Long balloon for balloon expansion stent system and preparation method thereof

By setting a stable flap structure in the middle of the balloon and controlling the winding conditions, the problem of uneven and scattered flaps of long balloons is solved, achieving stable withdrawal and surface protection of the balloon during surgery, and improving the success of the surgery. Rate.

CN115103703BActive Publication Date: 2024-10-01BIOTYX MEDICAL (SHENZHEN) CO LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202180012385.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-11-02
Filing Date
2021-11-02
Publication Date
2024-10-01
Estimated Expiration
2041-11-02

AI Technical Summary

Technical Problem

In the existing balloon-expandable stent system, the folding wings of the long balloon at the moment of placement or pumping are uneven, resulting in an increase in the inner diameter and resistance of the balloon when withdrawing, affecting the success rate of the operation, and the wings are prone to folding during transportation. Scattered or surface damaged.

Method used

A long balloon for balloon expansion stent system is designed, in which the middle part of the balloon has stable n flaps, n is an integer greater than or equal to 3, and the winding conditions such as temperature, pressure and time are controlled to ensure that the balloon The flaps do not fall apart during long-term placement and transportation, and maintain uniformity and shape stability during expansion and contraction.

Benefits of technology

It achieves uniform contraction of the long balloon's flaps during placement and extraction, reduces resistance during balloon withdrawal, avoids stent displacement and complications, ensures the integrity of the balloon surface, and improves the success of the operation. Rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115103703B_ABST
    Figure CN115103703B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of medical device technology, and specifically relates to a long balloon for a balloon expansion stent system and a preparation method thereof, wherein the middle portion of the long balloon has the same number of flaps as the two ends of the balloon, and the length of the balloon is greater than or equal to 38 mm. On the other hand, the present invention also discloses a preparation method for the long balloon, which is simple and convenient, and can ensure that the prepared long balloon can maintain a stable flap shape whether after a long period of storage, during long-distance transportation, or after multiple expansions and contractions, and its diameter is still maintained within a small range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of medical devices, and in particular relates to a long balloon and a preparation method thereof, and more particularly relates to a long balloon for a balloon expansion stent system and a preparation method thereof. Background Art

[0002] The balloon-expandable stent system is an effective way to treat peripheral vascular diseases such as atherosclerotic narrowing or blockage of lower extremity blood vessels. When the balloon-expandable stent system is implanted in the diseased blood vessel, the stent is expanded by expanding the balloon. The expanded stent makes the diseased blood vessel unobstructed, and the balloon is quickly deflated and withdrawn from the body after decompression. The balloon has a good folding effect. After decompression, the balloon still maintains the initial folding effect, which significantly reduces the diameter and reduces the resistance of the balloon to be withdrawn from the blood vessel, which can effectively improve the success rate of the operation.

[0003] Before the balloon and the stent are pressed and gripped, the balloon needs to be folded so that the balloon diameter reaches a smaller value so that it can be assembled with the stent. However, in actual production, long balloon folds often have uneven shrinkage effects: due to the low pressure generated, the balloon can only be partially folded, so that the two ends of the balloon remain in a folded state, while the folding effect of the middle part disappears, which will cause a flat straight line, C shape or S shape to appear in the middle part of the balloon, thereby greatly increasing the inner diameter and resistance of the balloon when withdrawing, making the balloon have a larger diameter when removed from the body than when entering the body, resulting in difficulty in withdrawal, stent displacement or complications. Therefore, effectively solving the problem of long balloon fold failure has very important application value in clinical surgery.

[0004] Due to the limitation of materials and technology, there are not many reports on the use of long balloons (balloons with a length of more than 38 mm) in balloon expansion stent systems. Some methods for improving the contraction performance of short balloons also have many limitations when applied to long balloons. For example, in patent application CN101808599A, an elastic expansion protection member is used, which expands together with the balloon during expansion, and generates an elastic restoring force during contraction to restore the balloon to the diameter of the balloon before expansion as much as possible. However, this method applied to the balloon expansion stent system will affect the compression and gripping effect of the balloon and the stent. In addition, the general production method of balloons on the market is to first fold the wings of the balloon so that the balloon has a specific number of winglets, and then coil it so that the winglets are tightly rolled together. Since the winglets are not constrained after the winglets are folded and coiled, the winglets will spread out after being placed for a period of time, resulting in an increase in the outer diameter of the balloon. In order to avoid this situation, the general practice is to use a protective sleeve to protect the balloon to prevent the surface of the balloon from being damaged during transportation. For example, patent application CN 110743089 A discloses a balloon protection sleeve, which includes an inner sleeve and an outer sleeve, wherein the inner sleeve is provided with two symmetrical first incisions along its axial direction or the inner sleeve is formed by a belt structure wrapped around the outside of the balloon. This method can protect the balloon folds from falling off and can also protect the balloon surface from damage. However, for a long balloon, it still cannot fundamentally solve the problem of uneven contraction of the balloon folds at the moment of pumping and compression. Summary of the invention

[0005] In order to overcome the defects existing in the above-mentioned prior art, the present invention provides a long balloon for a balloon expandable stent system and a preparation method thereof. The folding wings of the long balloon for the balloon expandable stent system will not fail during long-term placement or at the moment of compression, and the folding wings will shrink evenly. At the same time, the folding wings of the balloon will not fall off and the outer diameter will not increase during transportation, so that the surface of the balloon will not be damaged.

[0006] On one hand, the present invention proposes a long balloon for a balloon expandable stent system, the balloon having a proximal end, a distal end opposite to the proximal end, and a middle portion between the proximal end and the distal end, wherein the middle portion of the balloon has stable n flaps, wherein n is an integer greater than or equal to 3. Preferably, the number of flaps in the middle portion of the balloon is 3-12, and further preferably, the number of flaps in the middle portion of the balloon is 3-8. In some embodiments, the number n of flaps is 4, in other embodiments, the number n of flaps is 5, and in other embodiments, the value of n is 10, and in some other embodiments, the number of flaps is 7.

[0007] The "stable" mentioned in the present invention means that regardless of whether it is placed for a long time, transported in a bumpy manner, or repeatedly expanded and contracted, all parameters of the shape of the middle part of the balloon are stable, including the depth, width, and angle between adjacent folds, which are basically stable with a fluctuation range of less than 20%, that is, the n folds are kept unchanged, and at the same time, the depth, width, and angle between adjacent folds of each fold fluctuate very little, not exceeding 20%, and further within 15%, or even within 10%.

[0008] The balloon provided by the present invention is a long balloon with a length of more than 38 mm; further, the length of the balloon provided by the present invention is 38 mm-300 mm; further, the length of the balloon provided by the present invention can be a value of an interval composed of any two values ​​in the above interval, for example, the length of the long balloon provided by the present invention can be 50 mm-117 mm, or 118 mm-300 mm, or 73 mm-289 mm, and so on. In some embodiments of the present invention, the length of the balloon is 38 mm, while in other embodiments, the length of the balloon is 50 mm, 60 mm, 70 mm, 80 mm, 90 mm, 100 mm, 118 mm, 130 mm, 140 mm, 150 mm, 170 mm, 190 mm, 210 mm, 230 mm, 250 mm, 270 mm, 285 mm, 300 mm, etc., any value in the interval of 38 mm-300 mm.

[0009] The diameter R of the proximal end, the distal end opposite to the proximal end and the middle part between the proximal end and the distal end provided by the present invention is less than , and the diameter fluctuation range of the balloon at the three parts is within 15%; in the present invention, the fluctuation range of the balloon diameter between the proximal end, distal end and middle part of the balloon can be any value within the above value range, or it can be variable. For example, in some embodiments, the diameter fluctuation range of the balloon at the three parts is within 10%; in other embodiments, the diameter fluctuation range of the balloon at the three parts can be within 7.5%; in some other embodiments, the diameter fluctuation range of the balloon at the three parts can be within 5%. At the same time, the diameter fluctuation range between the middle and proximal end of the balloon, and between the middle and distal ends of the balloon can be different, such as the diameter fluctuation between the middle and proximal end of the balloon is 3.5%, and the diameter fluctuation between the middle and distal ends of the balloon is 2.3%, and so on.

[0010] The diameter R of the proximal end of the long balloon provided by the present invention is 1 ≤ , the diameter R of the distal end opposite to the proximal end 2 ≤ , the diameter R of the middle part between the proximal end and the distal end 3 ≤ , and the diameter fluctuation range of the long balloons in the three parts is within 15%.

[0011] The proximal end, distal end and middle part of the balloon provided by the present invention have the same number of flaps. In some embodiments, the proximal end, distal end and middle part of the balloon have three flaps, in other embodiments, the number of the flaps of the balloon is six, and in other embodiments, the number of the flaps of the balloon is eight.

[0012] The uniformity and uniformity of the balloon fold provided by the present invention can reach more than 80% after multiple expansions and contractions, and further, can reach more than 85%; further, the uniformity and uniformity of the balloon fold can reach more than 90% after multiple expansions and contractions. Multiple expansions refer to 2-10 expansions, further to 2-8 expansions, and further to 2-6 expansions. The uniformity in the present invention means that after multiple expansions and contractions, the shape and diameter of the middle, proximal and distal ends of the balloon are uniform; the uniformity in the present invention means that the shape and diameter after each expansion and contraction are uniform with the next expansion and contraction, and there is basically no significant change, and the maximum amplitude of the change will not exceed 20%, that is, the diameter of the balloon in the two contracted states before expansion and after multiple expansions and contractions (R 扩张后 -R 扩张前 ) / R 扩张前 ≤20%, the change here also refers to the dispersion rate, that is, the dispersion rate = (R 扩张后 -R 扩张前 ) / R 扩张前 ≤20%.

[0013] In the balloon provided by the present invention, the angles formed between each two adjacent flaps may be equal or unequal. When the angles formed between the two adjacent flaps are unequal, the fluctuation range of the two adjacent angles is within 20%, further, the fluctuation range of the two adjacent angles is within 13%, and further, the fluctuation range of the two adjacent angles is within 8%. That is, when a certain angle is 60°, the size of the adjacent angles may fluctuate between 48-72°, may fluctuate between 52.2°-67.8°, and may fluctuate between 55.2°-64.8°, but the shapes of the middle, proximal and distal ends of the balloon are still uniform.

[0014] The material of the balloon provided in the present invention is mainly selected from some flexible or soft materials, including but not limited to nylon, polyetheramide (Pebax), etc.

[0015] The above technical solution provided by the present invention is mainly for balloons with a length greater than or equal to 38 mm. When the balloon length is 38 mm or more, the flaps in the middle of the balloon are very likely to disappear during placement or use. Therefore, the present invention provides a method for ensuring that the middle of a long balloon has flaps that are substantially consistent with the flaps at both ends of the balloon (uniformity and uniformity ≥ 80%) for a long time. That is, the present invention also provides a method for preparing the above balloon, comprising the following steps:

[0016] Folding the balloon into n flaps, wherein n is an integer greater than or equal to 3;

[0017] The balloon folded into flaps is rolled up.

[0018] In the preparation method of the balloon provided by the present invention, the winding conditions of the balloon are: the winding temperature T is 25~90°C, the winding pressure P is 10 psi~200 psi, and the winding time t is 10 s~90 s; further, the winding temperature T is 25~90°C, the winding pressure P is 51 psi~200 psi, and the winding time t is 10 s~90 s; further, the winding temperature T is 25~90°C, the winding pressure P is 51 psi~200 psi, and the winding time t is 10 s~90 s. The above three parameters can be combined at will and are not limited to one or several values. For example, in some embodiments, the conditions for balloon winding are that the winding temperature T is 75°C, the winding pressure P is 100 psi, and the winding time t is 30 s; while in some other embodiments, the balloon winding temperature T is 45°C, the winding pressure P is 150 psi, and the winding time t is 30 s, etc. In the present invention, by controlling the number of windings, the winding temperature, the winding pressure, and the winding time, and making the four parameters effectively matched at the same time, the balloon crease effect and the thermal setting effect of the flap position can be improved, the stress of the balloon fold part can be eliminated, and the flap contraction size can be smaller when the balloon is expanded and then contracted, and the balloon contraction is more compact.

[0019] In the preparation method of the balloon provided by the present invention, the winding can cover more than 80% of the area of ​​the entire balloon, and the covered area or uncovered area has a certain degree of arbitrariness. The uncovered area can be a continuous section or multiple sections, including 2 sections, 3 sections, 4 sections, 5 sections, etc., and each section can be uniform, equal in length, or unequal in length. For example, in some embodiments, 10% of the area at each of the two ends of the balloon is not wound; in other embodiments, 10% of the area at each of the two ends adjacent to the left and right near the middle is not wound; in other embodiments, 15% of the proximal end of the balloon is not wound, 5% of the distal end is not wound, and the proximal unwound area is divided into 3 sections.

[0020] In the method for preparing the balloon provided by the present invention, the sum of the products of the winding parameters of the middle part of the balloon is greater than the sum of the products of the winding parameters of the two ends, wherein the winding parameters mainly include the winding pressure P, the winding temperature T, the number of windings N, and the winding time t. That is, ∑N 中部 *P 中部 *T 中部 *t 中部 >∑N 近端 *P 近端 *T 近端 *t 近端 , and / or ∑N 中部 *P 中部 *T 中部 *t 中部 >∑N 远端 *P 远端 *T 远端 *t 远端 ,in:

[0021] N 中部 is the number of times the balloon is wound in the middle, N 近端 N is the number of times the proximal end of the balloon is wound. 远端 is the number of times the distal end of the balloon is wound. Other parameters can also be deduced by analogy, such as P 中部 Represents the winding pressure borne / applied to the middle of the balloon during a single winding, T 近端 Represents the winding temperature borne / applied to the proximal end of a single winding balloon; N 中部 ≥1, N 近端 ≥1, N 远端 ≥1. In the present invention, during the winding process of the balloon, in some embodiments, when the temperatures used at the middle, proximal and distal ends of the balloon are equal, the above formula can also be equivalent to ∑N 中部 *P 中部 *t 中部 >∑N 近端 *P 近端 *t 近端 , and / or ∑N 中部 *P 中部 *t 中部 >∑N 远端 *P 远端 *t 远端 .

[0022] It should be noted that the winding of the present invention can be multiple windings, the number of windings is at least twice, can be 2-10 times, and further can be 2-5 times, and the winding pressure, winding time and winding temperature set for each winding can be different. When the winding pressure, winding time and winding temperature of each winding are the same during multiple windings, the summation symbol "∑" may not appear in the above formula, that is, it can be directly N 中部 *P中部 *T 中部 *t 中部 >N 近端 *P 近端 *T 近端 *t 近端 , and / or N 中部 *P 中部 *T 中部 *t 中部 >N 远端 *P 远端 *T 远端 *t 远端 ; When there are two or more values ​​for any of the three parameters, namely, winding pressure, winding time and winding temperature, during multiple winding processes, the above formula should be in the form of summation, such as ∑N 中部 *P 中部 *T 中部 *t 中部 >∑N 近端 *P 近端 *T 近端 *t 近端 , and / or ∑N 中部 *P 中部 *T 中部 *t 中部 >∑N 远端 *P 远端 *T 远端 *t 远端 .

[0023] In the above technical solution of the present invention, at least a part of the middle area of ​​the balloon is wound more times than the distal and proximal areas, that is, N 中部 >N 近端 ≥N 远端 .

[0024] In some technical solutions of the present invention, the total pressure on the middle part of the balloon during winding is greater than the total winding pressure on the proximal and distal ends, that is, P 中部总 >P 近端总 ≥P 远端总 , the pressure on the middle part can be greater than the pressure on the proximal and distal ends in a single time, or the sum of the pressures on the middle part can be greater than the sum of the pressures on the proximal and distal ends in multiple times. For example, the pressures on the three parts of the balloon in the first time are P 中部1 =25psi, P 近端1 =17psi, P 远端1 =26psi, the pressures on the three parts of the second balloon are P 中部2 =45psi, P 近端2 =36 psi, P 远端2 =32psi, then P 中部总 =70psi, P近端总 =53psi, P 远端总 =58psi. In some embodiments of the present invention, the total pressure P in the middle of the balloon is 中部总 Greater than or equal to 51psi, P 中部总 ≥51Psi, further, P 中部总 ≥60Psi, or P 中部总 ≥70Psi; In other embodiments, the total pressure of each part of the balloon is greater than 51Psi, that is, P 总 ≥51Psi, that is, the total pressure of the middle part, the proximal end and the distal end of the balloon is greater than 51Psi in one or more times; and in some other embodiments, P 总 ≥60Psi.

[0025] It should be noted that P in the present invention 总 P 中部总 , P 近端总 and P 远端总 The general term for 总 Represents t 中部总 ,t 近端总 and t 远端总 , such as P 总 ≥51Psi, means P 中部总 , P 近端总 and P 远端总 Both are greater than or equal to 51Psi.

[0026] In the above technical solution of the present invention, when the balloon is wound, the total winding time of the middle part is greater than the total winding time of the proximal and distal ends, that is, t 中部总 >t 近端总 ≥t 远端总 The total winding time can be the time of a single winding, or the sum of multiple winding times, that is, the total time of multiple windings.

[0027] It should be noted that in the present invention, if the entire area of ​​any area in the proximal, distal or middle area of ​​the balloon is wound, the number of times the area is wound is 1. If only a part of the area is wound, the number of times the wound area is wound is the proportion of the wound area to the entire area. The area is wrapped, then the number of wraps N 中部 for If the proximal end of the balloon The area is wrapped, then the number of wraps N 近端 for If the entire area of ​​the distal end of the balloon is rolled once, there is also The region of the coil is wrapped a second time, then the distal region is wrapped times, and so on.

[0028] In the above technical solution of the present invention, when the balloon is wound, all the X 1 >X 2 ≥X 3 Inequality of type X>X 2 =X 3 , and can also be X 1 >X 2 >X 3 .

[0029] In some embodiments of the present invention, when the winding is performed multiple times, the winding can be performed from the proximal end of the balloon to the distal end, or from the distal end to the proximal end. The multiple windings can be performed from different ends or from the same end. When the winding is performed from different ends, the multiple windings must satisfy that an area greater than 1 / 4 of the middle of the balloon is wound more than or equal to 2 times. When the winding is started from the same end, at least one winding is performed on the entire balloon or an area greater than 80% of the entire balloon, and at the same time, the middle of the balloon is wound. In some embodiments of the present invention, the number of windings in the middle area of ​​the balloon is greater than that at the two ends, and other parameters are the same, that is, in P 中部 =P 近端 =P 远端 , t 中部 =t 近端 =t 远端 , T 中部 =T 近端 =T 远端 When N 中部 >N 近端 , and / or N 中部 >N 远端 Preferably, the number of windings in the middle is at least greater than the number of windings at either end. , that is, N 中部 ≥ N 近端 , or N 中部 ≥ N 远端 , better, N middle ≥ N proximal, and N mid ≥ N distal end. In the present invention, the middle part is wound more times than the two ends, or the pressure and winding time of the middle part are greater than the pressure or winding time of the proximal or distal ends. By controlling the above three parameters, the middle part of the long balloon can maintain a long-term stable folded wing shape. On the one hand, it can avoid uneven shrinkage of the middle part of the balloon after pressure relief and a flat shape, thereby greatly reducing the inner diameter and resistance of the balloon when it is withdrawn during surgery, and avoiding displacement of the stent or damage to the inner wall coating of the stent when the balloon is withdrawn; on the other hand, it can reduce the number of folding times / pressure / folding time of the two ends of the balloon, and avoid damage to the two ends of the balloon.

[0030] In other embodiments of the present invention, the middle region of the balloon is wound the same number of times as the proximal and distal ends of the balloon, and the temperature and time of the winding are the same, and the pressure applied to the middle region is greater than the pressure applied to either the proximal or distal ends, that is, t 中部 =t 近端 =t 远端 , T 中部 =T 近端 =T 远端 , N 中部 =N 近端 =N 远端 , but P 中部 >P 近端 , and / or P 中部 >P 远端 , preferably, P 中部 ≥ P 近端 , or P 中部 ≥ P 近端 ; better, P 中部 ≥ P 近端 , and P 中部 ≥ P 近端 .

[0031] In some other embodiments of the present invention, the winding pressure, winding times and winding temperature of the middle part of the balloon are the same, except that the winding time of the middle part is longer than the winding time of either the proximal end or the distal end of the balloon, that is, T 中部 =T 近端 =T 远端 , N 中部 =N 近端 =N 远端 , P 中部 =P 近端 =P 远端 , but t 中部 >t 近端 , and / or t 中部 >t 远端Preferably, t 中部 > t 近端 , or t 中部 > t 远端 More preferably, t middle> t proximal, or t middle> t far end.

[0032] It should be noted that in the present invention, as long as ∑N 中部 *P 中部 *T 中部 *t 中部 >∑N 近端 *P 近端 *T 近端 *t 近端 , and / or ∑N 中部 *P 中部 *T 中部 *t 中部 >∑N 远端 *P 远端 *T 远端 *t 远端 That is, it is not limited to the above cases. For example, when N 中部 >N 近端 ≥N 远端 When the winding temperature, pressure and time of the middle, proximal and distal ends of the balloon are not necessarily the same, as long as the other parameters can ensure the final ∑N 中部 *P 中部 *T 中部 *t 中部 >∑N 近端 *P 近端 *T 近端 *t 近端 , and / or ∑N 中部 *P 中部 *T 中部 *t 中部 >∑N 远端 *P 远端 *T 远端 *t 远端 That is, better, other parameters can ensure the final ∑N 中部 *P 中部 *T 中部 *t 中部 > ∑N 近端 *P 近端 *T 近端 *t 近端 , and / or ∑N 中部 *P 中部 *T 中部 *t中部 > ∑N 远端 *P 远端 *T 远端 *t 远端 That's it.

[0033] In some other embodiments, the winding temperature, winding time, winding pressure and winding time applied to the middle part of the balloon, the proximal end of the balloon and the distal end of the balloon are all different. ≥ , and / or ≥ That's it.

[0034] In the present invention, "and / or" means that in some embodiments, the meaning of "and" is taken, that is, both the preceding and following conditions must be met, while in other embodiments, the meaning of "or" is taken, and only one of the conditions needs to be met. ≥ , and / or ≥ In some embodiments, when the meaning of "and" is taken, it satisfies ≥ At the same time, we also need to meet ≥ , while in other embodiments, the meaning of "or" is taken, that is, as long as " ≥ , ≥ "Any of these two conditions will do.

[0035] In the above technical solution provided by the present invention, before folding the balloon, the balloon is also preheated at 25°C to 90°C for 15 min to 30 min. The role of preheating is, on the one hand, to make the balloon evenly heated before folding, so as to ensure the uniformity of the folding wings of various parts of the balloon, and on the other hand, to ensure that the balloon is heated to a certain temperature before folding the wings, so as to ensure a better effect of folding the wings.

[0036] In the above technical solutions provided by the present invention, the balloons in the present invention are all made of polymer materials, and before the balloon is preheated, the surface of the balloon is also subjected to plasma treatment. When the present invention performs plasma treatment on the surface of the balloon, the physical and chemical properties of the balloon polymer surface will change, such as the intensification of molecular motion and the adjustment of the position of the molecular chain, the breaking of chemical bonds, the increase in the temperature of the material surface, etc. After the plasma treatment, the roughness of the balloon surface increases and the surface properties change. Therefore, by performing plasma treatment on the balloon after the folded wings, the friction and adhesion between the winglets formed after the folded wings of the balloon can be increased, thereby enhancing the interaction force between the winglets, and further improving the effect of the balloon folded wing winding.

[0037] In the above technical solution provided by the present invention, balloon folding includes the following steps:

[0038] 1) applying a pressure of 10 psi to 100 psi to the balloon at 25° C. to fill the balloon;

[0039] 2) Fold the inflated balloon into folded wings, with the folding time ranging from 10 s to 90 s;

[0040] Negative pressure is applied to the folded balloon for 10 s to 90 s. For ease of description, the terms "proximal end" and "distal end" are used in the present invention, where "proximal end" refers to the end close to the operator and "distal end" refers to the end far from the operator.

[0041] The values ​​of the interval range involved in the present invention are not limited to the provided interval range, but should be a new interval value composed of any two values ​​in the interval. For example, the winding pressure of the balloon described in the present invention is 10 psi~200 psi, wherein the winding pressure of the balloon is not limited to the interval range of 10 psi~200 psi, and can be a new interval composed of any two values ​​between 191 integer values ​​between 10-200, or a new interval composed of any two values ​​among countless non-integer values ​​between 10-200, such as 120 psi-180psi, or 135.2 psi-193.75 psi, and so on.

[0042] It should be understood that the terms used herein are only for the purpose of describing specific example embodiments and are not intended to be limiting. Unless the context clearly indicates otherwise, the singular forms "one", "an" and "said" as used herein may also be meant to include plural forms. The terms "include", "comprise", "contain", and "have" are inclusive, and therefore specify the existence of stated features, steps, operations, elements and / or parts, but do not exclude the existence or addition of one or more other features, steps, operations, elements, parts, and / or combinations thereof. The method steps, processes, and operations described herein are not interpreted as necessarily requiring them to be performed in the specific order described or illustrated, unless the execution order is clearly indicated. It should also be understood that additional or alternative steps may be used.

[0043] The balloon prepared by the present invention can shrink well after use, ensuring that the length of the columnar object formed after shrinkage in any diameter direction is much smaller than the diameter of the stent and the blood vessel. On the one hand, the balloon will not touch the inner wall or outer edge of the stent, and will not cause the stent to shift during the dragging of the balloon. At the same time, the drugs, polymers, etc. on the outside of the stent will not be scraped off, thereby causing problems such as hyperplasia of surrounding blood vessels. In addition, the balloon will not touch the blood vessel wall, thereby scratching the blood vessel and causing damage. The folded wings on the surface of the balloon prepared by the present invention will not spread out after being placed for a long time, and the original shape will be maintained. The balloon prepared by the present invention can also be well restored after being opened multiple times, and the wing depth change or dispersion rate will not be greater than 20%.

[0044] At present, most of the balloons made of soft or flexible materials have good resilience. After the balloon is prepared and placed for a period of time, different positions of the balloon will rebound to different degrees, so that the previously prepared balloon with multiple folded wings will at least partially recover to the state without folded wings, so that the diameter of the balloon that has recovered to the state without folded wings is significantly increased, which leads to adverse effects such as stent displacement during the withdrawal process. In particular, the longer the balloon is, the greater the extent to which the folded wings in the middle of the balloon disappear, and the greater the probability of causing adverse consequences during the operation. For example, the thermoplastic semi-crystalline material Pebax has a performance between thermoplastic elastomers and rubber bodies, and has good rebound and elastic recovery capabilities. When the balloon with folded wings is placed in the air by the conventional method, the middle of the balloon will slowly rebound to recover part of the deformation. After being prepared by the method of the present invention, the balloon made of Pebax material will not disappear in the middle folded wings during long-term placement or transportation or during multiple expansion and contraction processes, and the folded wings in the middle can still maintain more than 80% of the original shape. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present invention. Moreover, the same reference numerals are used throughout the accompanying drawings to represent the same components. Among them:

[0046] Figure 1 A comparison diagram of the balloon prepared in Example 1 and the balloon prepared in Comparative Example 1;

[0047] Figure 2 A comparison diagram of the balloon prepared in Example 1 and the balloon prepared in Comparative Example 2;

[0048] Figure 3 It is a cross-sectional comparison diagram of the balloon prepared in Example 1 and the balloon prepared in Comparative Example 2. DETAILED DESCRIPTION

[0049] The exemplary embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. Although the exemplary embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to fully convey the scope of the present invention to those skilled in the art.

[0050] Conformity test method:

[0051] The measurement of the balloon shape retention rate in the present invention is mainly to measure the diameters of the proximal, middle and distal ends of the balloon just prepared in a contracted state, the balloon after expansion, and the balloon in a contracted state after multiple expansions and contractions or long-term placement by a non-contact MicroVU measuring instrument, and obtain the result after a series of data processing and calculation. The specific operation steps are as follows:

[0052] First, measure the diameters R of the middle, proximal and distal ends of the newly prepared balloon in a contracted state. 1中部 , R 1近端 , R 1远端 and the diameters R of the middle, proximal, and distal ends of the balloon after the first dilation 中部 , R 近端 , R 远端 , respectively divide the former by the latter value to calculate the corresponding contraction rate Y of the balloon 中部 , Y 近端 , Y 远端 The value of the balloon is then measured, and the diameter R of the balloon after multiple expansions and contractions or after long-term placement in a contracted state is measured. ’ 1中部 , R ’ 1近端 , R ’1远端 , divided by the corresponding diameters R of the middle, proximal and distal ends of the balloon after the first dilation 中部 , R 近端 , R 远端 , calculate the corresponding shrinkage rate Y ’ 中部 , Y ’ 近端 , Y ’ 远端 The shape retention rate Z can be obtained by the ratio of the sum of the shrinkage rates of each part calculated twice before and after. The specific formula is as follows:

[0053] Z= = x 100%.

[0054] Balloon surface plasma parameters:

[0055]

[0056] Unless otherwise specified, the plasma process parameters of the present invention adopt the process parameters described in the above table.

[0057] Example 1

[0058] The preparation method of the balloon of this embodiment uses a long Pebax balloon of 5.0 mm x 150 mm, and the preparation method comprises the following steps:

[0059] Plasma treatment of the balloon surface (upper limit parameter);

[0060] Turn on the balloon folding machine and preheat it for 15-30 minutes to 40°C;

[0061] Apply 15 psi of pressure to the balloon to inflate it, then fold the balloon into flaps for 50 seconds, and then apply negative pressure to the balloon for 10 seconds;

[0062] The balloon was wound once, the winding temperature was set to 65°C, the curling aperture was set to 0.033 inches, the distal end, middle end, and proximal end of the balloon were sequentially sent into the winding mold to start winding, the winding pressure was set to 60 psi, 120 psi, and 60 psi, respectively, and the winding time was set to 15 s to complete the wing folding.

[0063] After the first expansion and contraction of the sample, the distal, middle and proximal ends of the balloon maintained three-flap folds, and the angle between adjacent flaps was tested to be about 120°; after 6 contractions, the distal, middle and proximal ends of the balloon maintained a 3-flap effect; after 6 expansions and contractions, the shape retention rate test result reached 82.7%, and after 18 months of placement, the shape retention rate test result reached 82.1% after 5 expansions and contractions.

[0064] Example 2

[0065] The preparation method of the balloon of this embodiment uses a long balloon made of Pebax material with a size of 4.0 mm x 150 mm. The preparation method includes the following steps:

[0066] Plasma treatment is performed on the surface of the balloon;

[0067] Turn on the balloon folding machine and preheat it for 15-30 minutes to 90°C;

[0068] Apply 10 psi of pressure to the balloon to inflate it, then fold the balloon into flaps for 10 seconds, and then apply negative pressure to the balloon for 10 seconds;

[0069] The balloon was wound twice, the winding temperature was set to 90°C, the winding pressure was set to 10psi, the curling aperture was set to 0.033inch, two-thirds of the length of the balloon was sent into the winding mold for winding, and the first winding was completed after the winding time was set to 10s. Then the entire balloon was sent into the winding mold for winding, and the second winding was completed after the winding time was set to 10s. After taking out, the balloon was obtained.

[0070] According to this embodiment, samples were made to test the following properties:

[0071] After the first expansion and contraction of the sample, the distal, middle and proximal ends of the balloon maintained three-flap folds, and the angle between adjacent flaps tested was about 120°; after the fourth contraction, the distal, middle and proximal ends of the balloon maintained a three-flap effect, and the angle between adjacent flaps tested was about 120°; after four expansions and contractions, the shape retention rate test result reached 81.5%, and after four expansions and contractions after placement for 6 months, the shape retention rate test result reached 81.0%.

[0072] Example 3

[0073] The preparation method of the balloon of this embodiment uses a long balloon made of Pebax material of 8.0 mm x 118 mm, and the preparation method comprises the following steps: opening the balloon folding machine, preheating for 15 min to 30 min, and raising the temperature to 25° C.;

[0074] Plasma treatment is performed on the surface of the balloon;

[0075] Apply 90 psi of pressure to the balloon to inflate it, then fold the balloon into flaps for 90 seconds, and then apply negative pressure to the balloon for 10 seconds;

[0076] The balloon was wound twice, the winding temperature was set to 25°C, the winding pressure was set to 200psi, the curling aperture was set to 0.033inch, two-thirds of the length of the balloon was sent into the winding mold for winding, and the first winding was completed after the winding time was set to 90s. Then the entire balloon was sent into the winding mold for winding, and the second winding was completed after the winding time was set to 90s. After taking out, the balloon was obtained.

[0077] The balloon has three flaps, and the angle between adjacent flaps is about 120°. After contraction for 6 times, the three-flap effect is maintained. After 6 expansion and contraction times, the shape retention rate test result reaches 90%.

[0078] After the first expansion and contraction of the sample, the distal, middle and proximal ends of the balloon maintained three-flap folds, and the angle between adjacent flaps was tested to be about 120°; after 10 further contractions, the distal, middle and proximal ends of the balloon maintained a three-flap effect; after 10 expansions and contractions, the test result reached 97.1%, and after 8 months of placement, the balloon expanded and contracted 10 times and the shape retention rate test result reached 96.3%.

[0079] Example 4

[0080] The preparation method of the balloon of this embodiment uses a long balloon made of nylon material with a size of 8.0 mm x 118 mm. The preparation method comprises the following steps:

[0081] Plasma treatment is performed on the surface of the balloon;

[0082] Turn on the balloon folding machine and preheat it for 15-30 minutes to 40°C;

[0083] Apply 15 psi of pressure to the balloon to inflate it, then fold the balloon into flaps for 25 seconds, and then apply negative pressure to the balloon for 10 seconds;

[0084] The balloon was wound twice, the winding temperature was set to 90°C, the winding pressure was set to 80psi, the curling aperture was set to 0.033inch, two-thirds of the length near the proximal end of the balloon was fed into the winding mold to start winding, and the first winding was completed after the winding time was set to 15s. Then, two-thirds of the length near the distal end of the balloon was fed into the winding mold to start winding, and the second winding was completed after the winding time was set to 15s. After taking out, the balloon was obtained.

[0085] After the first expansion and contraction of the sample, the distal, middle and proximal ends of the balloon maintained three-flap folds, and the angle between adjacent flaps was tested to be about 120°; after 8 contractions, the distal, middle and proximal ends of the balloon maintained a three-flap effect; the shape retention rate test result after 8 expansions and contractions reached 86.2%, and the shape retention rate test result after 8 months of placement and 8 expansions and contractions reached 85.7%.

[0086] Example 5

[0087] The preparation method of the balloon of this embodiment uses a long balloon made of Pebax material with a size of 4.0 mm x 118 mm. The preparation method includes the following steps:

[0088] Plasma treatment is performed on the surface of the balloon;

[0089] Turn on the balloon folding machine and preheat it for 15-30 minutes to 40°C;

[0090] Apply 15 psi of pressure to the balloon to inflate it, then fold the balloon into flaps for 25 seconds, and then apply negative pressure to the balloon for 10 seconds;

[0091] The balloon was wound twice, the winding temperature was set to 65°C, the winding pressure was set to 60psi, the curling aperture was set to 0.033inch, two-thirds of the length near the proximal end of the balloon was fed into the winding mold to start winding, and the first winding was completed after the winding time was set to 30s. Then, two-thirds of the length near the distal end of the balloon was fed into the winding mold to start winding, and the second winding was completed after the winding time was set to 30s. After taking out, the balloon was obtained.

[0092] According to this embodiment, samples were made to test the following properties:

[0093] After the first expansion of the sample, the distal, middle and proximal ends of the balloon maintained three-flap folds, and the angle between adjacent flaps was tested to be 120°; after 6 more contractions, the distal, middle and proximal ends maintained three-flap folds, and the angle between adjacent flaps was tested to be 120°; after 6 expansions and contractions, the shape retention rate test result reached 91.6%; after 3 months of placement and 6 expansions and contractions, the shape retention rate test result reached 92.3%.

[0094] Example 6

[0095] The preparation method of the balloon of this embodiment uses a long Pebax balloon of 7.0 mm x 118 mm, and the preparation method comprises the following steps:

[0096] Plasma treatment of the balloon surface (lower limit parameter);

[0097] Turn on the balloon folding machine and preheat it for 15-30 minutes to 40°C;

[0098] Apply 15 psi of pressure to the balloon to inflate it, then fold the balloon into flaps for 50 seconds, and then apply negative pressure to the balloon for 10 seconds;

[0099] The balloon was wound once, the winding temperature was set to 70°C, the curling aperture was set to 0.033 inches, the distal end, middle end and proximal end of the balloon were sequentially sent into the winding mold to start winding, the winding pressure was set to 100 psi, 100 psi and 100 psi, the distal end, middle end and proximal end winding time were set to 15 s, 30 s and 15 s respectively, and the wing folding was completed.

[0100] After the first expansion and contraction of the sample, the distal, middle and proximal ends of the balloon maintained three-petal folds, and the angle between adjacent winglets was tested to be about 120°; after seven contractions, the distal, middle and proximal ends of the balloon maintained a three-petal effect; after seven expansions and contractions, the shape retention rate test result reached 91.2%, and after a long-distance transportation of 1,200 kilometers, the shape retention rate of the balloon was 90.8%.

[0101] Example 7

[0102] The preparation method of the balloon of this embodiment uses a long Pebax balloon of 4.0 mm x 300 mm, and the preparation method comprises the following steps:

[0103] Plasma treatment is performed on the surface of the balloon;

[0104] Turn on the balloon folding machine and preheat it for 15-30 minutes to 40°C;

[0105] Apply 15 psi of pressure to the balloon to inflate it, then fold the balloon into flaps for 50 seconds, and then apply negative pressure to the balloon for 10 seconds;

[0106] The balloon was wound once, the winding temperature was set to 65°C, the curling aperture was set to 0.033 inches, the distal end, middle end and proximal end of the balloon were sequentially sent into the winding mold to start winding, the winding pressure was set to 50psi, 100psi and 50psi, and the winding time of the distal end, middle end and proximal end was set to 30s, 30s and 30s respectively to complete the wing folding.

[0107] After the first expansion and contraction of the sample, the distal, middle and proximal ends of the balloon maintained three-flap folds, and the angle between adjacent flaps was tested to be about 120°; after 10 contractions, the distal, middle and proximal ends of the balloon maintained a three-flap effect; the shape retention rate test result after 10 expansions and contractions reached 90.8%, and the shape retention rate test result after 10 expansions and contractions after placement for 8 months reached 90.0%.

[0108] Example 8

[0109] The preparation method of the balloon of this embodiment uses a long Pebax balloon of 4.0 mm x 300 mm, and the preparation method comprises the following steps:

[0110] Plasma treatment is performed on the surface of the balloon;

[0111] Turn on the balloon folding machine and preheat it for 15-30 minutes to 40°C;

[0112] Apply 15 psi of pressure to the balloon to inflate it, then fold the balloon into flaps for 50 seconds, and then apply negative pressure to the balloon for 10 seconds;

[0113] The balloon was wound four times, the winding temperature was set to 65°C, the winding pressure was set to 80psi, the curling aperture was set to 0.033inch, two-thirds of the length near the proximal end of the balloon was fed into the winding mold to start winding, the winding time was set to 15s, and the winding was completed twice. Then, two-thirds of the length near the distal end of the balloon was fed into the winding mold to start winding, the winding time was set to 15s, and the winding was completed twice. After taking out, a 4-times-wound balloon was obtained.

[0114] After the first expansion and contraction of the sample, the distal, middle and proximal ends of the balloon maintained three-flap folds, and the angle between adjacent flaps was tested to be about 120°; after 10 contractions, the distal, middle and proximal ends of the balloon maintained a three-flap effect; after 8 times of expansion and contraction, the shape retention rate test result reached 93.9%, and after 8 months of placement, the shape retention rate test result reached 93.4% after 8 times of expansion and contraction.

[0115] Example 9

[0116] The preparation method of the balloon of this embodiment uses a long balloon made of nylon material with a size of 8.0 mm x 118 mm. The preparation method includes the following steps:

[0117] Plasma treatment is performed on the surface of the balloon;

[0118] Turn on the balloon folding machine and raise the temperature to 40°C;

[0119] Apply 15 psi of pressure to the balloon to inflate it, then fold the balloon into flaps for 25 seconds, and then apply negative pressure to the balloon for 10 seconds;

[0120] The balloon was wound twice, the winding temperature was set to 90°C, the winding pressure was set to 116psi, the curling aperture was set to 0.033inch, two-thirds of the length near the proximal end of the balloon was fed into the winding mold to start winding, and the first winding was completed after the winding time was set to 15s. Then, two-thirds of the length near the distal end of the balloon was fed into the winding mold to start winding, and the second winding was completed after the winding time was set to 15s. After taking out, the balloon was obtained.

[0121] After the first expansion and contraction of the sample, the distal, middle and proximal ends of the balloon maintained three-flap folds, and the angle between adjacent flaps was tested to be about 120°; after 8 contractions, the distal, middle and proximal ends of the balloon maintained a 3-flap effect; the shape retention rate test result after 8 expansions and contractions reached 91.8%, and the shape retention rate test result after 8 months of placement and 8 expansions and contractions reached 92.0%.

[0122] Example 10

[0123] The preparation method of the balloon of this embodiment uses a long Pebax balloon of 5.0 mm x 150 mm, and the preparation method comprises the following steps:

[0124] Turn on the balloon folding machine and preheat it for 15-30 minutes to 40°C;

[0125] Apply 15 psi of pressure to the balloon to inflate it, then fold the balloon into flaps for 50 seconds, and then apply negative pressure to the balloon for 10 seconds;

[0126] The balloon was wound once, the winding temperature was set to 65°C, the curling aperture was set to 0.033 inches, the distal end, middle end and proximal end of the balloon were sequentially sent into the winding mold to start winding, the winding pressure was set to 80 psi, 140 psi and 80 psi respectively, the winding time was set to 15 s, and the wing folding was completed.

[0127] After the first expansion and contraction of the sample, the distal, middle and proximal ends of the balloon maintained three-flap folds, and the angle between adjacent flaps was tested to be about 120°; after 6 contractions, the distal, middle and proximal ends of the balloon maintained a 3-flap effect; after 6 expansions and contractions, the shape retention rate test result reached 83.5%, and after 18 months of placement, the shape retention rate test result reached 83.1% after 5 expansions and contractions.

[0128] Embodiment 11

[0129] The preparation method of the balloon of this embodiment uses a long balloon made of nylon material with a size of 8.0 mm x 118 mm. The preparation method includes the following steps:

[0130] Turn on the balloon folding machine and raise the temperature to 40°C;

[0131] Apply 15 psi of pressure to the balloon to inflate it, then fold the balloon into flaps for 25 seconds, and then apply negative pressure to the balloon for 10 seconds;

[0132] The balloon was wound twice, the winding temperature was set to 83°C, the winding pressure was set to 95psi, the curling aperture was set to 0.033inch, two-thirds of the length near the proximal end of the balloon was fed into the winding mold to start winding, and the first winding was completed after the winding time was set to 15s. Then, two-thirds of the length near the distal end of the balloon was fed into the winding mold to start winding, and the second winding was completed after the winding time was set to 15s. After taking out, the balloon was obtained.

[0133] After the first expansion and contraction of the sample, the distal, middle and proximal ends of the balloon maintained three-flap folds, and the angle between adjacent flaps was tested to be about 120°; after 8 contractions, the distal, middle and proximal ends of the balloon maintained a three-flap effect; the shape retention rate test result after 8 expansions and contractions reached 87.8%, and the shape retention rate test result after 8 months of placement and 8 expansions and contractions reached 87.1%.

[0134] Example 12

[0135] The preparation method of the balloon of this embodiment uses a long Pebax balloon of 4.0 mm x 300 mm, and the preparation method comprises the following steps:

[0136] Plasma treatment is performed on the surface of the balloon;

[0137] Turn on the balloon folding machine and preheat it for 15-30 minutes to 40°C;

[0138] Apply 15 psi of pressure to the balloon to inflate it, then fold the balloon into flaps for 50 seconds, and then apply negative pressure to the balloon for 10 seconds;

[0139] The balloon was wound once, the winding temperature was set to 75°C, the curling aperture was set to 0.033 inches, the distal end, middle end and proximal end of the balloon were sequentially sent into the winding mold to start winding, the winding pressure was 150 psi, the winding time was set to 30 seconds, and the wing folding was completed.

[0140] After the first expansion and contraction of the sample, the distal, middle and proximal ends of the balloon maintained three-flap folds, and the angle between adjacent flaps was tested to be about 120°; after 10 contractions, the distal, middle and proximal ends of the balloon maintained a three-flap effect; after 8 times of expansion and contraction, the shape retention rate test result reached 93.3%; after 8 months of placement, the shape retention rate test result reached 93.0% after 8 times of expansion and contraction.

[0141] Comparative Example 1

[0142] The preparation method of the balloon of this comparative example uses a long balloon made of Pebax material with a size of 4.0 mm x 118 mm, and the preparation method comprises the following steps:

[0143] Plasma treatment is performed on the surface of the balloon;

[0144] Turn on the balloon folding machine and preheat it for 15-30 minutes to 40°C;

[0145] Apply 15 psi of pressure to the balloon to inflate it, then fold the balloon into flaps for 25 seconds, and then apply negative pressure to the balloon for 10 seconds;

[0146] The balloon was wound once, and the winding temperature was set to 50°C, the winding pressure was set to 10psi, and the curling aperture was set to 0.033 inches. The entire balloon was placed into a winding mold and started to be wound. The winding was completed after setting the winding time to 10s, and the balloon was taken out to obtain.

[0147] The balloon has three folded flaps, and the angle between adjacent flaps tested was about 120°; when it was expanded for the second time and then contracted, a C effect appeared in the middle of the balloon, and the three-flap folded flap effect could not be maintained. After placement for 3 months, the balloon expanded and then contracted to present a C-shaped structure.

[0148] Comparative Example 2

[0149] The preparation method of the balloon of this comparative example uses a long balloon made of Pebax material with a size of 4.0 mm x 118 mm. The preparation method comprises the following steps:

[0150] The balloon surface is pre-plasma treated;

[0151] Turn on the balloon folding machine and preheat it for 15-30 minutes to 40°C;

[0152] Apply 15 psi of pressure to the balloon to inflate it, then fold the balloon into flaps for 25 seconds, and then apply negative pressure to the balloon for 10 seconds;

[0153] The balloon was wound twice, the winding temperature was set to 50°C, the winding pressure was set to 9psi, the curling aperture was set to 0.033inch, two-thirds of the length near the proximal end of the balloon was fed into the winding mold to start winding, and the first winding was completed after the winding time was set to 9s. Then, two-thirds of the length near the distal end of the balloon was fed into the winding mold to start winding, and the second winding was completed after the winding time was set to 9s. After taking it out, the balloon was obtained.

[0154] The balloon has three folded flaps, and the angle between adjacent flaps was tested to be approximately 120°; when the balloon was expanded for the second time and then contracted, an S-shaped effect appeared in the middle, and the three-folded flap effect could not be maintained.

[0155] See also Figure 1 , Figure 1The figures are comparison diagrams of the balloon prepared by the preparation method of comparative example 1 and the balloon prepared by the preparation method of embodiment 1 after being pressurized and released, wherein comparative example 1 adopts a single winding, which easily causes the middle part of the balloon to appear flat, such as C-shape or S-shape (it should be noted that the C-shape or S-shape here do not appear at the same time, but are two situations that appear in multiple comparative example experiments); while embodiments 1-8 adopt multiple windings or a single winding, in which the winding time or the winding pressure of the middle part is greater than the winding time or the winding pressure of the two ends, and the multiple windings have an overlapping area, which is between 1 / 4 and 3 / 4 of the length of the balloon, so that the middle part of the balloon is fully stressed, avoiding uneven shrinkage of the balloon after the middle part of the balloon is released, and appearing a flat shape, thereby greatly reducing the inner diameter and resistance of the balloon when it is withdrawn, and avoiding displacement of the stent or damage to the inner wall coating of the stent when the balloon is withdrawn.

[0156] See also Figure 2 and Figure 3 In the figure, compared with Comparative Example 2, the balloons prepared by the preparation methods of Examples 1-12 have smaller contraction sizes of the folded wings after pressure relief after inflation, and the balloons contract more tightly. In addition to the use of multiple windings, the winding time and the winding pressure are also increased. In the embodiments of the present invention, within the range of 10s to 90s for the winding time and within the range of 10psi to 200psi for the winding pressure, the balloons contract more tightly with the increase of the winding time and the winding pressure. Under a certain heating temperature, the winding pressure and the winding time are set in the embodiments of the present invention, which can improve the crease effect of the balloon and the heat setting effect of the folded wing position, eliminate the stress of the balloon folded part, and make the contraction size of the folded wings smaller when the balloon is expanded and then contracted, and the balloon contracts more tightly; after expansion and then contraction, Example 1 still maintains the shape of the three wings, and its shape retention rate reaches more than 80%.

[0157] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the protection scope of the claims.

Claims

1. A long balloon for a balloon expandable stent system, comprising a proximal end, a distal end opposite to the proximal end, and a middle portion located between the proximal end and the distal end, wherein: When the long balloon is expanded and then contracted, the middle part of the long balloon has n stable folded wings, wherein n is an integer greater than or equal to 3; the length of the long balloon is greater than or equal to 38 mm; the uniformity and uniformity of the folded wings of the long balloon after multiple expansion and contraction can reach more than 80%, wherein multiple times refers to 2 to 10 times; The diameter of the proximal end of the long balloon is R1≤ , the diameter R2 of the distal end opposite to the proximal end ≤ , the diameter R3 of the middle part between the proximal end and the distal end≤ , and the diameter fluctuation range of the long balloons in the three parts is within 15%.

2. The long balloon according to claim 1, characterized in that: The proximal end of the long balloon, the distal end opposite to the proximal end, and the middle part between the proximal end and the distal end have the same number of folded wings; the length of the long balloon is 50mm~300mm.

3. The long balloon according to claim 1, characterized in that: The included angles formed between every two adjacent folded wings are equal; the length of the long balloon is 70mm-300mm.

4. The long balloon according to claim 1, characterized in that: There are different included angles between every two adjacent folded wings, and the fluctuation range of the sizes of the two adjacent included angles is within 20%; the length of the long balloon is 80mm~300mm.

5. The long balloon according to claim 1, characterized in that: The long balloon is made of a flexible or soft material; the flexible or soft material is selected from nylon and Pebax; the length of the long balloon is 90 mm to 300 mm.

6. The long balloon according to claim 1, characterized in that: The length of the long balloon is 118 mm to 300 mm.

7. A method for preparing the long balloon according to any one of claims 1 to 6, characterized in that: The following steps are involved: 1) folding the long balloon into n flaps, wherein n is an integer greater than or equal to 3; 2) Winding the long balloon folded into wings; The temperature T for winding the long balloon is 5-125° C., the winding pressure P is 10 psi-200 psi, and the winding time t is 10 s-90 s.

8. The method for preparing the long balloon according to claim 7, characterized in that: The winding covers at least 80% of the area of ​​the entire long balloon.

9. The method for preparing the long balloon according to claim 7, characterized in that: The sum of the products of the winding times N, the single winding pressure P, the single winding temperature T and the single winding time t of the winding of the middle part of the long balloon is greater than the sum of the products of the corresponding winding parameters at both ends, that is, ∑N 中部 *P 中部 *T 中部 *t 中部 >∑N 近端 *P 近端 *T 近端 *t 近端 , and / or ∑N 中部 *P 中部 *T 中部 *t 中部 >∑N 远端 *P 远端 *T 远端 *t 远端 , where: N 中部 ≥1, N 近端 ≥1, N 远端 ≥1.

10. The method for preparing the long balloon according to claim 7 or 9, characterized in that: The sum of the products of the parameters of the winding of the middle part of the long balloon is at least the sum of the products of the parameters of the winding of the proximal end and / or the distal end. times, that is ≥ , and / or ≥ .

11. The method for preparing the long balloon according to claim 9, characterized in that: At least part of the middle part of the long balloon is wound more times than the distal and proximal parts, that is, N 中部 >N 近端 ≥N 远端 ; or the total pressure on the middle part of the long balloon during winding is greater than the total winding pressure on the proximal and distal ends, that is, P 中部总 >P 近端总 ≥P 远端总 Or when the long balloon is wound, the total winding time of the middle part is greater than the total winding time of the proximal and distal ends, that is, t 中部总 >t 近端总 ≥t 远端总 .

12. The method for preparing the long balloon according to claim 7, characterized in that: Before folding the long balloon, the long balloon is subjected to a preheating treatment of heating at 25 to 90° C. for 1 to 30 minutes.

13. The method for preparing the long balloon according to claim 12, characterized in that: Before the preheating treatment, the method further includes subjecting the surface of the elongated balloon to plasma treatment.

14. The method for preparing the long balloon according to claim 7, characterized in that: The long balloon folding comprises the following steps: 1) applying a pressure of 10-100 psi to the long balloon at 25-90° C. to inflate the long balloon; 2) Fold the inflated long balloon into folded wings, with the folding time ranging from 10 to 90 seconds.

Citation Information

Patent Citations

  • Controlled expansion balloon catheter

    CN101808599A

  • Drug balloon protective sleeve and drug balloon assembly including drug balloon protective sleeve

    CN110743089A

  • Polymer scaffold with multi-pleated balloon

    CN105120806A

  • Thin strut stent from bioabsorbable polymer with high fatigue and radial strength and method to manufacture thereof

    CN105992571A

  • Drug-loaded saccule and manufacture method thereof

    CN106075703A