Antioxidant solder paste and preparation method thereof

By introducing modified rosin and nano-aluminum particles into the flux, antioxidant solder paste is prepared, which solves the problem of poor antioxidant performance of the solder paste, significantly improves solder stability and performance, especially excellent performance in high temperature and high humidity environments .

CN115091079BActive Publication Date: 2024-11-22SHENZHEN XINGHONGTAI TIN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210683175.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-16
Publication Date
2024-11-22
Estimated Expiration
2042-06-16

AI Technical Summary

Technical Problem

The antioxidant performance of existing solder pastes is poor, resulting in a decrease in welding quality. Especially in high temperature and humidity environments, tin powder oxidation and sandification are prone to occur, affecting welding performance.

Method used

By introducing modified rosin into the flux, using nano-aluminum particles and a specific solvent combination, acrylic resin modified rosin is prepared and mixed with tin powder to form an antioxidant solder paste, reducing the oxidation activity of the tin powder and improving welding Stability and performance.

Benefits of technology

It significantly improves the antioxidant ability of the solder paste, extends the viscosity holding time of the solder paste, reduces the oxidation phenomenon of the tin powder, and significantly improves the welding performance, especially in high temperature and high humidity environments.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of solder paste, and discloses an anti-oxidation solder paste and a preparation method thereof. The solder paste is prepared from the following components: tin powder and soldering flux; the soldering flux is prepared from the following components: acrylic resin modified rosin, a thixotropic agent, an activator, an organic solvent, and a surfactant; the anti-oxidation solder paste prepared by the invention coats the tin powder with the modified rosin, thereby greatly reducing the oxidation activity of the tin powder, thereby significantly increasing the welding performance of the tin powder; the solder paste prepared by the invention exhibits excellent anti-oxidation ability under the accelerated oxidation environment conditions of 45°C, RH 90%, and 48h.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solder paste, and in particular to an anti-oxidation solder paste and a preparation method thereof. Background Art

[0002] Solder paste is a new type of welding material that came into being with SMT. Solder paste is a complex system, which is a paste made of tin powder, flux and other additives. Solder paste has a certain viscosity at room temperature, which can initially stick electronic components to a predetermined position. At the welding temperature, as the solvent and some additives evaporate, the components to be welded are welded to the printed circuit pads to form a permanent connection.

[0003] For example, the Chinese invention patent with the prior art publication number CN112276412A discloses a laser welding solder paste and its preparation method. The technical scheme adopted is: a laser welding solder paste, composed of the following weight percentage raw materials, alloy powder 86-88%, paste flux 12-14%; the alloy powder is an alloy powder with a eutectic component mixed with one or more tin-based alloy powders; the paste flux is composed of the following weight percentage raw materials: rosin 35-50%, thixotropic agent 5-10%, organic acid activator 3-6%, organic halogen activator 1-3%, organic solvent 35-45%, special solvent 5-10%. The advantages of the present invention are: it can inhibit the boiling of the flux caused by rapid temperature rise, and achieve the effect of inhibiting the splashing of solder balls and flux generated by rapid heating of the solder paste. However, its antioxidant performance is relatively poor, which is easy to reduce the welding quality of the solder paste.

[0004] Based on this, we propose an anti-oxidation solder paste, hoping to solve the shortcomings of the existing technology. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides an anti-oxidation solder paste and a preparation method thereof.

[0006] To achieve the above-mentioned purpose, the present invention provides the following technical solutions:

[0007] An anti-oxidation solder paste is prepared from the following ingredients by weight: 85-92 parts of tin powder and 8-15 parts of flux;

[0008] The soldering flux is made of the following ingredients by weight: 28-35 parts of acrylic resin modified rosin, 3-5 parts of thixotropic agent, 1-2 parts of activator, 15-20 parts of organic solvent and 3-6 parts of surfactant.

[0009] As a further technical solution, the preparation method of the acrylic resin modified rosin comprises the following steps:

[0010] (1) performing a pre-modification treatment on an acrylic resin to obtain a pre-modified acrylic resin solution;

[0011] (2) uniformly dispersing the nano-aluminum particles into the coupling agent ethanol solution, adjusting the temperature to 40-50° C., stirring for 1-2 hours, and then filtering to obtain active nano-aluminum particles;

[0012] (3) In a reaction kettle, rosin is added to ethanol, stirred evenly, and then butyl acetate and active nano-aluminum particles are added, an inert gas is introduced, the air in the reaction kettle is exhausted, and then the temperature is adjusted to 70-75° C., and after being kept warm and stirred for 40-50 minutes, the pre-modified acrylic resin solution is slowly added dropwise. After the addition is completed, the temperature in the reaction kettle is continued to be adjusted to 60-68° C., and stirred at a speed of 500-600 r / min for 3-4 hours, and then the temperature is reduced to 35-38° C., and the temperature is kept warm for 30-40 minutes, and then naturally cooled to room temperature, and the material is discharged to obtain a reaction material;

[0013] (4) Purifying the reaction material to obtain acrylic resin modified rosin.

[0014] As a further technical solution, the preparation method of the pre-modified acrylic resin solution is:

[0015] (1) adding butyl acrylate and methyl acrylate to ethanol in sequence and stirring evenly to obtain a mixed solution;

[0016] (2) adding the initiator to deionized water and stirring evenly to prepare an initiator solution;

[0017] (3) adding castor oil and maleic acid to ethanol in sequence, stirring evenly, to prepare a modified liquid;

[0018] (4) Add the mixed solution to the reactor, adjust the temperature to 60-70°C, keep warm, add the modified solution and the initiator solution, stir and react for 2-3 hours, then cool naturally to room temperature, and discharge the material to obtain the product.

[0019] As a further technical solution: the mixing mass ratio of butyl acrylate, methyl acrylate and ethanol is 1-3:1-3:30.

[0020] As a further technical solution, the initiator is ammonium persulfate;

[0021] The mass fraction of the initiator solution is 5-8%;

[0022] The castor oil, maleic acid and ethanol are mixed in a mass ratio of 3-5:1-2:30;

[0023] The mass ratio of the mixed solution, the modified solution and the initiator solution is 20-25:3-5:5-8.

[0024] As a further technical solution, the mass ratio of the nano-aluminum particles and the coupling agent ethanol solution is 1-2:40;

[0025] The mass fraction of the coupling agent ethanol solution is 10-12%;

[0026] The coupling agent ethanol solution is a titanate coupling agent ethanol solution.

[0027] As a further technical solution: the mixing mass ratio of the rosin, ethanol, butyl acetate, active nano-aluminum particles, and pre-modified acrylic resin solution is 20-25:30-35:5-8:0.3-0.6:5-10.

[0028] As a further technical solution: the inert gas is neon.

[0029] As a further technical solution, the thixotropic agent is stearic acid;

[0030] The active agent is lactic acid;

[0031] The organic solvent is tributyl citrate;

[0032] The surfactant is sodium dodecylbenzene sulfonate.

[0033] A method for preparing an antioxidant solder paste comprises the following steps:

[0034] (1) Weighing acrylic resin modified rosin, thixotropic agent, activator, organic solvent, and surfactant in parts by weight, and then adding them to a stirring device in sequence, stirring for 30-40 minutes at a stirring temperature of 100-108° C., then adjusting the temperature to 60-70° C., continuing to stir for 20-25 minutes, and standing for 2 hours to obtain a soldering flux;

[0035] (2) Weigh the flux and tin powder by weight, and then add the flux and tin powder into a stirring device and stir them at high speed for 40-50 minutes at a stirring speed of 1000 r / min until they are evenly stirred.

[0036] The solder powder used in the anti-oxidation solder paste prepared in the present invention has a small specific surface area. By introducing modified rosin into the soldering flux, the contact area between the solder powder and the soldering flux can be reduced, thereby reducing the chemical reaction between the solder powder and the soldering flux, making it difficult for the solder powder to agglomerate and adhere in the solder paste, and the solder paste viscosity can be kept suitable for a long time, thereby significantly reducing the sandification phenomenon of the solder paste. The present invention mainly introduces modified rosin into the soldering flux, in order to improve the stability of the solder paste, and by improving the stability of the solder paste, the welding performance of the solder paste is guaranteed.

[0037] The oxidation of tin powder will form an oxide film on the surface. The oxide has a high melting point. Therefore, at the melting temperature of the solder, the oxide is in a solid state and has a very low surface tension, which makes the solder non-wetting and seriously affects the welding performance. Therefore, the present invention modifies the rosin so that the modified rosin can cover the tin powder. By covering the tin powder, the oxidation phenomenon of the tin powder is reduced, so that the prepared solder paste has excellent anti-oxidation performance.

[0038] Compared with the prior art, the present invention provides an anti-oxidation solder paste having the following beneficial effects:

[0039] The anti-oxidation solder paste prepared by the present invention can significantly reduce the oxidation activity of the tin powder by coating the tin powder with modified rosin, thereby significantly improving the welding performance of the tin powder. The solder paste prepared by the present invention exhibits excellent anti-oxidation ability under the accelerated oxidation environment conditions of 45° C., RH 90%, and 48h. DETAILED DESCRIPTION

[0040] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0041] The following are specific embodiments:

[0042] Example 1

[0043] An anti-oxidation solder paste is prepared from the following ingredients by weight: 85 parts of tin powder and 8 parts of soldering flux;

[0044] The soldering flux is made of the following ingredients by weight: 28 parts of acrylic resin modified rosin, 3 parts of thixotropic agent, 1 part of activator, 15 parts of organic solvent and 3 parts of surfactant.

[0045] As a further technical solution, the preparation method of the acrylic resin modified rosin comprises the following steps:

[0046] (1) performing a pre-modification treatment on an acrylic resin to obtain a pre-modified acrylic resin solution;

[0047] (2) uniformly dispersing the nano-aluminum particles into the coupling agent ethanol solution, adjusting the temperature to 40° C., stirring for 1 hour, and then filtering to obtain active nano-aluminum particles;

[0048] (3) In a reaction kettle, rosin is added to ethanol, stirred evenly, and then butyl acetate and active nano-aluminum particles are added, an inert gas is introduced, the air in the reaction kettle is exhausted, and then the temperature is adjusted to 70° C., and after the temperature is kept and stirred for 40 minutes, the pre-modified acrylic resin solution is slowly added dropwise. After the addition is completed, the temperature in the reaction kettle is continued to be adjusted to 60° C., stirred at a speed of 500 r / min for 3 hours, and then the temperature is reduced to 35° C., kept warm for 30 minutes, and then naturally cooled to room temperature, and the material is discharged to obtain a reaction material;

[0049] (4) Purifying the reaction material to obtain acrylic resin modified rosin.

[0050] As a further technical solution, the preparation method of the pre-modified acrylic resin solution is:

[0051] (1) adding butyl acrylate and methyl acrylate to ethanol in sequence and stirring evenly to obtain a mixed solution;

[0052] (2) adding the initiator to deionized water and stirring evenly to prepare an initiator solution;

[0053] (3) adding castor oil and maleic acid to ethanol in sequence, stirring evenly, to prepare a modified liquid;

[0054] (4) Add the mixed solution to the reactor, adjust the temperature to 60°C, keep the temperature, add the modified solution and the initiator solution, stir and react for 2 hours, then cool naturally to room temperature, and discharge the material to obtain the product.

[0055] As a further technical solution: the mixing mass ratio of butyl acrylate, methyl acrylate and ethanol is 1:1:30.

[0056] As a further technical solution, the initiator is ammonium persulfate;

[0057] The mass fraction of the initiator solution is 5%;

[0058] The castor oil, maleic acid and ethanol are mixed in a mass ratio of 3:1:30;

[0059] The mass ratio of the mixed solution, the modified solution and the initiator solution is 20:3:5.

[0060] As a further technical solution, the mixing mass ratio of the nano-aluminum particles and the coupling agent ethanol solution is 1:40;

[0061] The mass fraction of the coupling agent ethanol solution is 10%;

[0062] The coupling agent ethanol solution is a titanate coupling agent ethanol solution.

[0063] As a further technical solution: the mixing mass ratio of the rosin, ethanol, butyl acetate, active nano-aluminum particles, and pre-modified acrylic resin solution is 20:30:5:0.3:5.

[0064] As a further technical solution: the inert gas is neon.

[0065] As a further technical solution, the thixotropic agent is stearic acid;

[0066] The active agent is lactic acid;

[0067] The organic solvent is tributyl citrate;

[0068] The surfactant is sodium dodecylbenzene sulfonate.

[0069] A method for preparing an antioxidant solder paste comprises the following steps:

[0070] (1) Weighing acrylic resin modified rosin, thixotropic agent, activator, organic solvent, and surfactant in parts by weight, and then adding them to a stirring device in sequence and stirring for 30 minutes at a stirring temperature of 100° C., then adjusting the temperature to 60° C., continuing to stir for 20 minutes, and standing for 2 hours to obtain a soldering flux;

[0071] (2) Weigh the flux and tin powder by weight, and then add the flux and tin powder into a stirring device and stir them at high speed for 40 minutes at a stirring speed of 1000 r / min until they are evenly stirred.

[0072] Example 2

[0073] An anti-oxidation solder paste is prepared from the following ingredients by weight: 90 parts of tin powder and 12 parts of flux;

[0074] The soldering flux is made of the following ingredients by weight: 32 parts of acrylic resin modified rosin, 4 parts of thixotropic agent, 1.5 parts of activator, 16 parts of organic solvent and 5 parts of surfactant.

[0075] As a further technical solution, the preparation method of the acrylic resin modified rosin comprises the following steps:

[0076] (1) performing a pre-modification treatment on an acrylic resin to obtain a pre-modified acrylic resin solution;

[0077] (2) uniformly dispersing the nano-aluminum particles into the coupling agent ethanol solution, adjusting the temperature to 45° C., stirring for 1.5 h, and then filtering to obtain active nano-aluminum particles;

[0078] (3) In a reaction kettle, rosin is added to ethanol, stirred evenly, and then butyl acetate and active nano-aluminum particles are added, an inert gas is introduced, the air in the reaction kettle is exhausted, and then the temperature is adjusted to 72° C., and after being kept warm and stirred for 41 minutes, the pre-modified acrylic resin solution is slowly added dropwise. After the addition is completed, the temperature in the reaction kettle is continued to be adjusted to 63° C., stirred at a speed of 520 r / min for 3.4 hours, and then the temperature is reduced to 36° C., kept warm for 35 minutes, and then naturally cooled to room temperature, discharged, and a reaction material is obtained;

[0079] (4) Purifying the reaction material to obtain acrylic resin modified rosin.

[0080] As a further technical solution, the preparation method of the pre-modified acrylic resin solution is:

[0081] (1) adding butyl acrylate and methyl acrylate to ethanol in sequence and stirring evenly to obtain a mixed solution;

[0082] (2) adding the initiator to deionized water and stirring evenly to prepare an initiator solution;

[0083] (3) adding castor oil and maleic acid to ethanol in sequence, stirring evenly, to prepare a modified liquid;

[0084] (4) Add the mixed solution to the reactor, adjust the temperature to 63°C, keep warm, add the modified solution and the initiator solution, stir and react for 2.2 hours, then cool naturally to room temperature, and discharge the material to obtain the product.

[0085] As a further technical solution: the mixing mass ratio of butyl acrylate, methyl acrylate and ethanol is 2:2:30.

[0086] As a further technical solution, the initiator is ammonium persulfate;

[0087] The mass fraction of the initiator solution is 6%;

[0088] The castor oil, maleic acid and ethanol are mixed in a mass ratio of 4:1.6:30;

[0089] The mass ratio of the mixed solution, the modified solution and the initiator solution is 24:4:7.

[0090] As a further technical solution, the mixing mass ratio of the nano-aluminum particles and the coupling agent ethanol solution is 1.5:40;

[0091] The mass fraction of the coupling agent ethanol solution is 11%;

[0092] The coupling agent ethanol solution is a titanate coupling agent ethanol solution.

[0093] As a further technical solution: the mixing mass ratio of the rosin, ethanol, butyl acetate, active nano-aluminum particles, and pre-modified acrylic resin solution is 22:31:6:0.5:7.

[0094] As a further technical solution: the inert gas is neon.

[0095] As a further technical solution, the thixotropic agent is stearic acid;

[0096] The active agent is lactic acid;

[0097] The organic solvent is tributyl citrate;

[0098] The surfactant is sodium dodecylbenzene sulfonate.

[0099] A method for preparing an antioxidant solder paste comprises the following steps:

[0100] (1) Weighing acrylic resin modified rosin, thixotropic agent, activator, organic solvent, and surfactant according to weight, and then adding them into a stirring device in sequence and stirring for 36 minutes at a stirring temperature of 103° C., then adjusting the temperature to 68° C., continuing to stir for 22 minutes, and standing for 2 hours to obtain a soldering flux;

[0101] (2) Weigh the flux and tin powder by weight, and then add the flux and tin powder into a stirring device and stir them at high speed for 42 minutes at a stirring speed of 1000 r / min until they are evenly stirred.

[0102] Example 3

[0103] An anti-oxidation solder paste is prepared from the following ingredients by weight: 88 parts of tin powder and 10 parts of flux;

[0104] The soldering flux is made of the following ingredients by weight: 31 parts of acrylic resin modified rosin, 4 parts of thixotropic agent, 1.5 parts of activator, 16 parts of organic solvent and 5 parts of surfactant.

[0105] As a further technical solution, the preparation method of the acrylic resin modified rosin comprises the following steps:

[0106] (1) performing a pre-modification treatment on an acrylic resin to obtain a pre-modified acrylic resin solution;

[0107] (2) uniformly dispersing the nano-aluminum particles into the coupling agent ethanol solution, adjusting the temperature to 45° C., stirring for 1.5 h, and then filtering to obtain active nano-aluminum particles;

[0108] (3) In a reaction kettle, rosin is added to ethanol, stirred evenly, and then butyl acetate and active nano-aluminum particles are added, an inert gas is introduced, the air in the reaction kettle is exhausted, and then the temperature is adjusted to 72° C., and after being kept warm and stirred for 45 minutes, the pre-modified acrylic resin solution is slowly added dropwise. After the addition is completed, the temperature in the reaction kettle is continued to be adjusted to 62° C., stirred at a speed of 550 r / min for 3.5 hours, and then the temperature is reduced to 36° C., kept warm for 35 minutes, and then naturally cooled to room temperature, and the material is discharged to obtain a reaction material;

[0109] (4) Purifying the reaction material to obtain acrylic resin modified rosin.

[0110] As a further technical solution, the preparation method of the pre-modified acrylic resin solution is:

[0111] (1) adding butyl acrylate and methyl acrylate to ethanol in sequence and stirring evenly to obtain a mixed solution;

[0112] (2) adding the initiator to deionized water and stirring evenly to prepare an initiator solution;

[0113] (3) adding castor oil and maleic acid to ethanol in sequence, stirring evenly, to prepare a modified liquid;

[0114] (4) Add the mixed solution to the reactor, adjust the temperature to 65°C, keep warm, add the modified solution and initiator solution, stir and react for 2.3 hours, then cool naturally to room temperature, and discharge the material to obtain the product.

[0115] As a further technical solution: the mixing mass ratio of butyl acrylate, methyl acrylate and ethanol is 2:2:30.

[0116] As a further technical solution, the initiator is ammonium persulfate;

[0117] The mass fraction of the initiator solution is 6%;

[0118] The castor oil, maleic acid and ethanol are mixed in a mass ratio of 4:1.2:30;

[0119] The mass ratio of the mixed solution, the modified solution and the initiator solution is 22:4:6.

[0120] As a further technical solution, the mixing mass ratio of the nano-aluminum particles and the coupling agent ethanol solution is 1.2:40;

[0121] The mass fraction of the coupling agent ethanol solution is 11%;

[0122] The coupling agent ethanol solution is a titanate coupling agent ethanol solution.

[0123] As a further technical solution: the mixing mass ratio of the rosin, ethanol, butyl acetate, active nano-aluminum particles, and pre-modified acrylic resin solution is 23:32:6:0.5:6.

[0124] As a further technical solution: the inert gas is neon.

[0125] As a further technical solution, the thixotropic agent is stearic acid;

[0126] The active agent is lactic acid;

[0127] The organic solvent is tributyl citrate;

[0128] The surfactant is sodium dodecylbenzene sulfonate.

[0129] A method for preparing an antioxidant solder paste comprises the following steps:

[0130] (1) Weighing acrylic resin modified rosin, thixotropic agent, activator, organic solvent, and surfactant according to weight, and then adding them into a stirring device in sequence and stirring for 35 minutes at a stirring temperature of 105° C., then adjusting the temperature to 66° C., continuing to stir for 22 minutes, and standing for 2 hours to obtain a soldering flux;

[0131] (2) Weigh the flux and tin powder by weight, and then add the flux and tin powder into a stirring device and stir them at high speed for 45 minutes at a stirring speed of 1000 r / min until they are evenly stirred.

[0132] Example 4

[0133] An anti-oxidation solder paste is prepared from the following ingredients by weight: 92 parts of tin powder and 15 parts of soldering flux;

[0134] The soldering flux is made of the following ingredients by weight: 35 parts of acrylic resin modified rosin, 5 parts of thixotropic agent, 2 parts of activator, 20 parts of organic solvent and 6 parts of surfactant.

[0135] As a further technical solution, the preparation method of the acrylic resin modified rosin comprises the following steps:

[0136] (1) performing a pre-modification treatment on an acrylic resin to obtain a pre-modified acrylic resin solution;

[0137] (2) uniformly dispersing the nano-aluminum particles into the coupling agent ethanol solution, adjusting the temperature to 50° C., stirring for 2 h, and then filtering to obtain active nano-aluminum particles;

[0138] (3) In a reaction kettle, rosin is added to ethanol, stirred evenly, and then butyl acetate and active nano-aluminum particles are added, an inert gas is introduced, the air in the reaction kettle is exhausted, and then the temperature is adjusted to 75° C., and after being kept warm and stirred for 50 minutes, the pre-modified acrylic resin solution is slowly added dropwise. After the addition is completed, the temperature in the reaction kettle is continued to be adjusted to 68° C., stirred at a speed of 600 r / min for 4 hours, and then the temperature is reduced to 38° C., kept warm for 40 minutes, and then naturally cooled to room temperature, and the material is discharged to obtain a reaction material;

[0139] (4) Purifying the reaction material to obtain acrylic resin modified rosin.

[0140] As a further technical solution, the preparation method of the pre-modified acrylic resin solution is:

[0141] (1) adding butyl acrylate and methyl acrylate to ethanol in sequence and stirring evenly to obtain a mixed solution;

[0142] (2) adding the initiator to deionized water and stirring evenly to prepare an initiator solution;

[0143] (3) adding castor oil and maleic acid to ethanol in sequence, stirring evenly, to prepare a modified liquid;

[0144] (4) Add the mixed solution to the reactor, adjust the temperature to 70°C, keep the temperature, add the modified solution and the initiator solution, stir and react for 3 hours, then cool naturally to room temperature, and discharge the material to obtain the product.

[0145] As a further technical solution: the mixing mass ratio of butyl acrylate, methyl acrylate and ethanol is 3:3:30.

[0146] As a further technical solution, the initiator is ammonium persulfate;

[0147] The mass fraction of the initiator solution is 8%;

[0148] The castor oil, maleic acid and ethanol are mixed in a mass ratio of 5:2:30;

[0149] The mass ratio of the mixed solution, the modified solution and the initiator solution is 25:5:8.

[0150] As a further technical solution, the mixing mass ratio of the nano-aluminum particles and the coupling agent ethanol solution is 2:40;

[0151] The mass fraction of the coupling agent ethanol solution is 11%;

[0152] The coupling agent ethanol solution is a titanate coupling agent ethanol solution.

[0153] As a further technical solution: the mixing mass ratio of the rosin, ethanol, butyl acetate, active nano-aluminum particles, and pre-modified acrylic resin solution is 25:35:8:0.6:10.

[0154] As a further technical solution: the inert gas is neon.

[0155] As a further technical solution, the thixotropic agent is stearic acid;

[0156] The active agent is lactic acid;

[0157] The organic solvent is tributyl citrate;

[0158] The surfactant is sodium dodecylbenzene sulfonate.

[0159] A method for preparing an antioxidant solder paste comprises the following steps:

[0160] (1) Weighing acrylic resin modified rosin, thixotropic agent, activator, organic solvent, and surfactant according to weight, and then adding them into a stirring device in sequence and stirring for 40 minutes at a stirring temperature of 108° C., then adjusting the temperature to 70° C., continuing to stir for 25 minutes, and standing for 2 hours to obtain a soldering flux;

[0161] (2) Weigh the flux and tin powder by weight, and then add the flux and tin powder into a stirring device and stir them at high speed for 50 minutes at a stirring speed of 1000 r / min until they are evenly stirred.

[0162] Comparative Example 1: The difference from Example 1 is that the rosin is not modified.

[0163] Comparative Example 2: The difference from Example 1 is that no pre-modified acrylic resin solution is added during the rosin modification.

[0164] test:

[0165] The viscosity of the solder paste samples of the examples was tested according to JIS Z 3284;

[0166] Table 1

[0167] Viscosity / Pa·s Example 1 180.5 Example 2 182.3 Example 3 182.9 Example 4 181.4

[0168] It can be seen from Table 1 that the antioxidant solder paste prepared by the present invention has a suitable viscosity.

[0169] The welding performance of the samples of the embodiment and the comparative example was tested according to IPC-A-610E;

[0170] Table 2

[0171] Welding performance Example 1 excellent Example 2 excellent Example 3 excellent Example 4 excellent Comparative Example 1 good Comparative Example 2 good

[0172] It can be seen from Table 2 that the solder paste prepared by the method of the present invention has excellent welding performance.

[0173] The expansion ratios of the embodiments and comparative examples were tested according to JIS Z 3284.

[0174] Table 3

[0175] Expansion rate / % Example 1 83.5 Example 2 82.5 Example 3 82.3 Example 4 83.1 Comparative Example 1 68.5 Comparative Example 2 73.7

[0176] It can be seen from Table 3 that the solder paste prepared by the present invention has excellent expansibility, thereby being able to further improve its welding performance.

[0177] The solder paste prepared by the invention exhibits excellent anti-oxidation ability under the accelerated oxidation environment conditions of 45° C., RH 90%, and 48 hours.

[0178] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. An anti-oxidation solder paste, It is characterized in that The composition is as follows: 85-92 parts of tin powder and 8-15 parts of soldering flux; The soldering flux is made of the following ingredients by weight: 28-35 parts of acrylic resin modified rosin, 3-5 parts of thixotropic agent, 1-2 parts of activator, 15-20 parts of organic solvent, and 3-6 parts of surfactant; The preparation method of the acrylic resin modified rosin comprises the following steps: (1) performing a pre-modification treatment on an acrylic resin to obtain a pre-modified acrylic resin solution; (2) uniformly dispersing the nano-aluminum particles into the coupling agent ethanol solution, adjusting the temperature to 40-50° C., stirring for 1-2 hours, and then filtering to obtain active nano-aluminum particles; (3) In a reaction kettle, rosin is added to ethanol, stirred evenly, and then butyl acetate and active nano-aluminum particles are added, an inert gas is introduced, the air in the reaction kettle is exhausted, and then the temperature is adjusted to 70-75° C., and after being kept warm and stirred for 40-50 minutes, the pre-modified acrylic resin solution is slowly added dropwise. After the addition is completed, the temperature in the reaction kettle is continued to be adjusted to 60-68° C., and stirred at a speed of 500-600 r / min for 3-4 hours, and then the temperature is reduced to 35-38° C., and the temperature is kept warm for 30-40 minutes, and then naturally cooled to room temperature, and the material is discharged to obtain a reaction material; (4) Purifying the reaction material to obtain acrylic resin modified rosin.

2. The anti-oxidation solder paste according to claim 1, It is characterized in that The preparation method of the pre-modified acrylic resin solution is: (1) adding butyl acrylate and methyl acrylate to ethanol in sequence and stirring evenly to obtain a mixed solution; (2) adding the initiator to deionized water and stirring evenly to prepare an initiator solution; (3) adding castor oil and maleic acid to ethanol in sequence, stirring evenly, to prepare a modified liquid; (4) Add the mixed solution to the reactor, adjust the temperature to 60-70°C, keep warm, add the modified solution and the initiator solution, stir and react for 2-3 hours, then cool naturally to room temperature, and discharge the material to obtain the product.

3. The anti-oxidation solder paste according to claim 2, Features: The mixing mass ratio of the butyl acrylate, methyl acrylate and ethanol is 1-3:1-3:

30.

4. The anti-oxidation solder paste according to claim 2, It is characterized in that The initiator is ammonium persulfate; The mass fraction of the initiator solution is 5-8%; The castor oil, maleic acid and ethanol are mixed in a mass ratio of 3-5:1-2:30; The mass ratio of the mixed solution, the modified solution and the initiator solution is 20-25:3-5:5-8.

5. The anti-oxidation solder paste according to claim 1, It is characterized in that The mass ratio of the nano-aluminum particles to the coupling agent ethanol solution is 1-2:40; The mass fraction of the coupling agent ethanol solution is 10-12%; The coupling agent ethanol solution is a titanate coupling agent ethanol solution.

6. The anti-oxidation solder paste according to claim 1, Features: The mixing mass ratio of the rosin, ethanol, butyl acetate, active nano-aluminum particles and pre-modified acrylic resin solution is 20-25:30-35:5-8:0.3-0.6:5-10.

7. The anti-oxidation solder paste according to claim 1, Features: The inert gas is neon.

8. The anti-oxidation solder paste according to claim 1, It is characterized in that The thixotropic agent is stearic acid; The active agent is lactic acid; The organic solvent is tributyl citrate; The surfactant is sodium dodecylbenzene sulfonate.

9. A method for preparing an anti-oxidation solder paste according to any one of claims 1 to 8, It is characterized in that The following steps are involved: (1) Weighing acrylic resin modified rosin, thixotropic agent, activator, organic solvent, and surfactant in parts by weight, and then adding them to a stirring device in sequence, stirring for 30-40 minutes at a stirring temperature of 100-108° C., then adjusting the temperature to 60-70° C., continuing to stir for 20-25 minutes, and standing for 2 hours to obtain a soldering flux; (2) Weigh the flux and tin powder by weight, and then add the flux and tin powder into a stirring device and stir them at high speed for 40-50 minutes at a stirring speed of 1000 r / min until they are evenly stirred.