A flocculant for reducing salt, ash, and coal dust in the return air main roadway water collection pool

By using an inorganic-organic composite flocculant of bentonite and starch modified flocculant, the efficiency and safety problems of existing flocculants in treating coal mine wastewater are solved, and efficient flocculation and degradation of coal powder, clay and salt are achieved. Significantly improve the sewage treatment effect and environmental friendliness.

CN115092998BInactive Publication Date: 2024-10-29XINZHUANG COAL MINE OF QINGYANG XINZHUANG COAL IND CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202210779774.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-04
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In existing sewage treatment, flocculants such as polyaluminium chloride and polyacrylamide have problems such as large dosage, slow settling speed, poor effect on organic matter, threats to human health, difficulty in degradation, and toxic and side effects, making it difficult to effectively treat them. Pollutants such as coal powder, clay and soluble salts in coal mine wastewater.

Method used

Bentonite is used as the silicon source and aluminum source to prepare inorganic polymer flocculant, and the organic polymer flocculant is prepared through graft copolymerization modification of natural polymer starch to form an inorganic-organic composite polymer flocculant, which is combined with silicon-aluminum composite flocculant and The advantage of starch modified flocculant is to prepare a salt-reducing, ash-removing and coal-dust flocculant for the return air alley collection tank through proportional mixing.

Benefits of technology

It achieves efficient flocculation of coal powder, clay, soluble salts and mechanical equipment oil in coal mine sewage, reduces the precipitation of harmful Al3+, improves the degradability and environmental friendliness of the flocculant, and has a stronger adsorption and bridging effect. And its ability to reduce salt and remove oil is better than traditional flocculants.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a salt-reducing, ash-reducing and coal-dust-removing flocculant for a return air lane water collection tank, and belongs to the technical field of sewage treatment. The mass ratio of the raw materials of the flocculant is: 6% to 10% starch, 0.8% to 1.5% hydrogen peroxide, 10% to 18% sodium hydroxide, 4% to 6% cationic polyacrylamide, 2% to 3% acrylonitrile, 13% to 25% bentonite, 3% to 5% dilute sulfuric acid, 8% to 12% anhydrous ethanol, and 24% to 36% deionized water. The flocculant of the present invention has a good flocculation effect on the common heavy metal ions, fly ash, sludge and emulsified oil in the sewage of the return air lane water collection tank through inorganic-organic polymer composite, and reduces the amount of metal ions introduced into the flocculant, is green, environmentally friendly and easy to degrade, has the advantages of both inorganic polymer flocculants and organic polymer flocculants, can effectively treat the sewage of the return air lane water collection tank, and has a strong application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sewage treatment, in particular to a flocculant for reducing salt, ash and coal dust for a return air lane water collection tank. Background Art

[0002] During the coal mining process, due to the mixing of coal powder, clay, and oil used in underground machinery and equipment during the mining process, it is inevitable that the coal mine wastewater will have problems such as suspended matter, turbidity, and emulsified oil exceeding the standard. Due to national requirements and environmental protection considerations, coal mine wastewater must be treated first and the water quality must be qualified before it can be used. As the most commonly used method in water treatment, flocculation is widely used in the field of sewage treatment due to its convenient operation, low cost, and high treatment efficiency. In terms of flocculant selection, the most commonly used ones are inorganic polymer flocculants polyaluminum chloride (PAC) and organic polymer flocculants polyacrylamide (PAM). However, in actual use, the dosage of PAC is large, the sedimentation rate is slow, the sedimentation effect on organic matter is poor, and a large amount of Al will be precipitated during use, which is more harmful to human health. 3+ ; PAM is more expensive and difficult to degrade, and has certain toxic side effects.

[0003] Therefore, the present invention selects low-cost bentonite as both a silicon source and an aluminum source to prepare an inorganic polymer flocculant, selects a widely available natural polymer starch to be modified by graft copolymerization to prepare an organic polymer flocculant, and prepares an inorganic-organic composite polymer flocculant by mixing the two in proportion, aiming to take into account the advantages of the silicon-aluminum composite flocculant in adsorption bridging and the starch-modified flocculant in environmental friendliness, salt reduction, and oil removal, give full play to the synergistic effect of inorganic polymers and organic polymers, and has more advantages than traditional flocculants. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a flocculant for reducing salt, ash and coal dust for the return air lane water collection pool. By utilizing the advantages of the silicon-aluminum composite flocculant and the starch graft copolymer modified flocculant, it can effectively flocculate pollutants such as coal powder, clay, soluble salt and oil used in underground mechanical equipment in mine sewage, which is friendly to the environment. The flocculant can simultaneously achieve the effects of reducing salt, ash and coal dust in coal mine sewage.

[0005] The mass ratio of raw material components of the flocculant is: 6%-10% starch, 0.8%-1.5% hydrogen peroxide, 10%-18% sodium hydroxide, 4%-6% cationic polyacrylamide, 2%-3% acrylonitrile, 13%-25% bentonite, 3%-5% dilute sulfuric acid, 8%-12% anhydrous ethanol and 24%-36% deionized water.

[0006] Wherein, bentonite, sodium hydroxide and dilute sulfuric acid are used to prepare the inorganic polymer solution 1, and starch, hydrogen peroxide, cationic polyacrylamide, acrylonitrile, anhydrous ethanol and deionized water are used to prepare the organic polymer solution 2.

[0007] The inorganic polymer solution 1 and the organic polymer solution 2 are mixed and stirred at a mass ratio of 1:1 to 3:1 to obtain a solution 3, and the solution 3 is dried and ground to obtain a flocculant.

[0008] The above-mentioned preparation process of the inorganic polymer solution 1 is as follows:

[0009] Slowly add 20% to 30% sodium hydroxide solution by mass to the bentonite for leaching, the mass ratio of sodium hydroxide to bentonite is 6:25, stir for 15 to 20 minutes to make it fully react, then add dilute sulfuric acid to adjust the pH of the solution to 2 to 5, mature at room temperature for 30 to 50 minutes, and obtain an inorganic polymer solution 1 as a silicon-aluminum composite flocculant.

[0010] The preparation process of the organic polymer solution 2 is as follows:

[0011] Add starch to the mixture of anhydrous ethanol and deionized water and stir thoroughly for 15 to 20 minutes, and place in a constant temperature water bath at 80°C for 30 minutes;

[0012] Then, adding a sodium hydroxide solution with a mass fraction of 20% to 30% to adjust the pH to 8 to 10 to obtain an alkaline modified starch solution;

[0013] Slowly add cationic polyacrylamide and acrylonitrile mixed solution to the alkaline modified starch solution and react at room temperature for 1 to 2 hours, then add hydrogen peroxide and stir evenly, and continue to react for 2 to 3 hours to obtain organic polymer solution 2 which is starch graft copolymer modified flocculant.

[0014] The drying temperature of solution 3 is 80°C and the drying time is 6 to 8 hours.

[0015] The starch mentioned above includes corn starch, sweet potato starch and potato starch.

[0016] Bentonite includes sodium bentonite and calcium bentonite.

[0017] The beneficial effects of the above technical solution of the present invention are as follows:

[0018] In the above scheme, the low-priced and easily available bentonite is used to provide aluminum source and silicon source at the same time to prepare the silicon-aluminum-based inorganic polymer flocculant, and cationic polyacrylamide and acrylonitrile are used with hydrogen peroxide as an initiator to carry out graft copolymerization on a natural polymer starch containing multiple modifiable materials, and the prepared inorganic polymer flocculant and the organic polymer flocculant are synergistically configured in a certain ratio. The prepared inorganic-organic polymer flocculant has the advantages of silicon-aluminum-based inorganic polymer flocculant in adsorption and bridging, and has the advantages of starch-modified flocculant in environmental friendliness, salt reduction, and oil removal, and at the same time reduces the harmful Al in the flocculant. 3+ The precipitation of iodine improves the biodegradability of the flocculant, which has greater advantages than traditional polymer flocculants. DETAILED DESCRIPTION

[0019] In order to make the technical problems to be solved, technical solutions and advantages of the present invention more clear, they are described in detail below in conjunction with specific embodiments.

[0020] The invention provides a flocculant for reducing salt, ash and coal dust for a return air lane water collection tank.

[0021] The mass ratio of raw material components of the flocculant is: 6%-10% starch, 0.8%-1.5% hydrogen peroxide, 10%-18% sodium hydroxide, 4%-6% cationic polyacrylamide, 2%-3% acrylonitrile, 13%-25% bentonite, 3%-5% dilute sulfuric acid, 8%-12% anhydrous ethanol and 24%-36% deionized water.

[0022] Wherein, bentonite, sodium hydroxide and dilute sulfuric acid are used to prepare the inorganic polymer solution 1, and starch, hydrogen peroxide, cationic polyacrylamide, acrylonitrile, anhydrous ethanol and deionized water are used to prepare the organic polymer solution 2.

[0023] The inorganic polymer solution 1 and the organic polymer solution 2 are mixed and stirred at a mass ratio of 1:1 to 3:1 to obtain a solution 3, and the solution 3 is dried and ground to obtain a flocculant.

[0024] This will be described below with reference to specific embodiments.

[0025] Example 1

[0026] A flocculant for reducing salt, ash and coal dust for return air main lane water collection pool, the main components of which include bentonite, starch, cationic polyacrylamide, acrylonitrile and hydrogen peroxide, and the mass ratio thereof is 1.3:1:0.65:0.35:0.15.

[0027] The flocculant preparation process comprises the following steps:

[0028] (1) Slowly add a sodium hydroxide solution with a mass fraction of 20% to 30% to the bentonite for leaching, the mass ratio of sodium hydroxide to bentonite is 6:25, and stir for 15 to 20 minutes to allow it to react fully. At this time, dilute sulfuric acid is added to adjust the pH of the solution to 2 to 5, and mature at room temperature for 30 to 50 minutes to obtain an inorganic polymer solution 1.

[0029] (2) Add starch to a mixture of anhydrous ethanol and deionized water, wherein the mass ratio of starch, anhydrous ethanol and deionized water is 1:1.2:3.6, stir thoroughly for 15 to 20 minutes, place in a constant temperature water bath at 80°C for 30 minutes, add a 20% to 30% sodium hydroxide solution by mass to adjust the pH to 8 to 10, and obtain an alkaline modified starch solution. Slowly add a mixed solution of cationic polyacrylamide and acrylonitrile to it and react for 1 to 2 hours at room temperature, then add hydrogen peroxide and stir evenly, and continue to react for 2 to 3 hours to obtain an organic polymer solution 2.

[0030] (3) The inorganic polymer solution 1 and the organic polymer solution 2 are prepared together in a ratio of 1:1. The prepared solution 3 is dried at 80° C. for 6 to 8 hours, and then crushed and ground to obtain the flocculant.

[0031] Example 2

[0032] A flocculant for reducing salt, ash and coal dust for return air main lane water collection pool, the main components of which include bentonite, starch, cationic polyacrylamide, acrylonitrile and hydrogen peroxide, and the mass ratio thereof is 2:0.7:0.5:0.2:0.1.

[0033] The flocculant preparation process comprises the following steps:

[0034] (1) Slowly add a sodium hydroxide solution with a mass fraction of 20% to 30% to the bentonite for leaching, the mass ratio of sodium hydroxide to bentonite is 6:25, and stir for 15 to 20 minutes to allow it to react fully. At this time, dilute sulfuric acid is added to adjust the pH of the solution to 2 to 5, and mature at room temperature for 30 to 50 minutes to obtain an inorganic polymer solution 1.

[0035] (2) Add starch to a mixture of anhydrous ethanol and deionized water, wherein the mass ratio of starch, anhydrous ethanol and deionized water is 1:1.2:3.6, stir thoroughly for 15 to 20 minutes, place in a constant temperature water bath at 80°C for 30 minutes, add 20% to 30% sodium hydroxide solution to adjust the pH to 8 to 10, and obtain an alkaline modified starch solution. Slowly add a mixed solution of cationic polyacrylamide and acrylonitrile to it and react for 1 to 2 hours at room temperature, then add hydrogen peroxide and stir evenly, and continue to react for 2 to 3 hours to obtain an organic polymer solution 2.

[0036] (3) The inorganic polymer solution 1 and the organic polymer solution 2 are prepared together in a ratio of 2:1. The prepared solution 3 is dried at 80° C. for 6 to 8 hours, and then crushed and ground to obtain the flocculant.

[0037] Example 3

[0038] A flocculant for reducing salt, ash and coal dust for return air lane water collection pool, the main components of which include bentonite, starch, cationic polyacrylamide, acrylonitrile and hydrogen peroxide, and the mass ratio is 2.5:0.6:0.4:0.2:0.08. The preparation process of the flocculant includes the following steps:

[0039] (1) Slowly add a sodium hydroxide solution with a mass fraction of 20% to 30% to the bentonite for leaching, the mass ratio of sodium hydroxide to bentonite is 6:25, and stir for 15 to 20 minutes to allow it to react fully. At this time, dilute sulfuric acid is added to adjust the pH of the solution to 2 to 5, and mature at room temperature for 30 to 50 minutes to obtain an inorganic polymer solution 1.

[0040] (2) Add starch to a mixture of anhydrous ethanol and deionized water, wherein the mass ratio of starch, anhydrous ethanol and deionized water is 1:1.2:3.6, stir thoroughly for 15 to 20 minutes, place in a constant temperature water bath at 80°C for 30 minutes, add 20% to 30% sodium hydroxide solution to adjust the pH to 8 to 10, and obtain an alkaline modified starch solution. Slowly add a mixed solution of cationic polyacrylamide and acrylonitrile to it and react for 1 to 2 hours at room temperature, then add hydrogen peroxide and stir evenly, and continue to react for 2 to 3 hours to obtain an organic polymer solution 2.

[0041] (3) The inorganic polymer solution 1 and the organic polymer solution 2 are prepared together in a ratio of 3:1. The prepared solution 3 is dried at 80° C. for 6 to 8 hours, and then crushed and ground to obtain the flocculant.

[0042] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A flocculant for reducing salt, ash and coal dust for return air lane water collection tank, characterized in that: The mass ratio of the raw material components is: starch 6% to 10%, hydrogen peroxide 0.8% to 1.5%, sodium hydroxide 10% to 18%, cationic polyacrylamide 4% to 6%, acrylonitrile 2% to 3%, bentonite 13% to 25%, dilute sulfuric acid 3% to 5%, anhydrous ethanol 8% to 12%, and deionized water 24% to 36%; The bentonite, sodium hydroxide and dilute sulfuric acid are used to prepare an inorganic polymer solution 1, and starch, hydrogen peroxide, cationic polyacrylamide, acrylonitrile, anhydrous ethanol and deionized water are used to prepare an organic polymer solution 2; The inorganic polymer solution 1 and the organic polymer solution 2 are mixed and stirred at a mass ratio of 1:1 to 3:1 to obtain a solution 3, and the solution 3 is dried and ground to obtain a flocculant; The preparation process of the inorganic polymer solution 1 is as follows: Slowly add 20% to 30% sodium hydroxide solution to the bentonite for leaching, the mass ratio of sodium hydroxide to bentonite is 6:25, stir for 15 to 20 minutes to make it fully react, then add dilute sulfuric acid to adjust the pH of the solution to 2 to 5, and ripen at room temperature for 30 to 50 minutes to obtain an inorganic polymer solution 1 as a silicon-aluminum composite flocculant; The preparation process of the organic polymer solution 2 is as follows: Add starch to the mixture of anhydrous ethanol and deionized water and stir thoroughly for 15 to 20 minutes, and place in a constant temperature water bath at 80°C for 30 minutes; Then, adding a sodium hydroxide solution with a mass fraction of 20% to 30% to adjust the pH to 8 to 10 to obtain an alkaline modified starch solution; Slowly add cationic polyacrylamide and acrylonitrile mixed solution to the alkaline modified starch solution and react at room temperature for 1 to 2 hours, then add hydrogen peroxide and stir evenly, and continue to react for 2 to 3 hours to obtain organic polymer solution 2 which is starch graft copolymer modified flocculant.

2. The flocculant for reducing salt, ash and coal dust for the return air lane water collection tank according to claim 1 is characterized in that: The drying temperature of the solution 3 is 80° C., and the drying time is 6 to 8 hours.

3. The flocculant for reducing salt, ash and coal dust for the return air lane water collection tank according to claim 1 is characterized in that: The starch includes corn starch, sweet potato starch and potato starch.

4. The flocculant for reducing salt, ash and coal dust for the return air lane water collection tank according to claim 1 is characterized in that: The bentonite includes sodium-based bentonite and calcium-based bentonite.

Citation Information

Patent Citations

  • Natural organic high-molecular flocculant and its preparation method

    CN101007668A

  • High-selectivity flocculating agent for separating hematite and preparation method thereof

    CN101863540A

  • Method of drinking water treatment with natural cationic polymers

    US5543056A