A superconducting wire welding packaging structure, packaging array and packaging method
By using tubular welded pipe structure and high-hard insulation materials in superconducting wire welding, the problems of large contact resistance of the solder joints, local hot spots, unsuitable solder joint size and poor packaging insulation are solved, and the stability and bendability of the solder joints are achieved. simplifies the maintenance process.
Patent Information
- Application Number
- CN202110307090.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-03-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-03-23
AI Technical Summary
The existing superconducting wire welding process has problems such as large contact resistance of solder joints, local hot spots, long solder joints, difficult to bend, difficult packaging insulation, and difficult maintenance and disassembly.
Using a tubular welded pipe structure, the superconducting bare wire that removes the wrapping layer is wound inside the welded pipe, and welded pipe base and head structure are welded, and solder is used to reinforce the welded pipe to avoid extra metal materials. High-hard insulation materials are used to form welded pipes .
The contact resistance of the solder joint is reduced, local hot spots are avoided, flexible bending and good insulation of the solder joints are achieved, and the maintenance and dismantling process is simplified.
Smart Images

Figure CN115117650B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of superconducting wire welding packaging, and in particular to a superconducting wire welding packaging structure, a packaging array and a packaging method. Background Art
[0002] Superconducting wires made of low-temperature metals have zero resistance characteristics under extremely low temperature conditions and play an important role in technical and engineering applications that require high currents and strong magnetic fields. In the application of low-temperature superconducting technology, welding problems between superconducting wires are inevitable. Due to the extremely low temperature zero resistance characteristics of superconducting wires, the welding process of superconducting wires is quite different from that of traditional ordinary wires. In order to ensure the welding quality, the welding of superconducting wires needs to focus on two points: avoiding local hot spots at the weld point and enhancing the stability of the weld point.
[0003] The currently widely used superconducting wire welding processes all take avoiding local hot spots and enhancing the stability of solder joints as the main technical points. The specific operations of the existing welding processes are as follows: before welding, the two superconducting busbars to be welded are pre-treated, the outer sheath of the superconducting busbars is removed, and a longer (200-300mm) superconducting bare wire to be welded is prepared, and the two superconducting bare wires to be welded are placed side by side; then a large amount of molten solder tin is prepared, and the solder tin is directly applied to the superconducting bare wires placed side by side for welding; after the superconducting bare wire welding is completed, a number of copper wires are used to weave and wrap around the outside of the welding part, and the entire wire after being wrapped with copper wires is welded again with solder tin to complete the solder joint reinforcement; finally, the reinforced welding wire is coated with insulating material to complete the entire welding work.
[0004] However, the existing welding process has the following disadvantages:
[0005] (1) Large contact resistance of solder joints
[0006] In the process of placing the superconducting bare wires in parallel, covering them with solder, wrapping copper wire around the solder joints and covering them with solder again, the solder does not completely wrap the wires, and solder gaps will appear in the solder joints, resulting in incomplete contact between the wires and increased contact resistance.
[0007] (2) Local hotspot hazards
[0008] When the copper wire is wrapped and reinforced, it also becomes a part of the solder joint to a certain extent. Electric current will pass through it, thus generating hot spots on the copper wire, posing a risk of causing the superconducting wire at the solder joint to heat up and quench.
[0009] (3) The solder joint is long and difficult to bend
[0010] The wrapped reinforced copper wire causes the entire solder joint to be longer and the wire diameter to be larger, making it difficult to bend the superconducting wire during its laying process. Forced bending will cause uneven stress inside the solder joint, posing a risk of superconducting wire breakage.
[0011] (4) Difficulty in packaging insulation
[0012] After copper wire winding reinforcement and soldering, the copper wire winding is uneven, resulting in local depressions or protrusions. The surface of the entire welding area is not smooth and continuous, causing the insulation layer to wear and break after the equipment has been running for a long time.
[0013] (5) Difficulty in maintenance and disassembly
[0014] Copper wire winding and solder covering make it difficult to disassemble and repair equipment using superconducting wires. The removal of solder joints is complicated and the wires are easily damaged during the disassembly process. Summary of the invention
[0015] The present invention provides a superconducting wire welding packaging structure, a packaging array and a packaging method, which can solve the technical problems in the prior art such as large contact resistance of welding points, hidden dangers of local hot spots, long welding points that are difficult to bend, difficult packaging insulation, and difficult maintenance and disassembly.
[0016] According to one aspect of the present invention, there is provided a superconducting wire welding packaging structure, the packaging structure comprising a welding tube, a first superconducting wire, a second superconducting wire and solder;
[0017] The welded pipe is a tubular structure, the welded pipe comprises a welded pipe body, a first end cap and a second end cap, the inner diameter of the first end of the first end cap is smaller than the inner diameter of the second end, the inner diameter of the first end of the second end cap is smaller than the inner diameter of the second end, the first end of the welded pipe body is connected to the second end of the first end cap, the second end of the welded pipe body is connected to the second end of the second end cap, the axis of the first end cap, the axis of the second end cap and the axis of the welded pipe body are all coincident, the welded pipe body comprises a welded pipe base and a welded pipe cover disposed on the welded pipe base, the height of the welded pipe base in the radial direction is greater than the height of the welded pipe cover in the radial direction, the first end cap comprises a first end cap base and a first end cap cover disposed on the first end cap base, the height of the first end cap base in the radial direction is greater than the height of the first end cap cover in the radial direction, the second end cap comprises a second end cap base and a second end cap cover disposed on the second end cap base, the height of the second end cap base in the radial direction is greater than the height of the second end cap cover in the radial direction;
[0018] The first superconducting wire and the second superconducting wire are arranged in parallel and penetrate the welded pipe, the middle part of the first superconducting wire is a first superconducting bare wire with the wrapping layer removed, and the two end parts are first superconducting busbars with the wrapping layer not removed, the middle part of the second superconducting wire is a second superconducting bare wire with the wrapping layer removed, and the two end parts are second superconducting busbars with the wrapping layer not removed, the first superconducting bare wire and the second superconducting bare wire are arranged to be wound, and the wound first superconducting bare wire and the second superconducting bare wire are located in the welded pipe body and on the axis of the welded pipe body;
[0019] The solder is poured into the welded tube base, the first end cap base and the second end cap base and submerges the wound first superconducting bare wire and the second superconducting bare wire, so as to weld the first superconducting wire and the second superconducting wire.
[0020] Preferably, the length of the first superconducting bare wire is the same as the length of the second superconducting bare wire, both of which are greater than or equal to 20 times the outer diameter of the first superconducting busbar and less than or equal to 30 times the outer diameter of the first superconducting busbar, wherein the outer diameter of the first superconducting busbar is the same as the outer diameter of the second superconducting busbar.
[0021] Preferably, the welded pipe body is a cylinder or a polygonal prism.
[0022] Preferably, the length of the welded pipe body is greater than or equal to 0.95 times the length of the first superconducting bare wire and less than the length of the first superconducting bare wire, and the thickness of the welded pipe body is greater than or equal to 1.5 times the outer diameter of the first superconducting busbar and less than or equal to 2.5 times the outer diameter of the first superconducting busbar; when the welded pipe body is a cylinder, the inner diameter of the welded pipe body is greater than or equal to 8 times the outer diameter of the first superconducting busbar and less than or equal to 12 times the outer diameter of the first superconducting busbar, and when the welded pipe body is a polygonal prism, the diameter of the inscribed circle of the welded pipe body is greater than or equal to 8 times the outer diameter of the first superconducting busbar and less than or equal to 12 times the outer diameter of the first superconducting busbar.
[0023] Preferably, the angle range between the two side endpoints of the cross-section of the welded pipe cover and the axis line of the welded pipe body is 80°~100°, the angle range between the two side endpoints of the cross-section of the first head cover and the axis line of the first head is 80°~100°, and the angle range between the two side endpoints of the cross-section of the second head cover and the axis line of the second head is 80°~100°.
[0024] Preferably, the inner diameter of the first end of the first head and the inner diameter of the first end of the second head are the same, both greater than 2 times the outer diameter of the first superconducting busbar and less than or equal to 2.05 times the outer diameter of the first superconducting busbar.
[0025] Preferably, the material of the welded pipe is an insulating material with high hardness.
[0026] According to another aspect of the present invention, a superconducting wire welding packaging array is provided, the packaging array comprising a plurality of packaging structures in the above-mentioned embodiments, wherein each of the first superconducting wires in the plurality of packaging structures is sequentially connected to form a whole, and each of the second superconducting wires in the plurality of packaging structures is sequentially connected to form a whole.
[0027] According to another aspect of the present invention, a method for welding and packaging a superconducting wire is provided, wherein the welding tube in the above embodiment is used to weld and package a first superconducting wire and a second superconducting wire, and the method comprises:
[0028] Removing the wrapping layer from the middle portion of the first superconducting wire and the middle portion of the second superconducting wire to obtain a first superconducting bare wire and a second superconducting bare wire of a preset length;
[0029] The first superconducting bare wire and the second superconducting bare wire are wound together and pre-welded to firmly connect the first superconducting bare wire and the second superconducting bare wire;
[0030] Connect one end of the welded pipe base to the second end of the first end cap base, and the other end to the second end of the second end cap base;
[0031] Placing the first superconducting wire and the second superconducting wire side by side in a base structure consisting of a welded pipe base, a first end cap base, and a second end cap base, placing the first end cap cover on the first end cap base, placing the second end cap cover on the second end cap base, and stretching both ends of the first superconducting wire and the second superconducting wire so that the first superconducting bare wire and the second superconducting bare wire that are fixedly connected are straightened and suspended in the welded pipe base;
[0032] Pouring solder into the base structure consisting of the welded tube base, the first end cap base and the second end cap base, so that the solder immerses the first superconducting bare wire and the second superconducting bare wire after being fixed, and performing a temperature reduction treatment on the solder;
[0033] The welded tube cover is placed on the welded tube base to complete the welding of the first superconducting wire and the second superconducting wire.
[0034] Preferably, after the welded pipe cover is disposed on the welded pipe base, the method further comprises: wrapping and bonding the welded pipe with insulating tape.
[0035] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0036] (1) Small solder joint contact resistance
[0037] The welding body is arranged so that the height of the welding pipe base in the radial direction is greater than the height of the welding pipe cover in the radial direction, and the first and second heads are arranged so that the height of the head base in the radial direction is greater than the height of the head cover in the radial direction, and the two superconducting bare wires are wound at the same time, and the axes of the two wound superconducting bare wires are coincident with the axis of the welding pipe body, so that the solder can fully contact the two wound superconducting bare wires, thereby reducing the contact resistance; at the same time, the problem of vacancies inside the weld and the existence of wire friction is avoided.
[0038] (2) Avoid local hot spots
[0039] The large amount of solder solidified inside the welded pipe base directly reinforces the welding wire, without the need to use other metal materials with electrical resistance as reinforcement measures, thus avoiding the hidden dangers of local hot spots caused by other metals.
[0040] (3) The welded package array can be bent
[0041] The welding point array formed by the multiple packaging structures of the packaging array can realize free bending of the entire packaging array by bending the superconducting busbars without removing the wrapping layer between the welding points.
[0042] (4) Good package insulation
[0043] The welding pipe uses an insulating material with relatively strong hardness, which not only improves the strength of the welding point, but also ensures the insulation performance of the welding point. At the same time, the outer surface of the packaging structure is smooth, hard and easy to fix, and it is not easy to generate heat by friction with other structures.
[0044] (5) Easy maintenance and disassembly
[0045] The packaging structure includes a welded pipe base, two heads and a welded pipe cover, and has assembly and disassembly capabilities, facilitating welding operations and weld point disassembly and maintenance. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] The included drawings are used to provide a further understanding of the embodiments of the present invention, which constitute a part of the specification, are used to illustrate the embodiments of the present invention, and together with the text description, explain the principles of the present invention. Obviously, the drawings in the following description are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0047] Figure 1 A schematic diagram of a superconducting wire welding packaging structure provided in accordance with an embodiment of the present invention is shown;
[0048] Figure 2 A schematic diagram of a superconducting wire welding packaging array provided according to an embodiment of the present invention is shown;
[0049] Figure 3 Shows Figure 2 A schematic diagram of a first superconducting wire and a second superconducting wire;
[0050] Figure 4 A flow chart of a superconducting wire welding packaging method provided in accordance with an embodiment of the present invention is shown;
[0051] Figure 5 A schematic diagram showing two superconducting bare wires suspended in a welded pipe substrate after winding according to an embodiment of the present invention is shown;
[0052] Figure 6 A schematic diagram of a welded pipe after solder pouring is shown according to an embodiment of the present invention;
[0053] Figure 7 A schematic diagram of a welded pipe after welding is shown according to an embodiment of the present invention.
[0054] Description of Reference Numerals
[0055] 10. welded pipe; 11. welded pipe body; 111. welded pipe base; 112. welded pipe cover;
[0056] 12. first end cap; 121. first end cap base; 122. first end cap cover;
[0057] 13. Second end cap; 131. Second end cap base; 132. Second end cap;
[0058] 20. a first superconducting wire; 21. a first superconducting bare wire; 22. a first superconducting busbar;
[0059] 30. second superconducting wire; 31. second superconducting bare wire; 32. second superconducting busbar;
[0060] 40. Solder. DETAILED DESCRIPTION
[0061] It should be noted that, in the absence of conflict, the embodiments in this application and the features in the embodiments can be combined with each other. The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0062] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0063] Unless otherwise specifically stated, the relative arrangement of the parts and steps described in these embodiments, numerical expressions and numerical values do not limit the scope of the present invention. At the same time, it should be understood that, for ease of description, the sizes of the various parts shown in the accompanying drawings are not drawn according to the actual proportional relationship. The technology, method and equipment known to ordinary technicians in the relevant field may not be discussed in detail, but in appropriate cases, the technology, method and equipment should be regarded as a part of the authorization specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values. It should be noted that similar reference numerals and letters represent similar items in the following drawings, so once a certain item is defined in an accompanying drawing, it does not need to be further discussed in subsequent drawings.
[0064] Figure 1 FIG. 1 is a schematic diagram of a superconducting wire welding packaging structure provided according to an embodiment of the present invention. Figure 1 As shown, the present invention provides a superconducting wire welding packaging structure, the packaging structure includes a welding tube 10, a first superconducting wire 20, a second superconducting wire 30 and a solder 40;
[0065] The welded pipe 10 is a tubular structure. The welded pipe 10 includes a welded pipe body 11, a first end cap 12 and a second end cap 13. The inner diameter of the first end of the first end cap 12 is smaller than the inner diameter of the second end. The inner diameter of the first end of the second end cap 13 is smaller than the inner diameter of the second end. The first end of the welded pipe body 11 is connected to the second end of the first end cap 12, and the second end of the welded pipe body 11 is connected to the second end of the second end cap 13. The axis of the first end cap 12, the axis of the second end cap 13 and the axis of the welded pipe body 11 are all coincident. The welded pipe body 11 includes a welded pipe base 111 and a welded pipe cover disposed on the welded pipe base 111. The pipe cover 112, the height of the welded pipe base 111 in the radial direction is greater than the height of the welded pipe cover 112 in the radial direction, the first end cap 12 includes a first end cap base 121 and a first end cap cover 122 covered on the first end cap base 121, the height of the first end cap base 121 in the radial direction is greater than the height of the first end cap cover 122 in the radial direction, the second end cap 13 includes a second end cap base 131 and a second end cap cover 132 covered on the second end cap base 131, the height of the second end cap base 131 in the radial direction is greater than the height of the second end cap cover 132 in the radial direction;
[0066] The first superconducting wire 20 and the second superconducting wire 30 are arranged in parallel and penetrate the welded pipe 10. The middle part of the first superconducting wire 20 is a first superconducting bare wire 21 without a sheathing layer, and the two end parts are first superconducting busbars 22 without a sheathing layer. The middle part of the second superconducting wire 30 is a second superconducting bare wire 31 without a sheathing layer, and the two end parts are second superconducting busbars 32 without a sheathing layer. The first superconducting bare wire 21 and the second superconducting bare wire 31 are arranged to be wound. After being wound, the first superconducting bare wire 21 and the second superconducting bare wire 31 are located in the welded pipe body 11 and on the axis of the welded pipe body 11.
[0067] The solder 40 is poured into the welding tube base 111 , the first end cap base 121 and the second end cap base 131 and submerges the wound first superconducting bare wire 21 and the second superconducting bare wire 31 for welding the first superconducting wire 20 and the second superconducting wire 30 .
[0068] Compared with the prior art, the present invention has the following beneficial effects:
[0069] (1) Small solder joint contact resistance
[0070] The welding body is arranged so that the height of the welding pipe base in the radial direction is greater than the height of the welding pipe cover in the radial direction, and the first and second heads are arranged so that the height of the head base in the radial direction is greater than the height of the head cover in the radial direction, and the two superconducting bare wires are wound at the same time, and the axes of the two wound superconducting bare wires are coincident with the axis of the welding pipe body, so that the solder can fully contact the two wound superconducting bare wires, thereby reducing the contact resistance; at the same time, the problem of vacancies inside the weld and the existence of wire friction is avoided.
[0071] (2) Avoid local hot spots
[0072] The large amount of solder solidified inside the welded pipe base directly reinforces the welding wire, without the need to use other metal materials with electrical resistance as reinforcement measures, thus avoiding the hidden dangers of local hot spots caused by other metals.
[0073] (3) The welded package array can be bent
[0074] The welding point array formed by the multiple packaging structures of the packaging array can realize free bending of the entire packaging array by bending the superconducting busbars without removing the wrapping layer between the welding points.
[0075] (4) Good package insulation
[0076] The welding pipe uses an insulating material with relatively strong hardness, which not only improves the strength of the welding point, but also ensures the insulation performance of the welding point. At the same time, the outer surface of the packaging structure is smooth, hard and easy to fix, and it is not easy to generate heat by friction with other structures.
[0077] (5) Easy maintenance and disassembly
[0078] The packaging structure includes a welded pipe base, two heads and a welded pipe cover, and has assembly and disassembly capabilities, facilitating welding operations and weld point disassembly and maintenance.
[0079] According to an embodiment of the present invention, the length of the first superconducting bare wire 21 is the same as the length of the second superconducting bare wire 31, both of which are greater than or equal to 20 times the outer diameter of the first superconducting busbar 22 and less than or equal to 30 times the outer diameter of the first superconducting busbar 22, wherein the outer diameter of the first superconducting busbar 22 is the same as the outer diameter of the second superconducting busbar 32. Through the above arrangement, the contact area of the welding point can be increased, thereby reducing the contact resistance.
[0080] According to an embodiment of the present invention, according to actual wiring space requirements, the welding pipe body 11 can be a cylinder or a polygonal prism.
[0081] According to an embodiment of the present invention, the length of the welded pipe body 11 is greater than or equal to 0.95 times the length of the first superconducting bare wire 21 and less than the length of the first superconducting bare wire 21, the thickness of the welded pipe body 11 is greater than or equal to 1.5 times the outer diameter of the first superconducting busbar 22 and less than or equal to 2.5 times the outer diameter of the first superconducting busbar 22; when the welded pipe body 11 is a cylinder, the inner diameter of the welded pipe body 11 is greater than or equal to 8 times the outer diameter of the first superconducting busbar 22 and less than or equal to 12 times the outer diameter of the first superconducting busbar 22; when the welded pipe body 11 is a polygonal prism, the diameter of the inscribed circle of the welded pipe body 11 is greater than or equal to 8 times the outer diameter of the first superconducting busbar 22 and less than or equal to 12 times the outer diameter of the first superconducting busbar 22. By limiting the length of the two superconducting bare wires, the length of the two superconducting bare wires after winding is substantially consistent with the length of the welded pipe body 11. Through the above arrangement, the welding tube base 111 can contain as much solder 40 as possible while meeting the volume requirement, so as to increase the contact area of the welding point and thus reduce the contact resistance.
[0082] According to one embodiment of the present invention, the angle range between the two side endpoints of the cross section of the welded pipe cover 112 and the axis line of the welded pipe body 11 is 80°~100°, the angle range between the two side endpoints of the cross section of the first head cover 122 and the axis line of the first head 12 is 80°~100°, and the angle range between the two side endpoints of the cross section of the second head cover 132 and the axis line of the second head 13 is 80°~100°, thereby ensuring that the welded pipe cover 112, the first head cover 122 and the second head cover 132 all have a smaller width, thereby ensuring that the base structure formed by the welded pipe base 111, the first head cover 122 and the second head cover 132 can hold enough solder 40.
[0083] According to one embodiment of the present invention, the inner diameter of the first end of the first head 12 and the inner diameter of the first end of the second head 13 are the same, both of which are greater than 2 times the outer diameter of the first superconducting busbar 22 and less than or equal to 2.05 times the outer diameter of the first superconducting busbar 22, so that the two superconducting wires are just stuck in the two heads.
[0084] According to an embodiment of the present invention, the material of the welding pipe 10 is a high-hardness insulating material to ensure the strength and insulation of the entire welding point. For example, the material of the welding pipe 10 can be epoxy resin.
[0085] According to an embodiment of the present invention, the solder 40 may be made of Wood's metal.
[0086] Figure 2FIG. 2 shows a schematic diagram of a superconducting wire welding packaging array provided according to an embodiment of the present invention. Figure 2 As shown, the present invention provides a superconducting wire welding packaging array, which includes a plurality of packaging structures in the above embodiments, wherein each of the first superconducting wires 20 in the plurality of packaging structures is connected in sequence to form a whole, and each of the second superconducting wires 30 in the plurality of packaging structures is connected in sequence to form a whole.
[0087] That is to say, the plurality of first superconducting wires 20 and the plurality of second superconducting wires 30 in the welding package array are all whole superconducting wires. In the actual operation, the wrapping layer of two superconducting wires to be welded is removed at intervals, and the positions where the wrapping layers of the two superconducting wires to be welded are removed are exactly the same, so as to obtain multiple pairs of one-to-one corresponding superconducting bare wires to be welded, as shown in FIG. Figure 3 As shown. Then, the welding tube 10 is used to weld and package each superconducting bare wire to be welded in turn to obtain a welding package array. Among them, each welding tube 10 after welding and packaging can be regarded as a welding point, and the welding package array can be regarded as a welding point array. The welding point array can ensure that the entire structure has a sufficiently long superconducting bare wire contact, and there are enough superconducting bare wires in the solder 40, thereby reducing the welding point resistance; at the same time, the welding point array can realize the arbitrary bending of the entire welding point array through the bending ability of the superconducting busbar that is not welded between each two welding tubes 10.
[0088] The welding package array can have one bend or multiple bends, and the number of bends and the bend angles are arranged according to the placement space and the position of the welding points. The bendable welding package array is helpful for arranging the superconducting wire and its welding points in a limited space.
[0089] Figure 4 FIG. 2 is a flow chart showing a superconducting wire welding packaging method according to an embodiment of the present invention. Figure 4 As shown, the present invention provides a superconducting wire welding packaging method, using the welding tube 10 in the above embodiment to weld and package the first superconducting wire 20 and the second superconducting wire 30, the method comprising:
[0090] S1, removing the wrapping layer from the middle portion of the first superconducting wire 20 and the middle portion of the second superconducting wire 30 to obtain a first superconducting bare wire 21 and a second superconducting bare wire 31 of a preset length;
[0091] S2, winding the first superconducting bare wire 21 and the second superconducting bare wire 31 and pre-welding them to firmly connect the first superconducting bare wire 21 and the second superconducting bare wire 31;
[0092] S3, connecting one end of the welded pipe base 111 to the second end of the first end cap base 121, and the other end to the second end of the second end cap base 131;
[0093] S4, placing the first superconducting wire 20 and the second superconducting wire 30 side by side in the base structure composed of the welded tube base 111, the first end cap base 121 and the second end cap base 131, covering the first end cap 122 on the first end cap base 121, and covering the second end cap 132 on the second end cap base 131, and stretching the first superconducting wire 20 and the second superconducting wire 30 at both ends so that the first superconducting bare wire 21 and the second superconducting bare wire 31 after being fixed are straightened and suspended in the welded tube base 111, as shown in FIG. Figure 5 As shown;
[0094] S5, pouring the solder 40 into the base structure composed of the welding tube base 111, the first end cap base 121 and the second end cap base 131, so that the solder 40 immerses the first superconducting bare wire 21 and the second superconducting bare wire 31 after being fixed, and cooling the solder 40, such as Figure 6 As shown;
[0095] S6, cover the welded tube cover 112 on the welded tube base 111 to complete the welding of the first superconducting wire 20 and the second superconducting wire 30, as shown in FIG. Figure 7 shown.
[0096] Compared with the prior art, the present invention has the following beneficial effects:
[0097] (1) Small solder joint contact resistance
[0098] The welding body is arranged so that the height of the welding pipe base in the radial direction is greater than the height of the welding pipe cover in the radial direction, and the first and second heads are arranged so that the height of the head base in the radial direction is greater than the height of the head cover in the radial direction, and the two superconducting bare wires are wound at the same time, and the axes of the two wound superconducting bare wires are coincident with the axis of the welding pipe body, so that the solder can fully contact the two wound superconducting bare wires, thereby reducing the contact resistance; at the same time, the problem of vacancies inside the weld and the existence of wire friction is avoided.
[0099] (2) Avoid local hot spots
[0100] The large amount of solder solidified inside the welded pipe base directly reinforces the welding wire, without the need to use other metal materials with electrical resistance as reinforcement measures, thus avoiding the hidden dangers of local hot spots caused by other metals.
[0101] (3) The welded package array can be bent
[0102] The welding point array formed by the multiple packaging structures of the packaging array can realize free bending of the entire packaging array by bending the superconducting busbars without removing the wrapping layer between the welding points.
[0103] (4) Good package insulation
[0104] The welding pipe uses an insulating material with relatively strong hardness, which not only improves the strength of the welding point, but also ensures the insulation performance of the welding point. At the same time, the outer surface of the packaging structure is smooth, hard and easy to fix, and it is not easy to generate heat by friction with other structures.
[0105] (5) Easy maintenance and disassembly
[0106] The packaging structure includes a welded pipe base, two heads and a welded pipe cover, and has assembly and disassembly capabilities, facilitating welding operations and weld point disassembly and maintenance.
[0107] In S1 of the present invention, the preset length may be any value that is greater than or equal to 20 times the outer diameter of the first superconducting busbar 22 and less than or equal to 30 times the outer diameter of the first superconducting busbar 22 .
[0108] In S2 of the present invention, in order to increase the contact area of the welding point, the first superconducting bare wire 21 and the second superconducting bare wire 31 are wound and arranged. In order to ensure that the two superconducting bare wires do not loosen after winding, indium (solder) can be used to pre-weld the two superconducting bare wires after winding so that the two superconducting bare wires are fixed together.
[0109] In S3 of the present invention, the connection between the welded pipe base 111 and the two end cap bases may be achieved by snap-fitting or bonding.
[0110] In S4 of the present invention, both ends of the first superconducting wire 20 and the second superconducting wire 30 are stretched simultaneously, so that the two superconducting bare wires after being fixed are in a straight state and suspended on the axis of the welded pipe base 111. The first end cap 122 and the first end cap base 121 can be connected by means of snap fastening or bonding, and the second end cap 132 and the second end cap base 131 can be connected by means of snap fastening or bonding.
[0111] In S5 of the present invention, Wood's alloy (solder) can be used to fill the entire base structure composed of the welded tube base 111, the first end base 121 and the second end base 131, so that the two superconducting bare wires suspended on the axis of the welded tube base 111 are fully immersed in the Wood's alloy, thereby achieving full contact between the Wood's alloy and the two superconducting bare wires after winding, reducing the contact resistance; and avoiding the problem of vacancies inside the welding point and the existence of wire friction. After the temperature is reduced, the Wood's alloy will solidify, realizing the welding of the two superconducting bare wires.
[0112] In S6 of the present invention, the connection between the welded pipe cover 112 and the welded pipe base 111 can be achieved by snapping or bonding.
[0113] According to an embodiment of the present invention, after the welding pipe cover 112 is covered on the welding pipe base 111, the method further includes: using insulating tape to wrap and bond the welding pipe 10 to further ensure the connection tightness and insulation of the welding pipe 10. Furthermore, the insulating tape can be made of glass cloth.
[0114] In the present invention, when packaging the array, each pair of superconducting bare wires can be welded and packaged using the above method in sequence.
[0115] By adopting the packaging structure or packaging method of the present invention, the contact area between superconducting wires can be increased as much as possible, the contact resistance can be reduced, and wire friction can be avoided, thereby ensuring the stability between the soldering point and the wires in its vicinity, thereby preventing the soldering point from generating local hot spots, thereby avoiding the phenomenon of the entire superconducting circuit being quenched due to the superconducting wire heating up and the normal operation of the equipment being interrupted.
[0116] By adopting the packaging structure or packaging method of the present invention, the solder joint itself is reinforced to prevent the solder joint from being broken due to external mechanical tensile force or tangential force. At the same time, the solder joint itself is insulated and fixed to prevent the solder joint from vibrating during equipment operation and generating friction heat with other external parts or equipment, which further causes the superconducting wire inside the solder joint to quench.
[0117] In the description of the present invention, it is necessary to understand that the directions or positional relationships indicated by directional words such as "front, back, up, down, left, right", "lateral, vertical, perpendicular, horizontal" and "top, bottom" are usually based on the directions or positional relationships shown in the drawings. They are only for the convenience of describing the present invention and simplifying the description. Unless otherwise specified, these directional words do not indicate or imply that the devices or elements referred to must have a specific direction or be constructed and operated in a specific direction. Therefore, they cannot be understood as limiting the scope of protection of the present invention. The directional words "inside and outside" refer to the inside and outside relative to the contours of each component itself.
[0118] For ease of description, spatially relative terms such as "above", "above", "on the upper surface of", "above", etc. may be used here to describe the spatial positional relationship between a device or feature and other devices or features as shown in the figure. It should be understood that spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientation described in the figure. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Thus, the exemplary term "above" can include both "above" and "below". The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatially relative descriptions used here are interpreted accordingly.
[0119] In addition, it should be noted that the use of terms such as "first" and "second" to limit components is only for the convenience of distinguishing the corresponding components. If not otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of the present invention.
[0120] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A superconducting wire welding packaging structure, characterized in that: The packaging structure comprises a welding tube (10), a first superconducting wire (20), a second superconducting wire (30) and solder (40); The welded pipe (10) is a tubular structure, comprising a welded pipe body (11), a first end cap (12) and a second end cap (13); the inner diameter of the first end of the first end cap (12) is smaller than the inner diameter of the second end; the inner diameter of the first end of the second end cap (13) is smaller than the inner diameter of the second end; the first end of the welded pipe body (11) is connected to the second end of the first end cap (12); the second end of the welded pipe body (11) is connected to the second end of the second end cap (13); the axis of the first end cap (12), the axis of the second end cap (13) and the axis of the welded pipe body (11) are all coincident; the welded pipe body (11) comprises a welded pipe base (111) and a cover disposed on the welded pipe base (111). a welded pipe cover (112), the height of the welded pipe base (111) in the radial direction being greater than the height of the welded pipe cover (112) in the radial direction, the first end cap (12) comprising a first end cap base (121) and a first end cap cover (122) disposed on the first end cap base (121), the height of the first end cap base (121) in the radial direction being greater than the height of the first end cap cover (122) in the radial direction, the second end cap (13) comprising a second end cap base (131) and a second end cap cover (132) disposed on the second end cap base (131), the height of the second end cap base (131) in the radial direction being greater than the height of the second end cap cover (132) in the radial direction; The first superconducting wire (20) and the second superconducting wire (30) are arranged in parallel and penetrate the welded pipe (10); the middle portion of the first superconducting wire (20) is a first superconducting bare wire (21) with the sheath removed, and the two end portions are first superconducting busbars (22) with the sheath not removed; the middle portion of the second superconducting wire (30) is a second superconducting bare wire (31) with the sheath removed, and the two end portions are second superconducting busbars (32) with the sheath not removed; the first superconducting bare wire (21) and the second superconducting bare wire (31) are arranged in a wound manner; and the wound first superconducting bare wire (21) and the second superconducting bare wire (31) are located inside the welded pipe body (11) and on the axis of the welded pipe body (11); The solder (40) is poured into the welded tube base (111), the first end cap base (121) and the second end cap base (131) and submerges the wound first superconducting bare wire (21) and the second superconducting bare wire (31) to weld the first superconducting wire (20) and the second superconducting wire (30).
2. The packaging structure according to claim 1, characterized in that: The length of the first superconducting bare wire (21) is the same as the length of the second superconducting bare wire (31), and both are greater than or equal to 20 times the outer diameter of the first superconducting busbar (22) and less than or equal to 30 times the outer diameter of the first superconducting busbar (22), wherein the outer diameter of the first superconducting busbar (22) is the same as the outer diameter of the second superconducting busbar (32).
3. The packaging structure according to claim 2, characterized in that: The welded pipe body (11) is a cylinder or a polygonal prism.
4. The packaging structure according to claim 3, characterized in that: The length of the welded pipe body (11) is greater than or equal to 0.95 times the length of the first superconducting bare wire (21) and less than the length of the first superconducting bare wire (21); the thickness of the welded pipe body (11) is greater than or equal to 1.5 times the outer diameter of the first superconducting busbar (22) and less than or equal to 2.5 times the outer diameter of the first superconducting busbar (22); when the welded pipe body (11) is a cylinder, the inner diameter of the welded pipe body (11) is greater than or equal to 8 times the outer diameter of the first superconducting busbar (22) and less than or equal to 12 times the outer diameter of the first superconducting busbar (22); when the welded pipe body (11) is a polygonal prism, the diameter of the inscribed circle of the welded pipe body (11) is greater than or equal to 8 times the outer diameter of the first superconducting busbar (22) and less than or equal to 12 times the outer diameter of the first superconducting busbar (22).
5. The packaging structure according to claim 2, characterized in that: The angle between the two side endpoints of the cross section of the welded pipe cover (112) and the axis line of the welded pipe body (11) is in the range of 80° to 100°, the angle between the two side endpoints of the cross section of the first head cover (122) and the axis line of the first head (12) is in the range of 80° to 100°, and the angle between the two side endpoints of the cross section of the second head cover (132) and the axis line of the second head (13) is in the range of 80° to 100°.
6. The packaging structure according to claim 2, characterized in that: The inner diameter of the first end of the first head (12) and the inner diameter of the first end of the second head (13) are the same, both being greater than 2 times the outer diameter of the first superconducting busbar (22) and less than or equal to 2.05 times the outer diameter of the first superconducting busbar (22).
7. The packaging structure according to claim 2, characterized in that: The material of the welded pipe (10) is an insulating material with high hardness.
8. A superconducting wire welding packaging array, characterized in that: The packaging array comprises a plurality of packaging structures according to any one of claims 1 to 7, wherein each of the first superconducting wires (20) in the plurality of packaging structures is sequentially connected to form a whole, and each of the second superconducting wires (30) in the plurality of packaging structures is sequentially connected to form a whole.
9. A superconducting wire welding packaging method, characterized in that: A first superconducting wire (20) and a second superconducting wire (30) are welded and packaged using a welding tube (10) in a packaging structure according to any one of claims 1 to 7, the method comprising: Removing the coating from the middle portion of the first superconducting wire (20) and the middle portion of the second superconducting wire (30) to obtain a first superconducting bare wire (21) and a second superconducting bare wire (31) of a preset length; The first superconducting bare wire (21) and the second superconducting bare wire (31) are wound together and then pre-welded to securely connect the first superconducting bare wire (21) and the second superconducting bare wire (31); Connecting one end of the welded pipe base (111) to the second end of the first end cap base (121), and connecting the other end to the second end of the second end cap base (131); Placing the first superconducting wire (20) and the second superconducting wire (30) side by side in a base structure consisting of a welded tube base (111), a first end cap base (121) and a second end cap base (131), placing the first end cap cover (122) on the first end cap base (121), placing the second end cap cover (132) on the second end cap base (131), and stretching both ends of the first superconducting wire (20) and the second superconducting wire (30) so that the first superconducting bare wire (21) and the second superconducting bare wire (31) are straightened and suspended in the welded tube base (111); Pouring solder (40) into a base structure consisting of a welded tube base (111), a first end cap base (121) and a second end cap base (131), allowing the solder (40) to submerge the first superconducting bare wire (21) and the second superconducting bare wire (31) that have been fixedly connected, and subjecting the solder (40) to a cooling treatment; The welded tube cover (112) is placed on the welded tube base (111) to complete the welding of the first superconducting wire (20) and the second superconducting wire (30).
10. The method according to claim 9, characterized in that After the welding pipe cover (112) is covered on the welding pipe base (111), the method further comprises: using insulating tape to wrap and bond the welding pipe (10) to fix it.
Citation Information
Patent Citations
Superconducting wire and method for manufacturing same
CN107438887A
A cylindrical sub-cable lap-on superconducting joint
CN109148074A
Wire harness
CN111164712A
Method for producing a pipe seal of a pipe string and method for producing a sealed pipe connection
DE102015117020A1
Method for connecting conductor of superconductive direct current cable
JP1998228933A