A high temperature extrusion pipe making method for pipe fittings for pressure vessels
By optimizing the calculation model of the mandrel working segment and the extruded pipe process parameters, the grain size and mandrel deformation problems of 00Cr30Ni60Fe10 nickel-based alloy seamless steel pipe are solved, and efficient and safe high-temperature extruded pipe production is achieved, satisfying the High thickness-to-diameter ratio requirements for special-purpose pressure vessels.
Patent Information
- Application Number
- CN202110300025.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-03-22
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-03-22
AI Technical Summary
In the production of 00Cr30Ni60Fe10 nickel-chromium-iron solid solution reinforced nickel-based alloy seamless steel pipes, the grain size control is difficult, which can easily lead to 'busy car' failure, and the core rod is deformed and broken, which cannot meet the high thickness diameter. Compared with the processing requirements of special purpose pressure vessels throughout the parts.
Optimize the design of the core rod working segment calculation model, reasonably set the extrusion pipe process parameters, adopt ring furnace preheating and electromagnetic induction furnace secondary heating, adjust the extrusion temperature and force, reduce the extrusion "bully car" fault, and improve crystal Grain size fineness and mandrel service life.
The production of fine grain size and high thickness-to-diameter ratio of high-temperature extruded pipes is realized, which reduces production costs and energy consumption, ensures production capacity and quality, extends the service life of the core rod, and improves the safety, reliability and efficiency of processing. .
Smart Images

Figure CN115106394B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a process for producing seamless steel pipes in the metallurgical and mechanical industries, and more specifically, to a high-temperature extrusion pipe-making method for pipe fittings for pressure vessels, which is particularly suitable for the high-temperature hot extrusion pipe-making production and processing of 00Cr30Ni60Fe10 nickel-chromium-iron-based solid solution strengthened nickel-based alloy seamless steel pipes with a finished pipe diameter of 100 mm and a wall thickness of more than 20 mm. Background Art
[0002] Seamless steel pipe is a common metallurgical metal product; the commonly used seamless steel pipe high temperature extrusion pipe production process mainly includes tube preparation, tube heating, tube piercing / expansion, billet dephosphorization, tube secondary heating, extrusion pipe making, finished product cooling, inspection, etc., among which extrusion pipe making is the core and key process of the entire high temperature extrusion pipe making process. Seamless steel pipe high temperature extrusion pipe making is a metal forming method that uses the good plasticity of metal materials at high temperatures under three-dimensional compressive stress state, through the die hole formed by the inner hole of the extrusion die and the outer circle of the mandrel, the metal is extruded above the recrystallization temperature, so that the tube (high temperature round steel) is extruded from a die hole to obtain a die hole shape section pipe; seamless steel pipe high temperature extrusion pipe making process, due to the large deformation, high production capacity, high dimensional tolerance control accuracy, uniform metal organization, easy one-time forming control, easy to organize continuous production and other characteristics, suitable for various alloy steel, stainless steel, high strength steel, nickel-based high temperature alloy and other pipe forming pipe, so it has gradually replaced the traditional hot rolling perforation process, and has become the main pipe making method for high-end seamless steel pipe production at home and abroad. Therefore, high temperature extrusion pipe making technology can be used to replace the original metal cutting technology as a processing method for preparing and processing pipe seat penetrations for special-purpose pressure vessels.
[0003] Pipe fittings for pressure vessels are penetrations, which are an important component of special-purpose pressure vessels. They use round seamless steel pipes to partially penetrate the outer shell of the pressure vessel, and connect the penetration with the outer shell of the pressure vessel through welding and other processes to form a tubular component that communicates the inside and outside of the pressure vessel. The so-called penetration refers to the penetration of the containment on the one hand. There are many pipelines that need to enter and exit the containment to install various pipelines. The containment is the third safety barrier of the nuclear power plant, and its integrity is directly related to the radiation safety of the nuclear power plant. Therefore, the penetration is required to be strictly sealed with the containment. On the other hand, it is used for the penetration of the control rod drive mechanism pipe seat of the reactor pressure vessel. As an important pressure boundary of the reactor's primary loop system, it is subjected to high temperature and high pressure and is in direct contact with the coolant. Therefore, the strength, plasticity, toughness, corrosion resistance, and fatigue resistance of the materials used for the penetration are extremely high. The above two types of penetrations have different installation locations and functions, especially the metal properties of the control rod drive mechanism pipe seat penetration are more stringent.
[0004] The first generation of special-purpose pressure vessels in the world were made of 600 alloy, which had relatively poor stress corrosion resistance. In September 1991, cracks were first discovered in the drive mechanism and thermocouple tube sockets in the French pressurized water reactor Bugey 3, which led to a leakage of primary water. This incident led to the international research and development and industrial production of penetration materials. The United States, France and other countries adopted 690 alloy (00Cr30Ni60Fe10) instead of 600 as the penetration material to improve the mechanical properties and corrosion resistance of the pipes used in the penetrations. 690 alloy, namely 00Cr30Ni60Fe10, is a nickel-chromium-iron based solid solution strengthened nickel based corrosion resistant alloy with a Cr content of up to 30%. It has good high temperature corrosion resistance and oxidation resistance, excellent cold and hot processing and welding properties, and has excellent thermal strength and plasticity below 700°C. It can be strengthened by cold working and can also be used for resistance welding, fusion welding or brazing connections, especially for the preparation and processing of oxidation resistant parts that bear low loads below 1100°C. Its main components include C=0.01~0.04%, Cr=28~31%, Ni≥58%, Fe=8~11%, Ti≤0.30%, S≤0.005%, P≤0.01%, etc.
[0005] At present, application research in related fields at home and abroad has shown that 00Cr30Ni60Fe10 alloy has excellent corrosion resistance in a variety of corrosive aqueous media and high-temperature atmospheres, and has better resistance to stress corrosion cracking than 600 and 800 alloys in chloride and sodium hydroxide solutions. It also has high strength, good metallurgical stability and excellent processing characteristics. Therefore, it has become a key component material for nuclear power, petrochemical and other equipment with harsh corrosion environments at home and abroad, especially widely used in penetration parts of special-purpose pressure vessels.
[0006] The research and development and industrial production of domestic special-purpose pressure vessel socket penetrations started in the 1990s. Due to various reasons such as material processing technology and technical equipment, the process of metal smelting → metal forging → mechanical cutting (first drilling and then boring) was adopted to prepare and process metal round steel into tubular components similar to seamless steel pipes. This process technology can complete the preparation and processing of domestic special-purpose pressure vessel socket penetrations, but the alloy material utilization rate is low, the loss is large, the cost is extremely high, and the metal structure is highly non-uniform and the quality is unstable. With the increasing requirements for the safety and reliability of socket penetration products, this process technology can no longer adapt to the sustainable development of the domestic energy (nuclear power) field. According to the development of equipment and process technology in the field of domestic seamless steel pipe production, optimizing and improving the production and processing technology of special-purpose pressure vessel penetrations can not only meet the demand for high-end seamless steel pipes in the energy (nuclear power) field, but also have positive significance for promoting the research and development and production of national heavy equipment, ensuring national energy security, and enhancing the core competitiveness of enterprises.
[0007] The commonly used hot extrusion production process of seamless steel pipes is: billet preparation → cut to size (band saw machine) → drill centering hole (centering hole drilling machine) → external cylindrical cutting (lathe) → drill deep hole (deep hole drilling machine) → end surface processing (lathe) → smooth billet inspection → grinding → cleaning and degreasing (cleaning machine) → preheating of billet (ring furnace) → 1st induction heating (electromagnetic induction furnace) → drilling / expansion (vertical reamer) → 2nd induction heating (electromagnetic induction furnace) → high temperature extrusion (horizontal extruder) → hot sawing (cut to size hot billet) → cooling on cooling bed (cooling bed) or quenching (quenching tank) → inspection → finished product delivery or transfer to cold processing production (see Figure 1 ).
[0008] Since there is no precedent for the production of 00Cr30Ni60Fe10 nickel-chromium-iron based solid solution strengthened nickel-based corrosion resistant alloy high temperature extrusion pipe in China, the yield rate is low when the trial production is carried out with reference to the process method of high temperature extrusion pipe of the same type of nickel-based alloy (similar element composition). The main problems are:
[0009] 1) High grain size requirements, difficult temperature control during extrusion pipe making, and easy to "stuck": Due to the high grain size control requirements for nickel-based alloy seamless steel pipes used for penetration parts (finer than grade 5 fine grains), under the existing technical equipment conditions, the fine grain size of hot extruded pipes processed by extrusion pipe making can only be met by reasonably adjusting (lowering) the extrusion temperature. However, as the extrusion temperature decreases, the deformation resistance of the nickel-based alloy material increases, and the outer dimensions of the finished pipe have determined that a 30.7% thickness-to-diameter ratio requires a larger extrusion pressure. However, the extrusion pressure of the extrusion equipment (extruder) has an upper limit and cannot be increased endlessly. In the work of material deformation resistance, The lower extrusion rod can neither extrude forward nor withdraw (commonly known as "stuck car" in production practice); not only does it cause the scrapping of the billet, but it also damages the core rod and extrusion barrel, etc., directly leading to process failure shutdown, and large energy and other shutdown losses; therefore, it can only be achieved by optimizing the deformation temperature of the billet during extrusion pipe making to overcome the influence of the enhanced deformation resistance of the material, and reduce the occurrence rate of "stuck car" failures on the basis of meeting the technical requirements of grain size for extrusion pipe making; in addition, the extrusion temperature of the same type of nickel-based alloy products such as 690 tubes is currently controlled at 1170±20℃, and the grain size of the hot extruded tube after extrusion is coarse, which does not meet the technical requirements of fine grains finer than level 5.
[0010] 2) The thickness-to-diameter ratio is large, and the diameter of the working section of the mandrel is small and easy to deform and break: The mandrel for extrusion is a slender concentric metal cylinder with a triangular thread on one end and a taper on the other end. The core of the cylinder is processed with a blind hole covering 90% of the total length of the extrusion mandrel. The cylinder consists of a working section, a supporting section, and an installation section. Among them: the working section is a cylinder with a demoulding taper, and its function is to pass through the circular hole in the core of the high-temperature tube blank to control the size and accuracy of the inner hole of the hot extrusion tube during extrusion; the supporting section is a cylinder, and its function is to ensure that the center line of the extrusion mandrel is consistent with the center line of the extrusion barrel; the installation section is a cylinder with a triangular thread and a rectangular flat body on one end, and its function is to connect the mandrel and the ejector rod; the function of the blind hole in the core of the extrusion mandrel is to pass water for cooling.
[0011] The finished product specification of 00Cr30Ni60Fe10 nickel-based alloy extruded tube for penetration is Φ114×35mm, and its thickness-to-diameter ratio (ratio of wall thickness to outer diameter) = 35 / 114 = 30.7%, while the thickness-to-diameter ratio of the same type of nickel-based alloy products is the largest = 34 / 178 = 19.1%, such as the thickness-to-diameter ratio of 690 tube = 15 / 95 = 14.8% or 8 / 76 = 10.5%. Therefore, the thickness-to-diameter ratio of 00Cr30Ni60Fe10 nickel-based alloy extruded tube for penetration is 2 to 3 times higher than that of the same type of nickel-based alloy tube; the larger the thickness-to-diameter ratio, the smaller the diameter of the mandrel working section used for extrusion pipe making; conversely, the smaller the thickness-to-diameter ratio, the larger the diameter of the mandrel working section used for extrusion pipe making; and the diameter of the mandrel working section directly determines the strength and service life of the mandrel in extrusion pipe making; the diameter of the extrusion mandrel working section with a large thickness-to-diameter ratio is small, and it is easy to deform and break during extrusion pipe making. Since the finished product specification size of 00Cr30Ni60Fe10 nickel-based alloy seamless steel pipe used for penetration parts is Φ114×35mm, the inner hole diameter of the hot extruded tube = 114-35×2=44mm, and the working section diameter of the mandrel is smaller than that of the extruded mandrel for the same type of nickel-based alloy products, that is: ΦD=(d×1.01+0.5)-2×s×1.018+0.3=(114×1.018+0.5)-2×35×1.018-0.3=45.59≈45.6mm.
[0012] In the model: D→extrusion core rod outer diameter;
[0013] d→Extended product outer diameter;
[0014] s→wall thickness of extruded product;
[0015] 1.018→Thermal expansion coefficient of the product (taking conventional nickel-based alloy as an example);
[0016] 0.5 → Extrusion die size correction factor based on lubricant thickness etc.;
[0017] 0.3 → Correction factor for extrusion mandrel size based on lubricant thickness etc.
[0018] In summary, in the high-temperature extrusion tube production of 00Cr30Ni60Fe10 nickel-chromium-iron based solid solution strengthened nickel-based corrosion-resistant alloy, it is necessary to meet the requirement of grain size finer than level 5, and to reduce mandrel deformation, breakage and extrusion "stuck car" and other failures. However, the current high-temperature tube making process has certain shortcomings and cannot meet the extrusion tube production of this model of product. Summary of the invention
[0019] In view of the above-mentioned defects existing in the prior art, the purpose of the present invention is to provide a high-temperature extrusion pipe making method for pipe fittings for pressure vessels. According to the elemental composition of 00Cr30Ni60Fe10 nickel-chromium-iron-based solid solution strengthened nickel-based corrosion-resistant alloy, the relevant process parameters such as extrusion pipe making are reasonably set, and the calculation model of the mandrel working section is optimized and designed. On the basis of meeting the technical requirements of high-temperature extrusion pipe making of 00Cr30Ni60Fe10 nickel-based corrosion-resistant alloy, the industrial production of through-pieces for special-purpose pressure vessels is realized; the high-temperature extrusion pipe making method for pipe fittings for pressure vessels of the present invention can not only reduce the deformation, fracture and extrusion "stuck car" and other failures of the mandrel, but also the prepared pipe fittings for pressure vessels meet the requirement of grain size finer than level 5, ensure production capacity and quality, be safe, reliable, practical and efficient, and have significant effects on energy saving, emission reduction and consumption reduction.
[0020] To achieve the above object, the present invention adopts the following technical solution:
[0021] A high temperature extrusion method for manufacturing a pipe fitting for a pressure vessel comprises the following steps:
[0022] (1) Billet preparation, processing according to the processing procedures of qualified billets;
[0023] (2) heating the blank, heating the qualified blank, the process comprising: cleaning and degreasing the blank, preheating the ring furnace, and heating the induction furnace;
[0024] (3) extrusion tube making, the high-temperature billet obtained by the treatment in step (2) is subjected to extrusion tube making, the process comprising optional installation of a mandrel ejector rod, optional installation of an extrusion cylinder, optional installation of a die base and die sleeve, setting extrusion parameters, applying a solid lubricant on the surface of the high-temperature billet, and high-temperature extrusion tube making;
[0025] (4) Material collection and inspection: the hot extruded tube obtained by the process of step (3) is subjected to hot sawing, cooling and inspection to obtain a finished pipe fitting for a pressure vessel.
[0026] Preferably, in step (1), the processing steps of the qualified blanks include round steel inspection, cut to size, external circle cutting, end face cutting, centering hole drilling, drilling / boring, blank inspection, surface grinding, and cleaning machine loading.
[0027] Preferably, in step (1),
[0028] The blank inspection includes size inspection and surface quality inspection; and / or
[0029] The surface grinding is performed by fixed-point grinding, wherein the ratio of the fixed-point grinding depth to the fixed-point grinding width is ≤1:8.
[0030] Preferably, in step (2),
[0031] During the preheating treatment in the annular furnace, the preheating temperature is 950-1050°C; and / or
[0032] During the induction furnace heating treatment, the heating temperature is 1050-1150°C.
[0033] Preferably, in step (2), the preheating temperature is 1000±30°C.
[0034] Preferably, in step (2), the heating temperature is 1090±20°C.
[0035] Preferably, in step (3), when the mandrel mandrel is installed, the working section diameter of the mandrel is:
[0036] ΦD=(d×1.01+0.5)-2×s×1.01-0.3;
[0037] Where: D is the outer diameter of the core rod, unit: mm;
[0038] d is the outer diameter of the finished pipe fittings for pressure vessels, in mm;
[0039] s is the wall thickness of the finished pipe fittings for pressure vessels, in mm;
[0040] The tolerance of the working section diameter of the mandrel is 0.05 mm.
[0041] Preferably, in step (3), the setting of extrusion parameters includes setting extrusion pressure, setting extrusion initial temperature, and setting extrusion speed; the extrusion pressure is ≥40MN, the extrusion initial temperature is 1090±20°C, and the extrusion speed is 150-200mm / s.
[0042] Preferably, in step (3), the extrusion pressure is 40 to 48 MN.
[0043] The high-temperature extrusion method for making pipes for pressure vessels provided by the present invention reasonably sets relevant process parameters such as extrusion pipe making according to the element composition of 00Cr30Ni60Fe10 nickel-chromium-iron-based solid solution strengthened nickel-based corrosion-resistant alloy, and optimizes the design of the mandrel working section calculation model. On the basis of meeting the technical requirements of high-temperature extrusion pipe making of 00Cr30Ni60Fe10 nickel-based corrosion-resistant alloy, the industrial production of penetration pieces for special-purpose pressure vessels is realized.
[0044] It also has the following beneficial effects:
[0045] 1) The process parameters are reasonably designed, the process flow is continuous and compact, and the process of preheating in an annular furnace → secondary heating in an electromagnetic induction furnace → high-temperature extrusion pipe making is adopted to reduce the processes of drilling, expanding holes and secondary heating. On the basis of meeting the technical requirements of high-temperature extrusion pipe making of 00Cr30Ni60Fe10 nickel-chromium-iron-based solid solution strengthened nickel-based corrosion-resistant alloy, it has a significant effect on energy saving, emission reduction and consumption reduction;
[0046] 2) The high-temperature extrusion method for making pipes for pressure vessels of the present invention is suitable for the high-temperature extrusion production requirements of special pipes with high thickness-diameter ratio, high strength, large deformation resistance and slender shape. The hot extruded pipe alloy structure after extrusion processing is uniform and the dimensional tolerance control accuracy is high;
[0047] 3) The core rod working section model is reasonably designed to reduce the core rod breakage failure on site, extend the service life, and reduce the downtime of on-site tooling and mold disposal and the repetitive labor intensity;
[0048] 4) The extrusion pipe temperature is set reasonably, and the temperature is adjusted from time to time through extrusion force feedback to meet the performance requirements of finer grains than grade 5;
[0049] 5) The extrusion pressure of the extrusion tube is set reasonably, and the extrusion pressure matches the deformation resistance of the tube blank, which reduces the "stuck car" failure in the extrusion tube, ensures the production capacity and quality, and is safe, reliable, practical and efficient;
[0050] 6) Accumulate relevant parameters through production practice to create good conditions for the future industrial-scale production of 00Cr30Ni60Fe10 nickel-chromium-iron-based solid solution strengthened nickel-based corrosion-resistant alloy seamless steel pipes;
[0051] 7) 7. Breaking international technical barriers, it has certain reference and application value for the industrial research and development of 00Cr30Ni60Fe10 nickel-based corrosion-resistant alloy seamless steel pipe high-temperature extrusion pipe making in the industry;
[0052] 8) Realize the domestic industrial-scale production of 00Cr30Ni60Fe10 nickel-based alloy seamless steel pipes, promote the localization of key materials in the domestic energy (nuclear power) field, and have broad market application prospects and considerable economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] Figure 1 It is a process flow chart of a high temperature extrusion method for alloy seamless steel pipe in the prior art;
[0054] Figure 2 It is a process flow chart of a high temperature extrusion pipe manufacturing method for a pipe fitting for a pressure vessel of the present invention;
[0055] Figure 3 It is a structural schematic diagram of the high-temperature extrusion pipe making working condition in the method of the present invention;
[0056] Figure 4 It is a schematic structural diagram of a mandrel used in high-temperature extrusion pipe making in the method of the present invention. DETAILED DESCRIPTION
[0057] In order to better understand the above technical solution of the present invention, the technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0058] like Figure 2 As shown, a high temperature extrusion method for manufacturing a pipe fitting for a pressure vessel of the present invention comprises the following steps:
[0059] (1) Billet preparation, processing according to the processing procedures of qualified billets;
[0060] The specific process is as follows: Through CNC processing equipment (such as CNC lathes, etc.), its function is to provide 00Cr30Ni60Fe10 nickel-based corrosion-resistant alloy billets that meet technical requirements, that is, qualified billets; its processing procedures include round steel inspection → cut to size → outer cylindrical surface cutting → end face cutting → drilling centering holes → drilling (boring) holes → billet inspection → surface defect grinding → cleaning machine loading;
[0061] The technical key points of this processing procedure: the processed billets (tube billets or round steel) must be inspected one by one. The billet inspection items include size and surface quality. If there are defects such as folds, cracks, black skin, etc. on the billet surface, local defects can be eliminated by fixed-point grinding. The ratio of fixed-point grinding depth to grinding width should be ≤1:8. The surface roughness of the grinding area must be consistent with the surface roughness of the billet (tube billet or round steel) after cutting.
[0062] (2) Billet heating: heating qualified billets, including billet cleaning and degreasing, ring furnace preheating, and induction furnace heating;
[0063] The specific process is as follows: using annular heating furnace, electromagnetic induction heating furnace, cleaning machine and other equipment, its role is to heat qualified billets, to provide high-temperature billets that meet the technical requirements of the extrusion pipe making process; its main processes include billet cleaning and degreasing → annular furnace preheating → induction furnace heating.
[0064] The technical points of this processing procedure are: controlling the charging temperature, heating time, holding time of the annular furnace and electromagnetic induction furnace and the temperature of qualified billets (tube billets or round steel), etc. The preheating temperature of the annular furnace is controlled at 950-1050℃, preferably 1000±30℃; the heating temperature of the electromagnetic induction furnace is controlled at 1050-1150℃, preferably 1090±20℃.
[0065] (3) extrusion tube making, the high temperature billet obtained by the step (2) is subjected to extrusion tube making, the process includes optional installation of a mandrel ejector, optional installation of an extrusion cylinder, optional installation of a die base and die sleeve, setting extrusion parameters, applying a solid lubricant on the surface of the high temperature billet, and high temperature extrusion tube making;
[0066] The specific process is as follows: High temperature extrusion pipe making conditions Figure 3 As shown, an extrusion unit is used in the high-temperature extrusion pipe making process, and its function is to perform high-temperature hot extrusion pipe making on the high-temperature billet 1 (billet or round steel) heated in step (2) and meeting the temperature requirements. The high-temperature billet 1 enters the extrusion unit along the K direction under the action of the extrusion rod 2, and then performs high-temperature extrusion processing under the action of the core rod 3, the extrusion barrel 4, the mold 5, the mold base 6, the mold sleeve 7, etc., to form a hot extruded tube 8 that meets the requirements; its main processes are optional installation of the core rod 3 and the ejector rod → optional installation of the extrusion barrel 4 → optional installation of the mold 5, the mold base 6, the mold sleeve 7 → setting the extrusion parameters → applying solid lubricant on the surface of the high-temperature billet → high-temperature extrusion pipe making;
[0067] The technical points of this processing procedure are: first, select and prepare the core rod 3, such as Figure 4 As shown in (a), (b) and (c), the mandrel 3 includes a working section M, a supporting section N and a mounting section H, wherein a cooling water blind hole 9 is provided inside the middle through hole of the mandrel 3; during the selection or preparation of the mandrel 3, according to the finished product specifications of the pipe fittings for the pressure vessel and in combination with the calculation model, the calculation model for the diameter of the working section M of the mandrel 3 is:
[0068] ΦD=(d×1.01+0.5)-2×s×1.01-0.3;
[0069] Where: D is the outer diameter of the core rod, unit: mm;
[0070] d is the outer diameter of the finished pipe fittings for pressure vessels, in mm;
[0071] s is the wall thickness of the finished pipe fittings for pressure vessels, in mm;
[0072] 1.01 is the thermal expansion coefficient of 00Cr30Ni60Fe10 alloy products;
[0073] 0.5 is the extrusion die size correction factor based on lubricant thickness;
[0074] 0.3 is the correction factor for the extrusion mandrel size based on the increase in the inner hole of the thick-walled tube when it cools;
[0075] The tolerance of the working section diameter of the core rod is 0.05mm.
[0076] The second is the extrusion parameters, including extrusion pressure, initial extrusion temperature, and extrusion speed. The initial extrusion temperature and extrusion speed are mainly controlled under the condition of extrusion pressure ≥ 40MN to reduce the temperature rise at the moment of extrusion. The initial extrusion temperature is 1090±20℃; the extrusion speed is 150-200mm / s; the extrusion pressure is preferably 40-48MN.
[0077] (4) Material collection and inspection: The hot extruded tube obtained in step (3) is subjected to hot sawing, cooling, and inspection to obtain a finished pipe fitting for a pressure vessel.
[0078] The specific process is as follows: hot sawing machine, cooling bed, water tank and special measuring tools are used, and the main function is to perform hot sawing, cooling (water cooling) and inspection (removing unqualified products) on the hot extruded tube after extrusion tube making. The main processes include hot sawing → cooling → hot extruded tube inspection, etc.
[0079] Technical points of this processing procedure: After high-temperature extrusion pipe making, the hot extruded pipe needs to be cooled by rapid water cooling (immersion in a water tank); the cooling bed operator must check the inner and outer surface quality of each hot extruded pipe one by one, and promptly feedback the surface quality to the extrusion pipe operator to avoid the recurrence of the same type of defects. Example
[0080] This embodiment takes the 00Cr30Ni60Fe10 nickel-chromium-iron-based solid solution strengthened nickel-based corrosion-resistant alloy seamless steel pipe with a blank specification of Φ239×Φ60×750mm and a finished hot extruded pipe specification of Φ114×35mm as an example. Its high-temperature hot extrusion pipe production process consists of four steps: blank preparation → blank heating → extrusion pipe making → material collection inspection. The seamless steel pipe high-temperature extrusion pipe production line involves pipe blank processing equipment (CNC machine tools), heating equipment (ring heating furnace, electromagnetic induction heating furnace), extrusion equipment (extrusion unit), and auxiliary equipment (hot sawing machine, cooling bed, water tank, cleaning, transmission roller, etc.).
[0081] (1) The blank preparation process is undertaken by CNC processing equipment (CNC lathe), whose function is to provide 00Cr30Ni60Fe10 nickel-based corrosion-resistant alloy blanks that meet the technical requirements; the main steps include: round steel inspection → cut to size → outer cylindrical surface cutting → end face cutting → drilling centering holes → drilling (boring) holes → blank inspection → surface defect grinding → cleaning machine loading, etc.
[0082] The technical key points of this process are: the processed tube billets or round steels must be inspected one by one according to Φ239×Φ60×750mm. The inspection items include size and surface quality. If there are defects such as folds, cracks, black skin, etc. on the surface of the tube billet or round steel, local defects can be eliminated by fixed-point grinding. The ratio of grinding depth to grinding width should be ≤1:8. The surface roughness of the grinding area must be consistent with the surface roughness of the tube billet or round steel after cutting.
[0083] (2) The billet heating process is undertaken by annular heating furnaces, electromagnetic induction heating furnaces, cleaning machines and other equipment. Its function is to heat qualified pipe billets or round steels to meet the process and technical requirements of extrusion pipe making. The main steps involved include: billet cleaning and degreasing → annular furnace preheating → induction furnace heating, etc.
[0084] The technical features of this process are: controlling the charging temperature, heating time, holding time of the annular furnace and electromagnetic induction furnace and the controlled temperature of qualified tube billets or round steel, among which the preheating control temperature of the annular furnace is in the range of 950-1050℃, preferably 1000±30℃, and the secondary heating control temperature of the electromagnetic induction furnace is in the range of 1050-1150℃, preferably 1090±20℃.
[0085] (3) The extrusion pipe making process is undertaken by the extrusion unit. Its function is to perform high-temperature hot extrusion pipe making processing on the billet or round steel that has been heated and meets the temperature requirements to produce hot extruded pipes that meet the technical requirements. The main steps involved include: optional installation of mandrel ejector → optional installation of extrusion cylinder → optional installation of mold, die base, and die sleeve → selection of relevant technical parameters → application of solid lubricant on the surface of high-temperature billet or round steel → high-temperature extrusion pipe making processing, etc.
[0086] The technical key points of this process are: first, the selection and preparation of the core rod, that is, the selection and preparation of the extrusion core rod according to the working section diameter calculation model, the calculation model is ΦD=(d×1.01+0.5)-2×s×1.01-0.3, where: D→extrusion core rod outer diameter;
[0087] d→Extended product outer diameter;
[0088] s→wall thickness of extruded product;
[0089] 1.01→00Cr30Ni60Fe10 alloy product thermal expansion coefficient;
[0090] 0.5 → Extrusion die size correction factor based on lubricant thickness etc.;
[0091] 0.3 → Correction factor for extrusion mandrel size based on the increase in the inner hole of thick-walled tube when it cools.
[0092] According to the finished hot extrusion tube specifications of Φ114×35mm, the parameters of the extrusion mandrel working section are calculated as follows:
[0093] ΦD=(d×1.01+0.5)-2×s×1.01-0.3=(114×1.01+0.5)-2×35×1.01-0.3=44.64≈44.6mm, with a tolerance of 0.05mm; therefore, it is appropriate to select and prepare the working section diameter of the core rod as Φ44.6±0.05mm.
[0094] The second is the control of relevant technical parameters of extrusion, based on the control of the initial extrusion temperature and extrusion speed under the condition of satisfying the extrusion pressure ≥ 40MN, to reduce the temperature rise at the moment of extrusion, that is:
[0095] Extrusion temperature control: The initial temperature is controlled in the range of 1050-1150℃, especially 1090±20℃, and the temperature is adjusted from time to time through the feedback of the extrusion pressure (based on satisfying the extrusion pressure ≥40MN).
[0096] Extrusion speed control: By adjusting the extrusion speed control, the temperature rise at the moment of extrusion can be reduced, that is, the running speed of the extrusion barrel (the running speed of the hydraulic main cylinder piston) should be 150-200mm / s, and the extrusion force (cylinder output pressure) should be 40-48MN.
[0097] (4) The material receiving and inspection process is performed by a hot sawing machine, a cooling bed, a water tank and special measuring tools. Its function is to perform hot sawing, cooling (water cooling) and inspection (eliminating unqualified products) on the hot extruded tube after high-temperature extrusion tube making. The main steps involved include: hot sawing → cooling → hot extruded tube inspection, and finally the pressure vessel pipe fittings of this embodiment are obtained.
[0098] The technical key points of this process are: after high-temperature extrusion pipe making, the hot extruded pipe needs to be cooled by rapid water cooling (immersion in a water tank); the cooling bed operator must check the inner and outer surface quality of each hot extruded pipe one by one, and promptly feedback the surface quality to the extrusion pipe making operator to avoid the recurrence of the same type of defects.
[0099] In summary, the high-temperature extrusion method for making pipes for pressure vessels of the present invention reasonably sets the relevant process parameters of the extrusion pipe making according to the element composition of the 00Cr30Ni60Fe10 nickel-chromium-iron-based solid solution strengthened nickel-based corrosion-resistant alloy, and optimizes the design of the mandrel working section calculation model. On the basis of meeting the technical requirements of the high-temperature extrusion pipe making of the 00Cr30Ni60Fe10 nickel-based corrosion-resistant alloy, the industrial production of penetration pieces for special-purpose pressure vessels is realized; the process parameters of the present invention are reasonably designed, the process flow is continuous and compact, and the method adopts The process of preheating in an annular furnace → secondary heating in an electromagnetic induction furnace → high-temperature extrusion pipe making reduces the processes of drilling, expanding holes and secondary heating. On the basis of meeting the technical requirements of high-temperature extrusion pipe making of 00Cr30Ni60Fe10 nickel-chromium-iron-based solid solution strengthened nickel-based corrosion-resistant alloy, it has a significant effect of energy saving, emission reduction and consumption reduction. The high-temperature extrusion pipe making method of the pressure vessel pipe fittings of the present invention is suitable for the high-temperature extrusion pipe making production requirements of special pipe fittings with high aspect ratio, high strength, large deformation resistance and slender shape. The alloy structure of the hot extruded pipe processed by extrusion pipe making is uniform, and the dimensional tolerance is controlled. The system has high precision; the core rod working section model is reasonably designed to reduce the on-site core rod breakage failure, extend the service life, reduce the on-site tooling and mold handling downtime and repetitive labor intensity; the extrusion pipe temperature setting is reasonable, and the temperature is adjusted from time to time through the extrusion force feedback to meet the performance requirements of fine grains finer than level 5; the extrusion pressure setting of the extrusion pipe is reasonable, and the extrusion force matches the deformation resistance of the tube blank, reducing the "stuck car" failure in the extrusion pipe, ensuring production capacity and quality, safe, reliable, practical and efficient; through the accumulation of relevant parameters in production practice, for the future 00Cr3 It creates good conditions for the industrial-scale production of 00Cr30Ni60Fe10 nickel-chromium-iron based solid solution strengthened nickel-based corrosion-resistant alloy seamless steel pipes; breaks international technical barriers, and has certain reference and application value for the industrial research and development of high-temperature extrusion pipe making of 00Cr30Ni60Fe10 nickel-based corrosion-resistant alloy seamless steel pipes in the industry; realizes the domestic industrial-scale production of 00Cr30Ni60Fe10 nickel-based alloy seamless steel pipes, promotes the localization of key materials in the domestic energy (nuclear power) field, and has broad market application prospects and considerable economic benefits.
[0100] Those skilled in the art should recognize that the above embodiments are only used to illustrate the present invention, and are not intended to limit the present invention. As long as they are within the spirit of the present invention, any changes or modifications to the above embodiments will fall within the scope of the claims of the present invention.
Claims
1. A high temperature extrusion method for manufacturing pipe fittings for pressure vessels, applicable to pipe fittings with a finished pipe diameter of more than 100 mm and a wall thickness of more than 20 mm, characterized in that: The steps include: (1) Billet preparation: Processing is carried out according to the processing procedures for qualified billets. The blank is a 00Cr30Ni60Fe10 nickel-based corrosion-resistant alloy blank; The processing procedures of the qualified blanks include round steel inspection, cut to size, external circle cutting, end face cutting, centering hole drilling, drilling / boring, blank inspection, surface grinding, and cleaning machine loading. The blank inspection includes size inspection and surface quality inspection; The surface grinding is performed by fixed-point grinding, wherein the ratio of the fixed-point grinding depth to the fixed-point grinding width is ≤1:8; (2) Heating the blank: heating the qualified blank, the process includes: cleaning and degreasing the blank, preheating the ring furnace, and heating the induction furnace. During the preheating treatment in the annular furnace, the preheating temperature is 950-1050°C; During the induction furnace heating treatment, the heating temperature is 1090±20°C; (3) Extrusion tube making, extruding the high-temperature billet obtained by the treatment in step (2) into a tube; the process includes optional installation of a mandrel and a push rod, optional installation of an extrusion cylinder, optional installation of a die, a die seat and a die sleeve, setting extrusion parameters, applying a solid lubricant on the surface of the high-temperature billet, and high-temperature extrusion tube making. When the mandrel mandrel is optionally installed, the calculation model of the working section diameter of the mandrel is: ΦD=(d×1.01+0.5)-2×s×1.01-0.3; Where: D is the outer diameter of the core rod, unit: mm; d is the outer diameter of the finished pipe fittings for pressure vessels, in mm; s is the wall thickness of the finished pipe fittings for pressure vessels, in mm; 0.5 is the extrusion die size correction factor based on the thickness of the lubricant; 0.3 is the correction factor for the extrusion mandrel size based on the increase in the inner hole of the thick-walled tube when it cools; The tolerance of the working section diameter of the mandrel is 0.05 mm; The extrusion parameters include extrusion pressure, extrusion initial temperature and extrusion speed. The extrusion pressure is ≥40MN, the extrusion initial temperature is 1090±20℃, the temperature is adjusted in real time through the feedback of the extrusion pressure, and the extrusion speed is 150-200mm / s. (4) Material collection and inspection: the hot extruded tube obtained by the process of step (3) is subjected to hot sawing, cooling and inspection to obtain a finished pipe fitting for a pressure vessel.
2. The high temperature extrusion pipe manufacturing method for a pressure vessel pipe according to claim 1, characterized in that: In the step (2), the preheating temperature is 1000±30°C.
3. The high temperature extrusion pipe manufacturing method for a pressure vessel pipe according to claim 1, characterized in that: In the step (3), the extrusion pressure is 40 to 48 MN.