Optical laminate with adhesive layer and image display device, and method for producing the same

Through the design of forming through holes in the optical laminate, the problems of difficult positioning and low yield of the optical laminate in the image display device are solved, and high functionality and large-scale display effects are achieved.

CN115087894BActive Publication Date: 2024-10-29NITTO DENKO CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202180014333.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-02-04
Publication Date
2024-10-29
Estimated Expiration
2041-02-04

AI Technical Summary

Technical Problem

Due to the presence of the adhesive layer in the existing optical laminate in the image display device, it is difficult to align the component positions, the yield is reduced, and functions such as cameras and speakers cannot be fully utilized, which affects the design of the entire display.

Method used

Design an optical laminate with through holes. By forming a first adhesive layer on one side of the optical film and a second adhesive layer on the other side, and integrally penetrating them, a through hole is formed to facilitate optical lamination. The fit between the body and other components and the full play of functions.

Benefits of technology

The yield rate of the image display device and the proportion of the display part are improved, the normal operation of functions such as cameras and speakers is ensured, the size of the non-display area is reduced, and the appearance and functionality are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115087894B_ABST
    Figure CN115087894B_ABST
Patent Text Reader

Abstract

Provided is an optical laminate with an adhesive layer that can realize an image display device with high functions and a large display portion ratio without reducing the yield rate. The optical laminate with an adhesive layer of the present invention comprises: an optical film, a first adhesive layer formed on one side of the optical film, and a second adhesive layer formed on the other side of the optical film. The optical laminate with an adhesive layer has a through hole that integrally penetrates the first adhesive layer, the optical film, and the second adhesive layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an optical laminate with a pressure-sensitive adhesive layer and an image display device, and methods for producing the same. Background Art

[0002] An optical laminate containing optical films such as polarizers and phase difference plates is used in image display devices such as smart phones, tablet terminals, and notebook personal computers (PCs). In recent years, the high functionality of image display devices has been promoted, equipped with various functions such as cameras, speakers, and various sensors. In addition, for image display devices, the whole surface display has been promoted. However, since the whole surface is used as a display, an optical laminate is also configured on the upper part of the part where the above-mentioned camera, speaker, and various sensors are configured, and sometimes their desired functions cannot be fully utilized. Therefore, an optical laminate having an opening portion formed in a manner corresponding to the portion having these functions is proposed (patent document 1).

[0003] The optical laminate is usually bonded to other components via an adhesive layer. When the optical laminate having an opening is bonded to other components via an adhesive layer, it becomes difficult to align the components of the image display device, which reduces the yield rate. Therefore, it is necessary to design the non-display area to be larger, which makes it difficult to display the entire surface.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2014-112238 Summary of the invention

[0007] Problem that the invention aims to solve

[0008] The present invention has been made to solve the above-mentioned conventional problems, and a main object of the present invention is to provide an optical laminate with a pressure-sensitive adhesive layer that can realize an image display device with high functionality and a large display portion ratio without reducing the yield.

[0009] Solutions for solving problems

[0010] The optical laminate with adhesive layer of the present invention comprises: an optical film, a first adhesive layer formed on one side of the optical film, and a second adhesive layer formed on the other side of the optical film. The optical laminate has a through hole that integrally penetrates the first adhesive layer, the optical film, and the second adhesive layer.

[0011] In one embodiment, the optical film is at least one selected from the group consisting of a polarizing plate, a retardation film, a conductive film for a touch panel, a pressure-sensitive film, and a transparent plastic film.

[0012] Another aspect of the present invention provides a method for manufacturing an optical laminate with an adhesive layer. The method for manufacturing an optical laminate includes: a step of forming a first adhesive layer on one side of an optical film; a step of forming a second adhesive layer on the other side of the optical film; and a step of forming a through hole that integrally penetrates the first adhesive layer, the optical film, and the second adhesive layer.

[0013] Effects of the Invention

[0014] According to the present invention, an optical laminate with an adhesive layer can be provided that can realize an image display device with high functions and a large display portion without reducing the yield rate. The optical laminate with an adhesive layer of the present invention comprises: an optical film, a first adhesive layer formed on one side of the optical film, and a second adhesive layer formed on the other side of the optical film. The optical laminate with an adhesive layer of the present invention has a through hole that integrally penetrates the first adhesive layer, the optical film and the second adhesive layer. By using the optical laminate with an adhesive layer of the present invention, even in the case of a configuration in which a camera, a speaker and various sensors are arranged in the display portion of the image display device, position alignment becomes easy, and the yield rate can be improved. Therefore, an image display device with a larger display area ratio (for example, an image display device with a full-surface display) can also be realized. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 This is a schematic cross-sectional view of an optical laminate with a pressure-sensitive adhesive layer according to one embodiment of the present invention.

[0016] Figure 2 It is a schematic cross-sectional view of an image display device according to one embodiment of the present invention. DETAILED DESCRIPTION

[0017] Embodiments of the present invention will be described below, but the present invention is not limited to these embodiments.

[0018] A. Overall structure of the optical laminate with pressure-sensitive adhesive layer

[0019] Figure 1Schematic cross-sectional view of an optical laminate with adhesive layer of one embodiment of the present invention. The optical laminate with adhesive layer 100 shown in the figure has: an optical film 10, a first adhesive layer 20 formed on one side of the optical film 10, and a second adhesive layer 30 formed on the other side of the optical film 10. In practical applications, in order to properly protect the first adhesive layer 20 and the second adhesive layer 30 until use, a release film 40 is temporarily pasted on these adhesive layers in a removable manner. The optical laminate with adhesive layer 100 has a through hole 50 that integrally penetrates the optical film 10, the first adhesive layer 20 and the second adhesive layer 30. The through hole 50 is formed in a manner corresponding to the position, size, number and shape of the camera, speaker and various sensors carried by the image display device. By making the optical laminate with adhesive layer 100 have such a through hole 50, when the optical film is attached to other components, the optical film and each adhesive layer will not be offset, and position alignment can become easy. In addition, since the through hole 50 is formed in a manner corresponding to the camera, speaker, and various sensors, the functions they have will not be hindered by the optical film and the adhesive layer, and can be fully exerted. Representatively, the optical laminate with an adhesive layer can be configured in an image display device in a manner such that the first adhesive layer is the recognition side of the image display device.

[0020] The through hole 50 can be formed in any appropriate shape and size. Examples of the shape of the through hole (shape when viewed from above) include circular and rectangular shapes. When a circular through hole is formed, for example, a through hole with a diameter of 1 mm to 30 mm is formed. The through hole can be a through hole that penetrates the optical laminate in the form of a column such as a cylinder or a polygonal column, or a through hole that penetrates the optical laminate in the form of a cone, i.e., a frustum. In addition, the size of the through hole can be different in each layer, such as an adhesive layer and an optical film.

[0021] In one embodiment, the through hole is a through hole that penetrates the optical laminate in a cone shape. In order to improve the appearance of the smartphone, a punch hole type is generally used as a way to set the front camera. Due to the high demand for selfies, the wide-angle of the front camera is expected, and the aperture is enlarged. On the other hand, in order to hide the hole section, prevent light leakage of the display, etc., it is necessary to perform black frame printing, and the expansion of the non-display area may reduce the appearance. By making the through hole a cone shape, it is possible to achieve wide-angle configuration and hiding of the hole end when configuring the camera, and to reduce the formation of black frame printing / non-display area. When the through hole is a cone shape, it can be designed in a way that the top view shape of the through hole on the outermost surface of the first adhesive layer (hereinafter also referred to as the planar shape of the first through hole) and the top view shape of the through hole on the outermost surface of the second adhesive layer (hereinafter also referred to as the planar shape of the second through hole) have any appropriate difference. For example, when the planar shape of the through hole is circular, the difference between the diameter of the planar shape of the first through hole and the diameter of the planar shape of the second through hole is preferably 5 μm to 500 μm, more preferably 10 μm to 250 μm, and further preferably 20 μm to 150 μm. In addition, when the planar shape of the through hole is rectangular or elliptical, for example, the difference between the size of the planar shape of the first through hole (e.g., the length of one side, the short diameter, the long diameter, etc.) and the size of the planar shape of the second through hole (e.g., the length of one side, the short diameter, the long diameter, etc.) is preferably 5 μm to 500 μm, more preferably 10 μm to 250 μm, and further preferably 20 μm to 150 μm. Regarding the difference in the size of the planar shape of the through hole, as long as the smallest difference is within the above range, it is sufficient. It should be noted that the planar shape of the first through hole and the planar shape of the second through hole can be different shapes or the same shape (i.e., similar shapes).

[0022] In one embodiment, the difference in size between the planar shape of the first through hole and the planar shape of the second through hole is preferably 500 μm or less, more preferably 300 μm or less, and further preferably 150 μm or less. In order to improve the appearance of the smartphone, a perforated type is generally used as a way to set a front camera. Reducing the aperture is preferred in appearance, but there is a problem of having to increase the width of the black frame printing due to the positional offset when the components are bonded and the dimensional deviation of the through holes. By making the difference between the planar shape of the first through hole and the planar shape of the second through hole within the above range, the width of the black frame printing can be reduced, and the appearance can be improved.

[0023] In this embodiment, the planar shape of the first through hole may be larger, or the planar shape of the second through hole may be larger. When the planar shape of the first through hole is larger than the planar shape of the second through hole, that is, when the planar shape of the through hole on the identification side is larger, for example, when the through hole is arranged in a manner corresponding to the camera part, it is possible to achieve a wide angle of the camera and hide the end of the hole, and it is possible to reduce the black frame printing / non-display area. In addition, when the planar shape of the first through hole is smaller than the planar shape of the second through hole, that is, when the top view shape of the through hole on the identification side is smaller, for example, when the through hole is arranged in a manner corresponding to the camera part, it is possible to reduce the black frame printing / non-display area and improve the appearance. Furthermore, the distance between the camera module and the identification side can be shortened and a wide angle can be achieved, and interference with the camera module can be prevented.

[0024] In one embodiment, the size of the top view shape of the through hole formed in the first adhesive layer and the second adhesive layer is preferably larger than the size of the through hole formed in the optical film. When the optical laminate with an adhesive layer having a through hole is bonded to an adherend, sometimes the adhesive overflows into the through hole due to the pressure during bonding, which reduces the appearance quality and damages the function of sensors such as cameras. The distance between the end of the through hole formed in the first adhesive layer and the second adhesive layer and the end of the through hole formed in the optical film is preferably 5μm to 1000μm, more preferably 10μm to 500μm, and further preferably 20μm to 250μm. By making the distance between the end of the through hole formed in the first adhesive layer and the end of the through hole formed in the optical film be the above range, an optical laminate with excellent appearance and good performance of the function of sensors such as cameras can be obtained. The distance between the end of the through hole formed in the first adhesive layer and the end of the through hole formed in the optical film, and the distance between the end of the through hole formed in the second adhesive layer and the end of the through hole formed in the optical film can be the same or different.

[0025] In the example shown in the figure, the through hole 50 is formed so as to penetrate the separator 40, but the through hole may not be formed in the separator 40. In addition, the separator 40 may have the same shape as the optical film and the first and second adhesive layers, or may have different shapes and sizes as long as it can properly protect the first adhesive layer and the second adhesive layer until use.

[0026] Any appropriate surface treatment layer may be provided between the optical film 10 and the first pressure-sensitive adhesive layer 20 depending on the purpose. Examples of the surface treatment layer include a hard coat layer, an antireflection layer, an antiglare layer, and an antiglare layer.

[0027] The optical film 10 , the first pressure-sensitive adhesive layer 20 , and the second pressure-sensitive adhesive layer 30 will be described in detail below.

[0028] B. Optical Film

[0029] As the optical film 10, any appropriate optical film can be used. The optical film can be a film consisting of a single layer or a laminate. As a specific example of an optical film consisting of a single layer, a polarizer and a phase difference film can be listed. As a specific example of an optical film consisting of a laminate, a polarizer (representatively a laminate of a polarizer and a protective film), a conductive film for a touch panel, a surface treatment film, a pressure-sensitive film, and a laminate (such as a circular polarizer for anti-reflection, a polarizer with a conductive layer for a touch panel) formed by appropriately stacking an optical film consisting of a single layer thereof and / or an optical film consisting of a laminate can be listed. Hereinafter, as an example, a polarizer is described in detail. Preferably, the optical film is at least one selected from the group consisting of a polarizer, a phase difference film, a conductive film for a touch panel, a pressure-sensitive film and a transparent plastic film (such as a cycloolefin resin, a polyethylene terephthalate resin, an acrylic resin, a polycarbonate resin, etc.).

[0030] B-1.Polarizing plate

[0031] The polarizing plate typically includes a polarizer and a protective film, and may further include the surface treatment layer described above, depending on the application and the like.

[0032] B-1-1. Polarizer

[0033] The polarizer is typically composed of a resin film containing a dichroic substance. As the resin film, any appropriate resin film that can be used as a polarizer can be adopted. The resin film is typically a polyvinyl alcohol-based resin (hereinafter referred to as "PVA-based resin") film.

[0034] As the PVA resin forming the above-mentioned PVA resin film, any appropriate resin can be used. For example, polyvinyl alcohol and ethylene-vinyl alcohol copolymer can be listed. Polyvinyl alcohol can be obtained by saponifying polyvinyl acetate. Ethylene-vinyl alcohol copolymer can be obtained by saponifying ethylene-vinyl acetate copolymer. The saponification degree of PVA resin is usually 85 mol% to 100 mol%, preferably 95.0 mol% to 99.95 mol%, and more preferably 99.0 mol% to 99.93 mol%. The saponification degree can be calculated according to JIS K 6726-1994. By using a PVA resin with such a saponification degree, a polarizer with excellent durability can be obtained. When the saponification degree is too high, there is a concern that gelation will occur.

[0035] The average degree of polymerization of the PVA-based resin can be appropriately selected depending on the purpose. The average degree of polymerization is usually 1000 to 10000, preferably 1200 to 4500, and more preferably 1500 to 4300. The average degree of polymerization can be determined in accordance with JIS K 6726-1994.

[0036] Examples of the dichroic substance contained in the resin film include iodine and organic dyes, which can be used alone or in combination of two or more, and iodine is preferably used.

[0037] The resin film may be a single-layer resin film or a laminate of two or more layers.

[0038] As a specific example of a polarizer composed of a single-layer resin film, a polarizer formed by applying an iodine-based dyeing treatment and a stretching treatment (representatively uniaxial stretching) to a PVA-based resin film can be listed. The above-mentioned iodine-based dyeing is performed, for example, by immersing the PVA-based film in an iodine aqueous solution. The stretching ratio of the above-mentioned uniaxial stretching is preferably 3 to 7 times. Stretching can be performed after the dyeing treatment, or it can be performed while dyeing. In addition, dyeing can also be performed after stretching. As needed, the PVA-based resin film can be subjected to swelling treatment, cross-linking treatment, cleaning treatment, drying treatment, etc. For example, by immersing the PVA-based resin film in water for washing before dyeing, not only can the stains and anti-blocking agents on the surface of the PVA-based film be cleaned, but the PVA-based resin film can also be swelled to prevent uneven dyeing.

[0039] As a specific example of a polarizer obtained using a laminate, there can be listed: a laminate of a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, or a laminate of a resin substrate and a PVA-based resin layer formed by coating the resin substrate. The polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer formed by coating the resin substrate can be made, for example, by the following method: a PVA-based resin solution is applied to a resin substrate, and the PVA-based resin layer is formed on the resin substrate by drying, thereby obtaining a laminate of the resin substrate and the PVA-based resin layer; the laminate is stretched and dyed to make the PVA-based resin layer into a polarizer. In the present embodiment, stretching typically includes immersing the laminate in an aqueous solution of boric acid for stretching. Furthermore, stretching may further include, as needed, air stretching the laminate at a high temperature (e.g., above 95°C) before stretching in an aqueous solution of boric acid. The obtained laminate of resin substrate / polarizer can be used directly (that is, the resin substrate can be used as a protective film of polarizer), or the resin substrate can be peeled off from the laminate of resin substrate / polarizer and any appropriate protective film corresponding to the purpose can be laminated on the peeled surface for use. The details of the manufacturing method of such a polarizer are described in, for example, Japanese Patent Publication No. 2012-73580. All the records of the publication are cited in this specification as a reference.

[0040] The polarizer preferably exhibits absorption dichroism at any wavelength of 380 nm to 780 nm. The single transmittance of the polarizer is preferably 43.0% to 46.0%, more preferably 44.5% to 46.0%. The polarization degree of the polarizer is preferably 97.0% or more, more preferably 99.0% or more, and further preferably 99.9% or more.

[0041] The thickness of the polarizer can be set to any appropriate value. The thickness is typically 0.5 μm or more and 80 μm or less, preferably 30 μm or less, more preferably 25 μm or less, further preferably 18 μm or less, particularly preferably 12 μm or less, and further particularly preferably less than 8 μm. The thickness of the polarizer is preferably 1 μm or more.

[0042] B-1-2. Protective film

[0043] As the protective film, any appropriate resin film can be used. As the forming material of the resin film, for example, cellulose resins such as (meth) acrylic resins, diacetyl cellulose, triacetyl cellulose, cycloolefin resins such as norbornene resins, olefin resins such as polypropylene, ester resins such as polyethylene terephthalate resins, polyamide resins, polycarbonate resins, and their copolymer resins can be listed. It should be noted that "(meth) acrylic resin" refers to acrylic resin and / or methacrylic resin.

[0044] The thickness of the protective film is typically 10 μm to 100 μm, preferably 20 μm to 40 μm. The protective film is typically laminated on the polarizer with the aid of an adhesive layer (specifically, an adhesive layer, an adhesive layer). The adhesive layer is typically formed by a PVA-based adhesive or an active energy ray-curable adhesive. The adhesive layer is typically formed by an acrylic adhesive. The acrylic adhesive may be the same as or different from the adhesive constituting the first adhesive layer or the second adhesive layer.

[0045] C. 1st adhesive layer

[0046] As the adhesive constituting the first adhesive layer, any suitable adhesive having adhesiveness and transparency that can be used for optical purposes can be adopted. As a specific example, acrylic adhesive, rubber adhesive, silicone adhesive, polyester adhesive, urethane adhesive, epoxy adhesive and polyether adhesive can be listed. The base resin of the adhesive can only use one, or two or more can be used in combination. From the viewpoints such as transparency, processability and durability, acrylic adhesive is preferably used.

[0047] The acrylic adhesive composition typically includes a (meth)acrylic polymer as a main component (base polymer). The (meth)acrylic polymer can be included in the adhesive composition in a proportion of, for example, 50% by weight or more, preferably 70% by weight or more, and more preferably 90% by weight or more of the solid content of the adhesive composition. As for the (meth)acrylic polymer, as a monomer unit, it contains an alkyl (meth)acrylate as a main component. It should be noted that the (meth)acrylate is an acrylate and / or a methacrylate. As the alkyl group of the alkyl (meth)acrylate, for example, a linear or branched alkyl group having 1 to 18 carbon atoms can be listed. The average carbon number of the alkyl group is preferably 3 to 9. As monomers constituting the (meth)acrylic polymer, in addition to the alkyl (meth)acrylate, copolymer monomers such as carboxyl-containing monomers, hydroxyl-containing monomers, amide-containing monomers, aromatic ring-containing (meth)acrylates, and heterocyclic (meth)acrylates can be listed. The copolymer monomer is preferably a hydroxyl-containing monomer and / or a heterocyclic (meth)acrylate, and more preferably N-acryloylmorpholine. The acrylic adhesive composition may preferably contain a silane coupling agent and / or a crosslinking agent. As the silane coupling agent, for example, an epoxy-containing silane coupling agent may be cited. As the crosslinking agent, for example, an isocyanate crosslinking agent and a peroxide crosslinking agent may be cited. The details of such an adhesive layer or acrylic adhesive composition are, for example, recorded in Japanese Unexamined Patent Publication No. 2014-115468 and Japanese Patent No. 4140736, and the records of the publication are cited in this specification as a reference.

[0048] The thickness of the first adhesive layer can be set to any appropriate value. The thickness of the first adhesive layer is preferably 20 μm or more, more preferably 40 μm or more, and further preferably 50 μm or more. In addition, the thickness of the first adhesive layer is preferably 500 μm or less, more preferably 350 μm or less, and further preferably 250 μm or less.

[0049] The storage modulus G' of the first adhesive layer at 25°C is preferably 1.0×10 4 Pa~1.0×10 7 Pa, more preferably 3.0×10 4 Pa~7.0×10 6 Pa, more preferably 5.0×10 4 Pa~5.0×10 6 Pa. By setting the storage modulus G' at 25°C to such a range, deformation of the adhesive layer can be prevented even when pressure is applied during lamination. Alternatively, through holes can be well formed in an optical laminate with an adhesive layer. It should be noted that in this specification, the storage modulus G' refers to a value measured according to the method described in JIS K7244-1 "Plastics - Test methods for dynamic mechanical properties".

[0050] D. Second adhesive layer

[0051] As the adhesive constituting the second adhesive layer, the same adhesive as the adhesive constituting the first adhesive layer can be used, or different adhesives can be used. When using an adhesive different from the first adhesive layer, as the adhesive, the conventional adhesive known in the art can be used. Specifically, adhesives based on polymers of rubber systems such as acrylic acid polymers, silicone polymers, polyesters, polyurethanes, polyamides, polyvinyl ethers, vinyl acetate / vinyl chloride copolymers, modified polyolefins, epoxy systems, fluorine systems, natural rubber, synthetic rubbers, etc. can be listed.

[0052] The thickness of the second pressure-sensitive adhesive layer can be set to any appropriate value, and is preferably 3 μm to 500 μm, more preferably 5 μm to 350 μm, further preferably 10 μm to 250 μm, and particularly preferably 10 μm to 150 μm.

[0053] The storage modulus G' of the second adhesive layer at 25°C is preferably 1.0×10 4 Pa~1.0×10 7 Pa, more preferably 3.0×10 4 Pa~5.0×10 6 Pa, more preferably 5.0×10 4 Pa~1.0×10 6Pa. When the storage elastic modulus G' of the second pressure-sensitive adhesive layer is within the above range, the optical laminate can be bonded well. In addition, through-holes can be formed well in the pressure-sensitive adhesive layer-attached optical laminate.

[0054] E. Other layers

[0055] The optical laminate with adhesive layer may further have any appropriate other layer except the above-mentioned optical film, the first and second adhesive layers. As other layers, the above-mentioned isolation film and optical functional film can be listed. The isolation film is used to properly protect the first adhesive layer and the second adhesive layer until use. The optical functional film is used to give the optical laminate with adhesive layer the desired optical function corresponding to the purpose. As the optical functional film, for example, a protective film of a polarizer or polarizing plate, an anti-reflection film, an anti-glare film, a conductive film for a touch panel, a pressure-sensitive film, etc. can be listed.

[0056] F. Method for producing an optical laminate with an adhesive layer

[0057] The optical laminate with adhesive layer of the present invention can be manufactured by any appropriate method. Preferably, the manufacturing method of the optical laminate with adhesive layer includes: a step of forming a first adhesive layer on one side of an optical film; a step of forming a second adhesive layer on the other side of the optical film; and a step of forming a through hole that integrally penetrates the first adhesive layer, the optical film and the second adhesive layer.

[0058] F-1. Formation of adhesive layer

[0059] The first adhesive layer and the second adhesive layer can be formed on the optical film by any appropriate method. For example, the adhesive layer can be formed by coating the optical film with an adhesive for forming the first adhesive layer or an adhesive for forming the second adhesive layer, or the adhesive layer can be formed by coating an adhesive on a release film or other resin film and then transferring the adhesive layer to the optical film. In addition, the first adhesive layer and the second adhesive layer can be formed in any appropriate order.

[0060] In one embodiment, the through-holes formed in the first adhesive layer and the second adhesive layer are larger than the through-holes formed in the optical film. In this embodiment, for example, the adhesive layer can be formed in such a manner that the ends of the through-holes formed in the adhesive layer and the ends of the through-holes formed in the optical film are at any appropriate distance.

[0061] As a coating method for the adhesive composition, any appropriate coating method can be used, for example, roll coating, lick roll coating, gravure coating, reverse coating, roller brush, spray coating, dip roll coating, rod coating, blade coating, air knife coating, curtain coating, lip coating, extrusion coating using a die coater, etc. can be listed.

[0062] F-2. Formation of through holes

[0063] The optical film having the first adhesive layer and the second adhesive layer is then formed with a through hole that integrally penetrates the first adhesive layer and the second adhesive layer. When forming the through hole, in order to appropriately protect the adhesive layer, a separator or a surface protection film is preferably laminated on the first adhesive layer and the second adhesive layer.

[0064] The through hole can be formed by any appropriate method. For example, a punching blade such as a Thomson blade or a Pinnacle blade, a cutting process based on a mandrel, a punching process based on a cutter or a laser, etc. can be listed. The processing conditions when forming the through hole can be set to any appropriate conditions according to the through hole forming means used, the thickness of the first adhesive layer, the optical film, the second adhesive layer, and the optional isolation film or surface protection film, the type of the optical film, etc.

[0065] In one embodiment, the through hole is formed in the following manner: the first adhesive layer, the optical film, and the second adhesive layer are integrally penetrated in a state where the first adhesive layer and the second adhesive layer are laminated on the optical film. By forming the through hole in a state where the first adhesive layer and the second adhesive layer are laminated on the optical film, it is possible to suppress deformation of the hole shape caused by tension and pressure when the layers are attached and / or when the separator is peeled off.

[0066] F-3. Other processes

[0067] The method for producing an optical laminate with an adhesive layer of the present invention may include any appropriate steps in addition to the above-mentioned steps of forming the adhesive layer and the step of forming the through-holes. For example, the steps include: a step of peeling off the surface protection film used in the step of forming the through-holes, a step of laminating a separator on the adhesive layer from which the surface protection film has been peeled off, etc.

[0068] G. Use of the optical laminate with pressure-sensitive adhesive layer

[0069] As described above, the optical laminate with adhesive layer of the present invention can make various functions (such as functions based on cameras, speakers, and various sensors) possessed by high-function image display devices highly exerted. Therefore, it can be suitably used in image display devices. As image display devices, for example, liquid crystal display devices and organic EL devices can be listed. Specifically, the liquid crystal display device has a liquid crystal panel including a liquid crystal unit and the above-mentioned polarizer configured on one side or both sides of the liquid crystal unit. The organic EL device has an organic EL panel configured with the above-mentioned polarizer on the recognition side.

[0070] In the image display device, the optical laminate with a pressure-sensitive adhesive layer of the present invention can be laminated on any appropriate adherend, such as a glass plate, a cell, and other optical laminates. The image display device will be described in detail below.

[0071] G-1. Image display device

[0072] The image display device of the present invention comprises: the above-mentioned optical laminate with an adhesive layer, a display panel arranged on one side of the optical laminate with an adhesive layer and having a through hole in a portion corresponding to the through hole of the optical laminate with an adhesive layer; and a glass layer or a plastic layer arranged on the other side of the optical laminate with an adhesive layer.

[0073] Figure 2 Schematic cross-sectional view of an image display device according to an embodiment of the present invention. The image display device 200 of the illustrated example includes an optical laminate 100, wherein the optical laminate 100 has: an optical film 10, a first adhesive layer 20 formed on one side of the optical film 10, and a second adhesive layer 30 formed on the other side of the optical film 10. In the illustrated example, a glass layer or a plastic layer 140 is laminated on the first adhesive layer 20, and a display panel 150 is laminated on the second adhesive layer 30. The display panel 150 has through holes at positions corresponding to the through holes formed in the optical film 100. In the illustrated example, a glass layer or a plastic layer 140 is laminated on the first adhesive layer 20, and a display panel 150 having through holes is laminated on the second adhesive layer 30, but a display panel 150 having through holes may be laminated on the first adhesive layer 20, and a glass layer or a plastic layer 140 may be laminated on the second adhesive layer 30. As described above, the through holes of the optical laminate are formed in a manner that becomes a position, size, quantity and shape corresponding to the camera, speaker and various sensors to be carried by the image display device. Not only the optical laminate, but also the display panel has a through hole corresponding to the through hole of the optical laminate, thereby, the functions of the camera, speaker and various sensors, etc. will not be hindered by the optical laminate and the display panel, and can be fully exerted. Representatively, it can be configured in a manner that a glass layer or a plastic layer 140 is laminated on the first adhesive layer 20 of the optical laminate with an adhesive layer and becomes the recognition side of the image display device.

[0074] As described above, in one embodiment, the through hole is a through hole that penetrates the optical laminate in a tapered manner. In this embodiment, the difference in size between the planar shape of the first through hole and / or the planar shape of the second through hole and the planar shape of the through hole formed in the display panel can be set to any appropriate value. The difference in size between the planar shape of the first through hole and / or the planar shape of the second through hole and the planar shape of the through hole formed in the display panel is preferably 500 μm or less, more preferably 300 μm or less, and further preferably 100 μm or less. By making the difference in size between the planar shape of the first through hole and / or the planar shape of the second through hole and the planar shape of the through hole formed in the display panel within the above range, the width of the black frame printing can be reduced and the appearance can be improved. It should be noted that the difference in size between the planar shape of the first through hole and the planar shape of the through hole formed in the display panel, and the difference in size between the planar shape of the second through hole and the planar shape of the through hole formed in the display panel, as long as the two differences are within the above range, can be the same or different.

[0075] The image display device 200 may further include any appropriate other components. For example, any appropriate other components may be included between the first adhesive layer and the second adhesive layer of the optical laminate 100 and the glass layer or plastic layer, or the display panel having a through hole. As other components, for example, a phase difference layer, an anti-reflection layer, a protective layer, a conductive film for a touch panel, a pressure-sensitive film, etc. can be listed. These other components are bonded to the optical laminate 100, the glass layer or plastic layer, or the display panel having a through hole by means of any appropriate adhesive layer or adhesive layer.

[0076] G-2. Method for manufacturing image display device

[0077] The image display device of the present invention can be manufactured by any appropriate method. In one embodiment, the manufacturing method of the image display device of the present invention includes: a process of forming a through hole in an optical film; a process of forming a first adhesive layer on one side of the optical film; a process of forming a through hole in the first adhesive layer; a process of forming a second adhesive layer on the other side of the optical film; a process of forming a through hole in the second adhesive layer; a process of forming a through hole in a display panel; a process of laminating the display panel on one side of the optical film; and a process of laminating a glass layer or a plastic layer on the other side of the optical film.

[0078] As described above, the optical film, the first adhesive layer and the second adhesive layer contained in the image display device have through holes. Regarding the through holes, the layers can be stacked after forming through holes in the optical film, the first adhesive layer, the second adhesive layer and the display panel, respectively, or the optical film, the first adhesive layer, the second adhesive layer and the display panel can be stacked and through holes can be formed in the stack (that is, through holes can also be formed in the optical film, the first adhesive layer, the second adhesive layer and the display panel at the same time). Preferably, the process of forming through holes in the optical film, the process of forming through holes in the first adhesive layer, the process of forming through holes in the second adhesive layer, and the process of forming through holes in the display panel are carried out simultaneously. As a method for forming through holes simultaneously, for example, a through hole can be formed in a state where the optical film, the first adhesive layer, the second adhesive layer and the display panel are stacked.

[0079] In another embodiment, the image display device can be made by laminating the above-mentioned optical laminate and a display panel having a through hole corresponding to the through hole of the optical laminate. In this embodiment, through holes are also formed in the adhesive layer formed between the optical laminate and the display panel. The formation of the through holes in the adhesive layer can be carried out simultaneously with the display panel (in a state where the adhesive layer is laminated on the display panel), or an adhesive layer having through holes formed separately can be attached to the optical laminate or the display panel. The through holes formed in the adhesive layer are formed in a position and size corresponding to the through holes formed in the above-mentioned optical laminate and the display panel.

[0080] The pressure-sensitive adhesive layer can be formed by any appropriate method, for example, by the method described in F-1 above.

[0081] The through hole can be formed by any appropriate method. For example, it can be formed by the method described in F-2. When the through hole is formed in the adhesive layer, it is preferred to form the adhesive layer on any appropriate substrate and / or separator, and form the through hole in a state where the adhesive layer is sandwiched by the substrate and / or separator.

[0082] Example

[0083] The present invention will be specifically described below by way of examples, but the present invention is not limited to these examples. Evaluation items in the examples are as follows.

[0084] (1) Quality of through-holes

[0085] The quality of the through-holes of the display panels of the respective examples and comparative examples was evaluated according to the following criteria: The state of the through-holes was visually confirmed.

[0086] Advantages: The hole position is consistent between layers, which can reduce the non-display area

[0087] Good: The hole positions are slightly offset between the layers, which makes it practical by increasing the non-display area.

[0088] No: The position of the hole is too far away and cannot be used practically

[0089] (2) Camera adaptability

[0090] The image quality of the camera of the display panel of each example and comparative example was evaluated according to the following criteria.

[0091] Good: Except for the outermost layer, all layers including the panel have through holes, which can prevent the reflection of light at the interface, so the image quality is good and suitable for camera counterparts.

[0092] No: There is a layer without through holes. The image quality is impaired due to light reflection at the interface. It is not suitable for camera-compatible parts.

[0093] (3) Ease of production

[0094] The manufacturing process of the display panel of each example and comparative example was evaluated according to the following criteria.

[0095] Advantages: Fewer punching times, no need to align the through-hole positions during lamination

[0096] Good: Fewer punches are needed, but the holes must be aligned properly.

[0097] No: The number of punching times is very large, and the number of laminations that require alignment of the through-hole positions is also large. As the adhesive laminate A, use CS9866US (a product with a heavy-peel release film / adhesive layer A (thickness 150 μm, storage modulus G' at 25°C: 0.14 MPa) / light-peel release film structure manufactured by Nitto Denko Corporation).

[0098] As the adhesive laminate B, a product of Nitto Denko Corporation, product name: CS9864US (a product having a structure of heavy release film / adhesive layer B (thickness 100 μm, storage elastic modulus G′ at 25° C.: 0.14 MPa) / light release film) was used.

[0099] Manufacturing Example 1: Preparation of Adhesive Composition 1

[0100] In a detachable flask equipped with a thermometer, a stirrer, a reflux condenser and a nitrogen inlet tube, 99 parts by weight of butyl acrylate (BA) as a monomer component, 1 part by weight of 4-hydroxybutyl acrylate (4HBA), 0.2 parts by weight of azobisisobutyronitrile as a polymerization initiator and ethyl acetate as a polymerization solvent were added to make the solid content 20%. Then, nitrogen was circulated and nitrogen substitution was performed for about 1 hour while stirring. The flask was then heated to 60°C and reacted for 7 hours to obtain an acrylic polymer with a weight average molecular weight (Mw) of 1.1 million. 0.8 parts by weight of trimethylolpropane toluene diisocyanate ("Coronate L" manufactured by Nippon Polyurethane Industry Co., Ltd.) and 0.1 parts by weight of a silane coupling agent ("KBM-403" manufactured by Shin-Etsu Chemical Co., Ltd.) as an isocyanate crosslinking agent were added to the above-mentioned acrylic polymer solution (100 parts by weight of solid content) to prepare an adhesive composition (solution).

[0101] Production Example 2: Preparation of Adhesive Laminated Body C

[0102] The obtained adhesive solution was applied to a polyethylene terephthalate release liner having a thickness of 38 μm or 50 μm so as to have a thickness of 20 μm after drying, and then heated and dried at 60° C. for 1 minute under normal pressure and then heated and dried at 150° C. for 1 minute to prepare a laminate having an adhesive layer C (adhesive laminate). This adhesive laminate was used as adhesive laminate C.

[0103] <Production of polarizer>

[0104] A laminate having a polyvinyl alcohol (PVA) resin layer (thickness: 9 μm) formed on an amorphous polyethylene terephthalate (PET) substrate was subjected to aerial auxiliary stretching at a stretching temperature of 130° C. to produce a stretched laminate. Next, the stretched laminate was dyed with iodine to obtain a colored laminate. Then, the colored laminate was stretched in boric acid water at a stretching temperature of 65° C. to a total stretching ratio of 5.94 times, to produce a laminate having a PVA resin layer (polarizer) having a thickness of 5 μm stretched integrally with the amorphous PET substrate.

[0105] <Production of single-side protective polarizing plate>

[0106] A polyvinyl alcohol-based adhesive was applied to the surface of the polarizer side of the laminate having the above-mentioned PVA resin layer in such a manner that the thickness of the adhesive layer was 0.1 μm, and a transparent protective film (a film obtained by corona-treating a (meth) acrylic resin film having a lactone ring structure having a thickness of 20 μm) (film b-1) was attached and dried at 50° C. for 5 minutes. Next, the amorphous PET substrate was peeled off to prepare a single-side protected polarizing plate.

[0107] <Example 1>

[0108] The adhesive laminate C was bonded to the polarizer of the single-sided protective polarizing plate via the adhesive layer C. Next, the separator on one side was peeled off from the adhesive laminate A, and the peeled surface was bonded to the protective layer of the single-sided protective layer polarizing plate. Through holes (circular, 5 mm in diameter) were formed in the obtained optical laminate with an adhesive layer to obtain an optical laminate with a separator and an adhesive layer.

[0109] Similarly, through holes (circular, 5 mm in diameter) were formed at positions corresponding to the through holes of the pressure-sensitive adhesive layer-attached optical laminate in the display panel (organic EL (OLED) panel).

[0110] The separator was peeled off from the adhesive layer A of the optical laminate with the separator and the adhesive layer, and a cover glass (thickness 0.5 mm) was attached. In addition, the separator was peeled off from the adhesive layer C, and a display panel with through holes was attached in a manner that the through holes of the optical laminate with the adhesive layer corresponded to the positions of the through holes of the display panel, thereby obtaining an image display device 1.

[0111] <Example 2>

[0112] The adhesive layer A was formed with through holes (circular, 5 mm in diameter).

[0113] Adhesive laminate C was bonded to the polarizer protecting the polarizing plate on one side via adhesive layer C. Next, the release liner was peeled off, and the display panel (OLED panel) was bonded via adhesive layer C. Next, through holes (circular, 5 mm in diameter) were formed at positions corresponding to the through holes formed in the above-mentioned adhesive laminate A, to obtain a display panel with an optical laminate having through holes formed therein.

[0114] Then, the separator on one side was peeled off from the adhesive laminate A, and a glass cover sheet (thickness 0.5 mm) was attached. Next, the other separator of the adhesive laminate A was peeled off, and the through-holes of the adhesive layer A and the through-holes of the display panel with the optical laminate were aligned and attached to obtain an image display device 2.

[0115] <Example 3>

[0116] An adhesive layer A with a separator film peeled off on one side was laminated on an optical film (manufactured by Japan Zeon Co., Ltd., product name: ZF14-050) via an adhesive layer A. Next, an adhesive layer B with a separator film peeled off on one side was laminated on the other side of the optical film via an adhesive layer B to prepare an optical film laminate. Through holes (circular, 5 mm in diameter) were formed in the obtained optical film laminate to obtain an optical film laminate having through holes formed therein.

[0117] After the adhesive laminate C is laminated on the polarizer of the single-side protective polarizing plate with the aid of the adhesive C, the separator is peeled off and the display panel (OLED panel) is laminated to obtain a display panel with an optical laminate. Next, a through hole (circular, 5 mm in diameter) is formed at a position of the display panel with an optical laminate corresponding to the through hole of the optical film laminate having the through hole formed therein, to obtain a display panel with an optical laminate having the through hole formed therein.

[0118] The isolation film is peeled off from the adhesive layer A of the optical film stack having through holes, and after pasting a glass cover (thickness 0.5 mm), the isolation film is peeled off from the adhesive stack B, and the polarizer of the optical film stack having through holes and the display panel of the optical stack having through holes are aligned with each other's through holes and pasted together to obtain an image display device 3.

[0119] <Example 4>

[0120] PSA laminate A with one release film peeled off was bonded to one side of an optical film (manufactured by Zeon Co., Ltd., product name: ZF14-050), and PSA laminate B with one release film peeled off was bonded to the other side to obtain an optical film having a PSA layer.

[0121] Separately, the adhesive laminate C was laminated on the polarizer protecting the polarizing plate on one side via the adhesive C, and then the separator was peeled off and a display panel (OLED panel) was laminated to obtain a display panel with an optical laminate.

[0122] The separator was peeled off from the adhesive layer B of the optical film having an adhesive layer, and the polarizer of the display panel with the optical laminate was bonded via the adhesive layer B. Then, a through hole (circular, 5 mm in diameter) was formed at a predetermined position of the bonded laminate. Then, the separator was peeled off from the adhesive layer A, and a cover glass (thickness 0.5 mm) was bonded, thereby obtaining an image display device 4.

[0123] <Example 5>

[0124] The pressure-sensitive adhesive layer stack C is bonded to the polarizer that protects the polarizing plate on one side via the pressure-sensitive adhesive layer C to obtain a pressure-sensitive adhesive layer-attached polarizing plate.

[0125] Next, through holes (circular, 5 mm in diameter) were formed at predetermined positions of the polarizing plate with an adhesive layer, adhesive laminate A, adhesive laminate B, touch screen panel (TSP), and display panel (OLED panel).

[0126] Then, the layers formed with through holes and a glass cover sheet (thickness 0.5 mm) were stacked in the order of glass cover sheet / adhesive layer A / TSP / adhesive layer B / protective layer / polarizer / adhesive layer C / display panel to obtain an image display device 5. It should be noted that the layers having through holes were laminated in a manner such that the positions of the respective through holes corresponded to each other.

[0127] <Example 6>

[0128] Image display device 6 was obtained in the same manner as in Example 3 except that the configuration of the image display device was changed to cover glass / adhesive layer A / protective layer / polarizer / adhesive layer C / TSP / adhesive layer B / display panel.

[0129] <Example 7>

[0130] The above-mentioned adhesive laminate C is attached to the polarizer of the single-sided protective polarizer with the aid of the adhesive layer C to obtain a polarizer with an adhesive layer. Next, the isolation film on one side is peeled off from the above-mentioned adhesive laminate A, and the peeled surface is attached to the protective layer of the single-sided protective layer polarizer. Then, the isolation film is peeled off from the adhesive layer C and attached to the display panel (OLED panel), and a through hole (circular, 5 mm in diameter) is formed at a specified position. Then, the isolation film is peeled off, and a glass cover (thickness 0.5 mm) is laminated with the adhesive layer A to obtain an image display device 7.

[0131] <Example 8>

[0132] The above-mentioned adhesive laminate C is attached to the polarizer of the single-sided protective polarizer with the aid of an adhesive layer C to obtain a polarizer with an adhesive layer. Then, the isolation film is peeled off from the adhesive layer C, and the polarizer is attached to the display panel (OLED panel) with the aid of an adhesive layer C. Next, adhesive laminate B, TSP, and adhesive laminate A are sequentially stacked on the protective layer side of the polarizer with an adhesive layer to obtain a laminate stacked in the order of adhesive layer A / TSP / adhesive layer B / protective layer / polarizer / adhesive layer C / display panel. A through hole (circular, 5 mm in diameter) is formed at a specified position of the laminate. Then, the isolation film is peeled off from the laminate formed with a through hole, and a glass cover sheet (0.5 mm in thickness) is stacked with the aid of an adhesive layer A to obtain an image display device 8.

[0133] (Comparative Example 1)

[0134] A through hole (circular, 5 mm in diameter) was formed in the display panel (OLED panel).

[0135] Separately, the above-mentioned adhesive laminate C is laminated to the polarizer of the single-side protective polarizing plate via the adhesive layer C to obtain a polarizing plate with an adhesive layer. The isolation film is peeled off from the adhesive layer C of the polarizing plate with an adhesive layer, and laminated to the display panel formed with a through hole. Next, the adhesive laminate A is laminated to the protective layer of the polarizing plate with an adhesive layer, and a glass cover sheet (thickness 0.5 mm) is laminated via the adhesive layer A to obtain an image display device C1.

[0136] (Comparative Example 2)

[0137] A through hole (circular, 5 mm in diameter) was formed in the display panel (OLED panel).

[0138] Separately, the above-mentioned adhesive laminate C is laminated to the polarizer of the single-sided protective polarizing plate with the aid of an adhesive layer C to obtain a polarizing plate with an adhesive layer. The isolation film is peeled off from the adhesive layer C of the polarizing plate with an adhesive layer and laminated to a display panel having a through hole. Next, an adhesive laminate B is laminated to the protective layer of the polarizing plate with an adhesive layer, and TSP is laminated with the aid of the adhesive layer B. Then, the adhesive laminate A is laminated on the TSP, and a glass cover sheet (thickness 0.5 mm) is laminated with the aid of the adhesive layer A to obtain an image display device C2.

[0139] [Table 1]

[0140] Quality of through-holes Camera quality Ease of process Example 1 good good good Example 2 good good good Example 3 good good good Example 4 excellent good excellent Example 5 good good No Example 6 good good No Example 7 excellent good excellent Example 8 excellent good excellent Comparative Example 1 excellent No good Comparative Example 2 excellent No good

[0141] <Examples 9 to 11> (Comparative Example 3)

[0142] A through hole (circular, 5 mm in diameter) is formed at a predetermined position of the above-mentioned single-sided protective polarizing plate. Next, through holes are formed in the adhesive laminate A and the adhesive laminate C in such a way that the distance from the end of the through hole formed in the single-sided protective polarizing plate is the value recorded in Table 2. Next, the isolation film on one side is peeled off from the adhesive laminate A and the adhesive laminate C, and the center of the through hole formed in the adhesive layer is aligned with the center of the through hole formed in the polarizing plate to obtain an optical laminate (isolation film / adhesive layer A / protective layer / polarizer / adhesive layer C / isolation film). The through holes of the optical laminate obtained are visually confirmed from the adhesive layer A side to evaluate the presence or absence of overflow of the adhesive layer.

[0143] [Table 2]

[0144]

[0145] <Example 12>

[0146] The separator on one side was peeled off from the adhesive laminate B, and the adhesive layer B was laminated on the protective layer side of the above-mentioned single-sided protective polarizing plate. The adhesive laminate D was obtained in the same manner as in Production Example 2 except that the coating was performed so that the thickness after drying was 25 μm. The separator on one side was peeled off from the obtained adhesive laminate D, and the adhesive layer D was laminated on the polarizer of the above-mentioned single-sided protective polarizing plate. Through holes (circular, 5 mm in diameter) were formed at predetermined positions of the obtained laminate of the separator / adhesive layer B / protective layer / polarizer / adhesive layer D / separator to obtain an optical laminate.

[0147] <Example 13>

[0148] Adhesive stack A is used instead of adhesive stack B, and a phase difference film (thickness 50 μm) is used instead of the single-sided protective polarizing plate. The adhesive stack is applied in a manner such that the thickness after drying is 100 μm. Otherwise, adhesive stack E is prepared in the same manner as in Manufacturing Example 2, and an optical stack is prepared in the same manner as in Example 12 except that adhesive stack E is used.

[0149] <Example 14>

[0150] An adhesive laminate F was prepared in the same manner as in Production Example 2, except that a transparent film (thickness 50 μm) was used instead of the single-sided protective polarizing plate and the coating was performed so that the thickness after drying was 50 μm. An optical laminate was prepared in the same manner as in Example 12, except that the adhesive laminate F was used.

[0151] (Comparative Example 4)

[0152] Through holes (circular shape, diameter: 5 mm) were formed at predetermined positions of the adhesive layered body B to obtain a layered body.

[0153] The following evaluations were performed using the laminates having through holes obtained in Examples 12 to 14 and Comparative Example 4.

[0154] The diameters of the through holes of the laminates obtained in Examples 12 to 14 and Comparative Example 4 were processed, and then laminated to a panel just after peeling off one separator, and then measured respectively. The profile was calculated by the following formula based on the obtained values. It should be noted that the diameter of the through hole was the value of the part with the largest diameter value as the diameter of the through hole. The results are shown in Table 3.

[0155] Profile = designed through hole diameter / measured through hole diameter

[0156] [Table 3]

[0157]

[0158] <Examples 15 to 17> (Comparative Examples 5 to 6)

[0159] The separator on one side is peeled off from the adhesive laminate A, and the adhesive layer A is laminated on the protective layer of the single-sided protective polarizing plate. Next, the separator on one side is peeled off from the adhesive laminate C, and the adhesive layer C is laminated on the polarizer of the single-sided protective polarizing plate to obtain an optical laminate. The diameter of the through hole on the outermost surface of the adhesive layer A (the surface on the separator side) is set to The diameter of the through-holes on the outermost surface of the adhesive layer C (surface on the separator side) is denoted as by and Tapered through-holes were formed so as to have the values ​​described in Table 4, thereby obtaining an optical layered body having through-holes.

[0160] Separately, a black frame having the outer diameter, inner diameter and width shown in Table 4 was printed on the panel. Next, the separator of the adhesive layer C was peeled off, and the optical laminate was laminated on the panel by aligning the center of the through hole with the center of the black frame printed on the panel.

[0161] The following evaluations were performed on the laminated bodies of Examples 15 to 17 and Comparative Examples 5 and 6.

[0162] (Appearance)

[0163] The through-holes of the obtained laminate were visually checked from the viewing side (adhesive layer A side), and it was evaluated whether the cross section of the hole and the cross section of the display region were visible.

[0164] (Wide Angle)

[0165] A camera module was arranged on the panel side of the obtained laminated body corresponding to the through-holes, and the degree of widening of the angle of view was evaluated based on the following criteria from the captured images.

[0166] Good: The shooting area is wide, and the cross section of the through hole does not enter the shooting area at all, which does not hinder image capture

[0167] Good: The shooting area is slightly narrow, but the cross section of the through hole does not enter the shooting area, which does not hinder image capture. Acceptable: The shooting area is narrow, but the cross section of the through hole does not enter the shooting area, which does not hinder image capture. Unacceptable: The shooting area is narrow, and the cross section of the through hole is included in the shooting area.

[0168] (Appearance)

[0169] The appearance of the through-holes was evaluated according to the following criteria.

[0170] Pros: The black frame cannot be seen through the through hole

[0171] Good: The black frame can be slightly discerned from the through hole

[0172] Yes: The black frame can be seen through the through hole without affecting the appearance.

[0173] No: The black frame can be clearly seen through the through hole, and the size of the camera-related part is smaller than the designed through hole size.

[0174] [Table 4]

[0175]

[0176] <Examples 18 to 20> (Comparative Example 7)

[0177] The separator on one side is peeled off from the adhesive laminate A, and the adhesive layer A is laminated on the protective layer of the single-sided protective polarizing plate. Next, the separator on one side is peeled off from the adhesive laminate C, and the adhesive layer C is laminated on the polarizer of the single-sided protective polarizing plate to obtain an optical laminate. The diameter of the through hole on the outermost surface of the adhesive layer A (the surface on the separator side) is set to The diameter of the through-holes on the outermost surface of the adhesive layer C (surface on the separator side) is denoted as by and Tapered through-holes were formed so as to have the values ​​described in Table 4, thereby obtaining an optical layered body having through-holes.

[0178] Separately, a black frame having the outer diameter, inner diameter and width shown in Table 5 was printed on the panel. Next, the separator of the adhesive layer C was peeled off, and the optical layered body was laminated on the panel by aligning the center of the through hole with the center of the black frame printed on the panel.

[0179] The laminated bodies of Examples 18 to 20 and Comparative Example 7 were evaluated as follows.

[0180] (put one's oar in)

[0181] A camera module was placed on the panel side of the obtained laminate so as to correspond to the through-hole, and the presence or absence of interference with the through-hole of the camera module was evaluated according to the following criteria.

[0182] Advantage: The camera module does not contact the through hole, and the distance between the camera module and the identification side surface of the optical stack can be shortened.

[0183] Good: Although the camera module is in contact with the through hole, it has no effect on the shooting function and can shorten the distance between the camera module and the identification side surface of the optical stack.

[0184] [Table 5]

[0185]

[0186] <Examples 21 to 23> (Comparative Example 8)

[0187] The separator on one side is peeled off from the adhesive laminate A, and the adhesive layer A is laminated on the protective layer of the single-sided protective polarizing plate. Next, the separator on one side is peeled off from the adhesive laminate C, and the adhesive layer C is laminated on the polarizer of the single-sided protective polarizing plate to obtain an optical laminate. The diameter of the through hole on the outermost surface of the adhesive layer A (the surface on the separator side) is set to The diameter of the through-holes on the outermost surface of the adhesive layer C (surface on the separator side) is denoted as by and Tapered through-holes were formed so as to have the values ​​described in Table 6, thereby obtaining an optical layered body having through-holes.

[0188] Separately, a black frame having the outer diameter, inner diameter and width shown in Table 6 was printed on the panel. Next, the separator of the adhesive layer C was peeled off, and the optical laminate was laminated on the panel by aligning the center of the through hole with the center of the black frame printed on the panel.

[0189] The following evaluations were performed on the laminated bodies of Examples 21 to 23 and Comparative Example 8. The results are shown in Table 6.

[0190] (end visible)

[0191] The through-hole was visually confirmed from the identification side to evaluate whether the end of the through-hole cross section could be seen from the through-hole. In any of the examples and comparative examples, the end could not be visually seen, which was an excellent result.

[0192] (Black frame width)

[0193] The degree to which the opening of the through-hole was affected by the black frame was evaluated according to the following criteria.

[0194] Pros: The edge of the black frame cannot be seen through the through hole, which does not hinder the wide-angle of the camera.

[0195] Good: The edge of the black frame can be seen through the through hole, but it does not hinder the wide-angle of the camera.

[0196] Possible: The width of the black frame can be seen through the through hole, but it is not enough to prevent the camera from widening its angle.

[0197] No: A black frame can be seen through the opening of the through hole, and the camera cannot be widened.

[0198] [Table 6]

[0199]

[0200] Industrial Applicability

[0201] The optical layered body of the present invention can be suitably used in image display devices such as liquid crystal display devices and organic EL devices.

[0202] Description of Reference Numerals

[0203] 10 Optical Film

[0204] 20 1st adhesive layer

[0205] 30 Second adhesive layer

[0206] 40 Isolation film

[0207] 50 Through hole

[0208] 100 Optical laminate with adhesive layer

[0209] 140 Glass layer or plastic layer

[0210] 150 Display Panel

[0211] 200 Image display device

Claims

1. An optical laminate with an adhesive layer, comprising: Optical films, a first adhesive layer formed on one side of the optical film, and a second adhesive layer formed on the other side of the optical film, The optical laminate with adhesive layer has a through hole that integrally penetrates the first adhesive layer, the optical film and the second adhesive layer. The size of the through-holes formed in the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer in a plan view is larger than the size of the through-holes formed in the optical film.

2. The optical laminate with an adhesive layer according to claim 1, wherein The optical film is at least one selected from the group consisting of a polarizing plate, a phase difference film, a conductive film for a touch panel, a pressure-sensitive film, and a transparent plastic film.

3. A method for producing an optical laminate with an adhesive layer, comprising: forming a first adhesive layer on one side of the optical film; forming a second adhesive layer on the other side of the optical film; as well as a step of forming a through hole that integrally penetrates the first adhesive layer, the optical film, and the second adhesive layer, The size of the through-holes formed in the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer in a plan view is larger than the size of the through-holes formed in the optical film.

4. An image display device, comprising: The optical laminate with an adhesive layer according to claim 1 or 2; a display panel disposed on one side of the optical laminate with the pressure-sensitive adhesive layer and having through holes in portions corresponding to the through holes in the optical laminate with the pressure-sensitive adhesive layer; and A glass layer or a plastic layer is disposed on the other surface of the optical laminate with a pressure-sensitive adhesive layer.

5. The image display device according to claim 4, wherein: The through hole of the pressure-sensitive adhesive layer-attached optical laminate and the through hole of the display panel are through holes that integrally penetrate the optical laminate and the display panel.

6. A method for manufacturing an image display device, comprising: A step of forming through holes in the optical film; forming a first adhesive layer on one side of the optical film; forming a through hole in the first adhesive layer; forming a second adhesive layer on the other side of the optical film; forming a through hole in the second adhesive layer; A step of forming a through hole in the display panel; A step of laminating the display panel on one side of the optical film; and The process of laminating a glass layer or a plastic layer on the other side of the optical film, The size of the through-holes formed in the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer in a plan view is larger than the size of the through-holes formed in the optical film.

7. The manufacturing method according to claim 6, wherein: The steps of forming a through hole in the optical film, forming a through hole in the first adhesive layer, forming a through hole in the second adhesive layer, and forming a through hole in the display panel are performed simultaneously.

Citation Information

Patent Citations

  • Manufacturing method of thin polarizing film

    JP2012073580A

  • Camera lens structures and display structures for electronic devices

    JP2014112238A

  • Optical film having adhesive agent on both sides, and manufacturing method of image display unit using the same

    JP2014115468A

  • Polarizing plate and image display unit