammonium persulfate.

[0025] In one embodiment of the present invention, the step of preparing the second coating layer comprises:

[0026] Coating a layer of polyacrylic acid on the surface of the first coating layer to form a polyacrylic acid layer; and

[0027] Lithium hydroxide is added to the polyacrylic acid layer to generate lithium polyacrylate to form a second coating layer.

[0028] In one embodiment of the present invention, the preparation method further comprises drying the first coating layer and the second coating layer.

[0029] The present invention proposes a lithium battery negative electrode composite material and a preparation method thereof. Through a double-layer coating treatment, the surface roughness of silicon oxide particles is increased, and relative displacement between the double-layer coated silicon oxide particles and graphene is effectively prevented. The double-layer coated silicon oxide particles can provide more contact sites with graphene, reduce the expansion rate of the lithium battery negative electrode material, and improve the conductivity of the lithium battery negative electrode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a schematic diagram of preparing the negative electrode composite material of the lithium battery in the present invention.

[0031] Figure 2 It is a schematic diagram of preparing the negative electrode composite material of the lithium battery in the present invention.

[0032] Figure 3 The present invention is a flow chart of a method for preparing a lithium battery negative electrode composite material.

[0033] Description of reference numerals:

[0034] 100. Silicon oxide particles; 200. A first coating layer; 300. A second coating layer; 400. Carbon nanotubes; 500. Graphene. DETAILED DESCRIPTION

[0035] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0036] It should be noted that the illustrations provided in this embodiment are only used to illustrate the basic concept of the present invention in a schematic manner. Therefore, the drawings only show components related to the present invention rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.

[0037] The technical solution of the present invention is further described in detail below in conjunction with several embodiments and drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0038] Among negative electrode materials, silicon-based negative electrode materials are considered to be a type of negative electrode material that can effectively improve the energy density of lithium-ion batteries due to their high theoretical specific capacity, and have received extensive attention and research. Lithium-ion batteries made from silicon-based negative electrode materials are widely used in portable electronic products such as mobile phones, tablet computers, laptops, and digital cameras. They are one of the most promising energy storage devices and bring a lot of convenience to people's lives.

[0039] See also Figure 1As shown, the present invention provides a lithium battery negative electrode composite material, including silicon dioxide particles 100, a first coating layer 200, a second coating layer 300, carbon nanotubes 400 and graphene 500. Among them, the first coating layer 200 is coated on the surface of the silicon dioxide particles 100, the second coating layer 300 is coated on the surface of the first coating layer 200, one end of the carbon nanotube 400 is located in the second coating layer 300, and the other end is suspended, and the double-layer coated silicon dioxide particles are evenly distributed between adjacent layers of graphene 500.

[0040] See also Figure 3 As shown, the present invention also provides a method for preparing a lithium battery negative electrode composite material, including but not limited to steps S100-S500.

[0041] S100, providing silicon dioxide particles.

[0042] S200, coating the surface of the silicon monoxide particles with a layer of porous material to form a first coating layer.

[0043] S300, coating the surface of the first coating layer with a second coating layer.

[0044] S400, implanting carbon nanotubes into the second coating layer.

[0045] S500, mixing graphene with the double-layer coated silicon dioxide particles to form the lithium battery negative electrode composite material, wherein the double-layer coated silicon dioxide particles are filled between adjacent graphene layers.

[0046] See also Figures 2 to 3 As shown, in one embodiment of the present invention, in step S100, the particle size of the provided silicon dioxide particles 100 may be, for example, in the range of 200 nm-5 μm, and further, optionally, the particle size of the silicon dioxide particles 100 may be, for example, in the range of 1-3 μm. The silicon dioxide particles 100 have a small and uniform particle size, and the negative electrode material obtained when stacked has a larger porosity, which provides a certain space for the volume expansion of silicon dioxide during charging, thereby avoiding damage to the overall structure of the electrode active layer.

[0047] See also Figures 2 to 3As shown, in one embodiment of the present invention, in step S200, the first coating layer 200 is a porous structure, and the porosity of the first coating layer 200 is, for example, 30-60%. In one embodiment of the present invention, the thickness of the first coating layer 200 is, for example, 1 / 5-1 / 4 of the particle size of the silicon oxide particles 100, and further, the thickness of the first coating layer 200 is, for example, 1 / 5 of the particle size of the silicon oxide particles 100. In one embodiment of the present invention, the thickness of the first coating layer 200 is, for example, 0.04-1.3 μm. In one embodiment of the present invention, the porous first coating layer 200 has a certain elasticity. When charging, the coated silicon oxide particles 100 expand, and the first coating layer 200 will extend outward with the silicon oxide particles 100. When discharging, the coated silicon oxide particles 100 shrink, and the first coating layer 200 rebounds inward with the silicon oxide particles 100. During this process, the first coating layer 200 always tightly coats the silicon oxide particles 100, playing a buffering role, and when the thickness of the first coating layer 200 is 1 / 5 of the particle size of the silicon oxide particles 100, the buffering effect is optimal, which can effectively prevent the silicon oxide particles 100 from being squeezed and destroying the overall structure of the electrode active layer.

[0048] See also Figures 2 to 3 As shown, in one embodiment of the present invention, in step S200, the first coating layer 200 is made of a porous material, and the first coating layer 200 is made of, for example, a porous carbon material or a porous polymer material. Further, in one embodiment of the present invention, the first coating layer 200 is made of, for example, polydiallyldimethylammonium chloride (PDDAC).

[0049] See also Figures 2 to 3As shown, the present invention does not limit the method for preparing the first coating layer 200 on the surface of the silicon dioxide particles 100. In one embodiment, for example, the first coating layer 200 is prepared by soaking the silicon dioxide particles 100 in a diallyldimethylammonium chloride (DDAC) monomer solution and then adding an initiator. In another embodiment, for example, the silicon dioxide particles 100 can also be soaked in a polydiallyldimethylammonium chloride (PDDAC) solution to prepare the first coating layer 200. Further, in this embodiment, the silicon dioxide particles 100 are placed in a reaction container, and a diallyldimethylammonium chloride (DDAC) monomer aqueous solution is added to the reaction container, the pH value is adjusted to, for example, 4 to 6, and nitrogen is used for deoxygenation for, for example, 1 hour, and an initiator is added to polymerize to prepare the first coating layer 200 on the surface of the silicon dioxide particles 100. In one embodiment of the present invention, the polymerization temperature for preparing the first coating layer 200 is set to, for example, 60-80°C, and the polymerization time is set to, for example, 1-2h. Further, the polymerization temperature for preparing the first coating layer 200 is set to 80° C., and the polymerization time is set to 1 hour. The present invention does not limit the type of initiator for preparing the first coating layer 200. In one embodiment of the present invention, the initiator is, for example, any one of azobisisoheptanenitrile (ABVN), diisopropyl peroxydicarbonate (IPP) or ammonium persulfate (APS).

[0050] See also Figures 2 to 3 As shown, in one embodiment of the present invention, before preparing the second coating layer 300, the silicon oxide particles 100 coated with the first coating layer 200 need to be dried so that the first coating layer 200 and the silicon oxide particles 100 are more tightly combined. In one embodiment of the present invention, for example, the silicon oxide particles 100 coated with the first coating layer 200 are dried by spray drying. In one embodiment of the present invention, the temperature of the spray drying is set to 90-120°C, for example.

[0051] See also Figures 2 to 3 As shown, in one embodiment of the present invention, in step S300, the thickness of the second coating layer 300 can be set in the range of 5-15 μm, for example. A layer of polyacrylate lithium (PAALi) is coated on the surface of the first coating layer 200 to form the second coating layer 300, and the second coating layer 300 is within the above thickness range, which can not only form a stable interface between the silicon dioxide particles 100, but also isolate the contact between the silicon dioxide particles 100 and the electrolyte, avoiding the direct reaction with the electrolyte to form a SEI film, and further increasing the initial charge and discharge efficiency.

[0052] See also Figures 2 to 3As shown, in step S300, the present invention does not limit the preparation method of the second coating layer 300. In one embodiment, for example, the silicon oxide particles 100 coated by the first coating layer 200 can be directly immersed in a lithium polyacrylate (PAALi) solution to prepare the second coating layer 300. In another embodiment, for example, the silicon oxide particles 100 coated by the first coating layer 200 can also be immersed in a polyacrylic acid solution, and then lithium hydroxide is added to prepare the second coating layer 300. In other embodiments, for example, the silicon oxide particles 100 coated by the first coating layer 200 can also be immersed in an acrylic acid solution, an initiator is added to form polyacrylic acid, and then lithium hydroxide is added to prepare the second coating layer 300.

[0053] See also Figures 2 to 3 As shown, in one embodiment of the present invention, in step S300, the silicon oxide particles 100 coated by the first coating layer 200 are placed in a reaction container, acrylic acid and an initiator are added to the reaction container, a polyacrylic acid layer is formed on the surface of the first coating layer 200, and then lithium hydroxide is continuously added to the reaction container to prepare the second coating layer 300. In one embodiment of the present invention, in the step of forming the polyacrylic acid layer, the initiator can be, for example, ammonium persulfate (NH4)2S2O8, and the amount of ammonium persulfate (NH4)2S2O8 is, for example, 8-15% of the mass of acrylic acid. In one embodiment of the present invention, in the step of forming the polyacrylic acid layer, isopropanol can also be added as a molecular weight regulator to control the molecular weight of polyacrylic acid. In one embodiment of the present invention, in the step of forming the polyacrylic acid layer, the polymerization temperature is, for example, controlled within 60-100°C, and the polymerization time is, for example, 1-3h. In one embodiment of the present invention, lithium hydroxide is added to the silicon oxide particles 100 coated with the polyacrylic acid layer, and the hydrogen bonds in the polyacrylic acid are broken to react and generate lithium polyacrylate (PAALi) to form the second coating layer 300 .

[0054] See also Figures 2 to 3 As shown, in one embodiment of the present invention, in step S400, when preparing the second coating layer 300, carbon nanotubes can be added to the polyacrylate lithium (PAALi) solution to implant the carbon nanotubes 400 in the second coating layer 300. On the one hand, the implantation of the carbon nanotubes 400 can improve the conductivity of the double-layer coated silicon oxide particles. On the other hand, the implantation of the carbon nanotubes 400 can improve the surface roughness of the double-layer coated silicon oxide particles, increase resistance, and effectively prevent the relative displacement between the double-layer coated silicon oxide particles and the graphene 500. The implantation of the carbon nanotubes 400 can also provide more contact sites with the graphene 500.

[0055] See also Figures 2 to 3As shown, in one embodiment of the present invention, before preparing the double-layer coated silicon oxide composite material, the double-layer coated silicon oxide particles need to be dried to improve the stability and density of the second coating layer 300. In one embodiment of the present invention, the second coating layer 300 is dried, for example, by spray drying or spray granulation, and residual impurities are removed. Further, the temperature of spray drying or spray granulation is set to 80-100°C, for example.

[0056] See also Figure 1 and 3 As shown, in one embodiment of the present invention, in step S500, the graphene 500 and the double-layer coated silicon oxide particles 100 can be mixed in a liquid phase mixing manner to prepare a silicon oxide composite material. The double-layer coated silicon oxide particles 100 are evenly dispersed between the graphene 500 sheets, and the double-layer coated silicon oxide particles 100 contain carbon nanotubes 400 on the surface, which can effectively prevent the double-layer coated silicon oxide particles 100 from shifting between the graphene 500 sheets.

[0057] In summary, the present invention proposes a lithium battery negative electrode composite material and a preparation method, in which an elastic porous layer is coated on the surface of silicon oxide to effectively prevent squeezing between silicon oxide particles, a layer of lithium polyacrylate is further coated on the surface of silicon oxide coated with the elastic porous layer to effectively isolate the contact between silicon oxide particles and electrolyte, and carbon nanotubes are implanted in the lithium polyacrylate layer to improve the roughness of the double-layer coated silicon oxide, effectively prevent relative displacement between the double-layer coated silicon oxide particles and graphene, and provide more contact sites between the double-layer coated silicon oxide particles and graphene, thereby reducing the expansion rate of the negative electrode material and improving its conductivity.

[0058] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in the present application is not limited to the technical solution formed by a specific combination of the above-mentioned technical features, but should also cover other technical solutions formed by any combination of the above-mentioned technical features or their equivalent features without departing from the inventive concept, such as a technical solution formed by replacing the above-mentioned features with (but not limited to) technical features with similar functions disclosed in this application.

[0059] Except for the technical features described in the specification, the remaining technical features are known technologies to those skilled in the art. In order to highlight the innovative features of the present invention, the remaining technical features will not be described here in detail.

Claims

1. A method for preparing a lithium battery negative electrode composite material, characterized in that: At least the following steps are included: Providing silicon dioxide particles; The silicon oxide particles are immersed in a diallyldimethylammonium chloride monomer aqueous solution, and an initiator is added to carry out polymerization at a polymerization temperature of 60-80° C. and a polymerization time of 1-2 hours; Preparing a first coating layer of polydiallyldimethylammonium chloride on the surface of the silicon oxide particles; The silicon oxide particles coated with the first coating layer are subjected to spray drying treatment, wherein the spray drying temperature is 90-120° C.; Soaking the dried silicon dioxide particles coated with the first coating layer in a lithium polyacrylate solution to prepare a lithium polyacrylate second coating layer; Drying the double-layer coated silicon dioxide particles; as well as Mixing the graphene with the dried double-layer coated silicon dioxide particles to form the lithium battery negative electrode composite material; Wherein, when preparing the second coating layer, carbon nanotubes are added to the lithium polyacrylate solution, and the carbon nanotubes are implanted in the second coating layer; In the lithium battery negative electrode composite material, the first coating layer is a porous structure, the double-layer coated silicon dioxide particles are filled between adjacent graphene sheets, one end of the carbon nanotube is located in the second coating layer, and the other end is suspended; The particle size of the silicon oxide particles is 200nm-5μm; The thickness of the second coating layer is 5-15 μm.

2. The method for preparing a lithium battery negative electrode composite material according to claim 1, characterized in that: The initiator includes any one of azobisisoheptanenitrile, diisopropyl peroxydicarbonate or ammonium persulfate.

3. The method for preparing a lithium battery negative electrode composite material according to claim 1, characterized in that: When the double-layer coated silicon oxide particles are dried, they are dried by spray drying or spray granulation, and the temperature of spray drying or spray granulation is 80-100°C.

4. The method for preparing a lithium battery negative electrode composite material according to claim 1, characterized in that: The porosity of the first coating layer is 30-60%.

5. The method for preparing a lithium battery negative electrode composite material according to claim 1, characterized in that: The thickness of the first coating layer is 1 / 5-1 / 4 of the particle size of the silicon oxide particles.

6. A lithium battery negative electrode composite material, characterized in that: The method is obtained by the preparation method according to any one of claims 1 to 5.