Method for producing sintered ore
By enriching oxygen in the middle and lower parts of the belt sintering machine, the problems of strength and powderization rate of sintered ore in the blast furnace are solved, and efficient sintered ore production is achieved, avoiding the cost of using gas fuel and Issues of lower ventilation.
Patent Information
- Application Number
- CN202180014681.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-02-27
- Filing Date
- 2021-02-22
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-02-22
AI Technical Summary
The prior art has shortcomings in improving the strength of sintered ore and reducing the powdering rate, especially in the transportation and storage process in blast furnaces, and the method of using gas fuel has problems of cost and ventilation.
In the downward suction belt sintering machine, oxygen enrichment is avoided by performing oxygen enrichment in the middle and lower portions of the raw material loading layer, and oxygen enrichment is started about 4 minutes after ignition, and it continues until 13 minutes. Oxygen enrichment was performed using oxygen-enriched air at an oxygen concentration of more than 25 vol.% but not more than 50 vol.%.
The overall strength of the sintered ore is significantly improved, the productivity is reduced, the efficient sintering reaction and the stability of the finished product are ensured, and the powdering rate is reduced.
Smart Images

Figure CN115135781B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing sintered ore by oxygen enrichment operation using a downdraft belt-type (Dwight-Lloyd, DL) sintering machine. Background Art
[0002] A blast furnace is a device that uses an iron source such as lump ore or sintered ore, loads raw materials containing the iron source from the upper part of the furnace, and blows reducing gas from the lower part of the furnace, thereby melting and reducing the iron source to produce molten iron. Generally speaking, in the furnace of a blast furnace, in order to promote the reaction between the reducing gas and the iron source, the reducing gas must flow fully. For this reason, it is effective to improve the air permeability in the blast furnace, as a result, it is possible to achieve an increase in the productivity of molten iron and a reduction in cost. In order to improve the air permeability in the blast furnace, the powder rate of the iron source raw material must be suppressed. In order to reduce the powder rate, it is effective to use raw materials with high strength. For this reason, various methods have been proposed in the past to improve the strength of the iron source raw material, i.e., sintered ore, loaded in the blast furnace.
[0003] For example, Patent Document 1 proposes a technique for promoting combustion and improving the yield by blowing oxygen into the raw material loading layer on the pallet of a DL sintering machine. The technique disclosed in the document is a method for enriching oxygen in the upper layer of the raw material loading layer on the pallet for the purpose of improving productivity, increasing the yield, or reducing the powder generation rate when the sintered cake is crushed. However, it is described that the position of oxygen enrichment in the prior art is limited to the ignition position of the raw material loading layer, and oxygen enrichment after this point has no effect. In addition, there is no clear record of the raw material properties, etc., and there is no mention of the strength of the finished sintered ore, especially the method of reducing the powder generated during transportation and storage before reaching the furnace of the blast furnace.
[0004] In addition, a method for producing sintered ore by supplying gas fuel to the raw material loading layer on the trolley of the DL sintering machine is proposed in Patent Document 2. According to this method, the combustion area (combustion zone) in the raw material loading layer during sintering is expanded, and during the production, the weak strength part is also filled with heat, which can improve the strength of the finished product.
[0005] Furthermore, Patent Document 3 proposes a method for producing a high-strength sintered ore by blowing a gas fuel together with oxygen during sintering to create a temperature condition suitable for sintering in a raw material loading layer.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Laid-Open No. 2-073924
[0009] Patent Document 2: Japanese Patent Application Publication No. 2008-95170
[0010] Patent Document 3: Japanese Patent Application Publication No. 2014-31580
[0011] Patent Document 4: Japanese Patent Application Publication No. 2010-126773
[0012] Patent Document 5: Japanese Patent Application Laid-Open No. 9-227958 Summary of the invention
[0013] Problems to be solved by the invention
[0014] The above-mentioned prior art, especially the technology described in Patent Document 1, is a method of enriching the upper layer of the raw material loading layer with oxygen only immediately after ignition, with the purpose of compensating for the combustion and melting reaction (sintering reaction) of the upper layer of the raw material loading layer with less heat input. In this method, although the powder generation rate is reduced when the sintered cake is crushed, it has no significant effect on the reduction of the overall strength of the finished sintered ore after crushing, that is, the reduction of the powder generated during transportation and storage to the blast furnace.
[0015] In addition, the methods disclosed in Patent Documents 2, 3, and 4 must be used in combination with gas fuel, which has a cost problem. In addition, these methods expand the combustion area / molten liquid generation area during combustion, resulting in a problem of reduced air permeability and reduced productivity.
[0016] In addition, in Patent Document 5, as part of the exhaust gas circulation process technology using the sintering machine, a method of oxygen enrichment in the middle layer of the raw material loading layer is proposed. That is, the proposal is a technology that oxygen-enriched air and circulating exhaust gas are sucked into the middle layer of the raw material loading layer, and the exhaust gas after the reaction of these gases is further sucked into the lower layer of the raw material loading layer and circulated. However, since the oxygen concentration of the circulating exhaust gas is low, this technology will cause the combustion reaction to stagnate in the lower layer, so it is a method of enriching the middle layer with low concentration of oxygen in advance. Therefore, this technology is not a technology for promoting the sintering reaction in the middle layer. In addition, the exhaust gas circulation process in this technology is used to reduce the environmental burden caused by the exhaust gas of the sintering machine, and the ratio of the area of the oxygen-enriched air and the circulating exhaust gas should be designed according to the conditions of the raw materials, the sintering machine, and the exhaust gas treatment equipment, and the effect of the sintering reaction brought about by oxygen enrichment alone cannot be expected. Therefore, it can be considered that the oxygen enrichment of the sintering raw material layer was originally expected not to be used in combination with the exhaust gas circulation process.
[0017] An object of the present invention is to provide a method for producing high-strength sintered ore while maintaining high productivity by not using gaseous fuel in the operation of a sintering machine and by appropriately enriching oxygen at a position closer to a discharge portion than an ignition position.
[0018] Solutions to the problem
[0019] In order to solve the above problems and achieve the above objectives, the inventors stopped supplying gas fuel from above the sintering bed (raw material loading layer) of the sintering machine, and on the other hand, investigated the influence of the position (timing) and time of oxygen enrichment on the strength and productivity of the sintered ore. As a result, it was found that, in the case of the method disclosed in Patent Document 1, i.e., oxygen enrichment at the timing of combustion of the upper layer of the sintering bed (raw material loading layer), although the yield rate was improved, the strength of the finished product (sintered ore) was basically not increased. It can be considered that this is because: in the above-mentioned prior art, the sintering reaction is insufficient, and although the strength of the upper layer of the raw material loading layer with low strength is increased to the extent that it does not pulverize when crushed due to oxygen enrichment, the strength of the finished product is only equal to or less than the strength of the middle layer to the lower layer of the raw material loading layer, and the strength of the finished product as a whole is not improved.
[0020] Therefore, the inventors tried to perform oxygen enrichment using oxygen-enriched air at the timing of combustion not only in the upper layer of the raw material loading layer, but also in the middle layer and the lower layer. As a result, it was found that by oxygen enrichment in the middle layer to the lower layer of the raw material loading layer, the pulverization rate during crushing was low, and a certain degree of strength could be expected. Although the yield rate was reduced, the productivity was not reduced, and the strength of the entire finished product could be greatly improved.
[0021] In particular, it was found that if oxygen enrichment of the raw material loading layer is carried out at least in the middle layer, the effect of improving the overall strength of the finished product is increased. It was found that based on the oxygen enrichment of the middle layer, it is effective to further implement oxygen enrichment of the upper layer and / or oxygen enrichment of the lower layer of the raw material loading layer as needed.
[0022] That is, the present invention relates to a method for manufacturing sintered ore, which comprises: loading sintering mixed raw materials including iron ore and carbon material into a raw material supply section on a circulating trolley of a sintering machine to form a raw material loading layer, then, using an ignition furnace arranged on the downstream side of the raw material supply section to ignite the carbon material on the upper surface (upper layer) of the above-mentioned raw material loading layer, and further, sucking gas above the above-mentioned raw material loading layer through a bellows arranged under the trolley, introducing the gas into the raw material loading layer, and causing the carbon material in the raw material loading layer to burn in sequence, thereby sintering the mixed raw materials to manufacture sintered ore, wherein, when oxygen enrichment is performed from above the above-mentioned raw material loading layer on the sintering machine, oxygen enrichment treatment is performed at a position closer to the discharge section side than the position of the raw material loading layer when 4 minutes have passed since the upper surface of the raw material loading layer was ignited, and sintering is performed.
[0023] (1) In the method of the present invention, it is preferred that the oxygen enrichment be terminated before 13 minutes have passed since the ignition of the raw material loading layer.
[0024] (2) In the above method of the present invention, the time for oxygen enrichment of the raw material loading layer is preferably set to 1 to 7 minutes in terms of the passage time of the sintering compound raw material.
[0025] (3) In the above method of the present invention, preferably, oxygen enrichment is not performed until 4 minutes have passed since the upper surface of the loading layer is ignited.
[0026] (4) The above method of the present invention is preferably not used in combination with an exhaust gas recycling process.
[0027] (5) In the above method of the present invention, it is preferred that the oxygen concentration of the oxygen-enriched air introduced into the above raw material loading layer exceeds 25 vol.%.
[0028] Effects of the Invention
[0029] According to the method of the present invention with the above structure, first, the effect of oxygen enrichment is improved, and the strength of the sintered ore can be improved. In this regard, the operation of oxygen enrichment of the raw material loading layer based on the prior art is a method of helping the upper part of the sintering bed (sintering raw material layer) to burn coke at an earlier time (just after ignition) or a technology of filling the circulating exhaust gas. Therefore, although it is effective for improving the yield rate, it is not expected to improve the strength. In contrast, in the case of the method of the present invention, since it is a method of oxygen enrichment treatment of the middle and lower parts of the sintering bed (raw material loading layer), it will not lead to a decrease in the yield rate (productivity), and can greatly improve the overall strength of the finished product (sintered ore). In particular, in the method of the present invention, since it is a suitable oxygen enrichment treatment of the middle part of the raw material loading layer, it is possible to alleviate excessive heat supply, so that the phenomenon of strength reduction can be avoided. That is, in the method of the present invention, since it is possible to achieve effective oxygen enrichment in the middle part of the raw material loading layer, the effect of improving strength is increased.
[0030] It should be noted that although the oxygen enrichment of the upper layer and / or the oxygen enrichment of the lower layer of the raw material loading layer has a lower effect on improving the strength than the oxygen enrichment of the middle layer, it does not hinder the effect of oxygen enrichment of the middle layer. Therefore, it can be implemented together with the oxygen enrichment of the middle layer as a prerequisite. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a schematic diagram showing the state of the cross section of the raw material loading layer between the ore supply section and the ore discharge section of the raw material loading layer on the DL sintering machine cart. DETAILED DESCRIPTION
[0032] The present invention proposes a method for producing sintered ore by performing oxygen enrichment operation using a downward suction belt (DL) sintering machine, which is basically used to make the effect of oxygen enrichment appear at least when the middle layer of the raw material loading layer is burned. Therefore, in the present invention, the upper surface of the above-mentioned raw material loading layer is first ignited, and then, after a certain period of time, the blowing of oxygen enriched gas is started, which means oxygen enrichment of the middle layer. That is, after ignition, the raw material loading layer on the trolley passes (moves) to the discharge side for a certain period of time, and then oxygen enrichment begins. On the other hand, this oxygen enrichment is completed after only a given time.
[0033] Thus, the present invention is a method for oxygen enrichment by blowing oxygen-enriched gas from above the raw material loading layer on the sintering machine trolley from a given time after ignition. That is, the present invention is characterized in that the following oxygen enrichment treatment is performed and sintering is performed, and the oxygen enrichment treatment is: at a normal sintering machine trolley speed (1.5 to 3.5 m / min), oxygen enrichment is performed by supplying oxygen-enriched gas from a position about 4 minutes after ignition from the upper surface of the raw material loading layer, and the oxygen enrichment is continued for a certain time on the discharge part side.
[0034] The timing of ignition of the upper surface of the raw material loading layer can be determined by measurement with a thermometer or the like, and the timing of passing through the outlet of the ignition furnace can be simply regarded as the timing of ignition.
[0035] When the middle layer of the raw material loading layer is oxygen-enriched by introducing oxygen-enriched gas at the above-mentioned position, whether using oxygen-enriched air obtained by enriching the air obtained by directly sucking external gas with a given concentration of oxygen, or in any case where the exhaust gas of the sintering machine is to be circulated, in order to prevent abnormal combustion in non-target areas due to leakage of enriched oxygen and to achieve reliable oxygen enrichment in designated areas, it is preferred to supply oxygen into the hood using a hood-like cover or the like.
[0036] In the present invention, in order to ensure a given firing time and allow the sintering reaction to proceed sufficiently, the oxygen concentration of the introduced oxygen-enriched air is preferably 21 vol.% or more and 50 vol.% or less. The reason is that if the oxygen concentration after oxygen enrichment exceeds 50 vol.%, the combustion of coke is accelerated and the movement speed of the combustion zone increases, so the high-temperature retention time of the combustion zone in each layer is reduced, and the sintering reaction cannot proceed sufficiently. On the other hand, if the oxygen concentration after oxygen enrichment is less than 21 vol.%, the oxygen concentration is lower than that of ordinary air, and compared with the case of directly sucking external air, the oxygen concentration is reduced, which reduces the sinterability. It is preferably 23 vol.% or more and 50 vol.% or less, and more preferably 25 vol.% or more and 50 vol.% or less.
[0037] Hereinafter, a method for enriching oxygen in the middle layer portion which is preferred and suitable for the present invention was tested, and the results thereof will be described.
[0038] (Test 1)
[0039] In this test, the sintering bed (raw material loading layer) was divided into three equal parts in the height direction (upper layer, middle layer, and lower layer), and oxygen-enriched air was introduced to each position to carry out oxygen enrichment in this way. First, as a basic case, a firing test without oxygen enrichment was carried out (Comparative Example 1), and the firing time (15.5 minutes) that became the basis (baseline) was determined. The time obtained by subtracting 1 minute required for the ignition operation from the firing time was divided into three equal parts, and the time obtained was used as the oxygen enrichment time (following formula).
[0040] Oxygen enrichment time = (basic sintering time - 1) / 3
[0041] In addition, in this test, as a sintering raw material, a sintering blend raw material shown in Table 1 whose basicity (B2) was adjusted to 2.0 was used. Then, while adding water to the sintering blend raw material so that the water content reached 7.5 mass%, granulation was performed by a tumble mixer, and the obtained granules were calcined using a calcining pot. In this calcining test, the wind pressure was set to a constant (6 kPa), and the oxygen concentration of the oxygen-enriched air was set to 30 vol.%.
[0042] [Table 1] (mass %)
[0043]
[0044] The results of the test are shown in Table 2. In this test, since the basic firing time is 15.5 minutes, the oxygen enrichment time for each position is 4.8 minutes. Therefore, the 4.8 minutes of oxygen enrichment were carried out in the upper layer (Comparative Example 2), the middle layer (Inventive Example 1), and the lower layer (Inventive Example 2) of the sintering raw material layer. The results show that the strength (TI strength) of the sintered ore can be improved to the greatest extent when oxygen enrichment is carried out in the middle layer. This means that it is best to carry out oxygen enrichment 5.8 minutes after the start of ignition, that is, between 4.8 minutes after the ignition is completed and the next 4.8 minutes. Finally, considering the oxygen enrichment effect on the upper layer (Comparative Example 2) and the lower layer (Inventive Example 2), it is effective to carry out oxygen enrichment of the sintering bed (sintering raw material layer) at a position closer to the discharge side than the position 4 minutes after ignition.
[0045] It should be noted that, according to the results described in Table 2, although the oxygen enrichment of the lower layer following the middle layer is not as good as that of the middle layer, it can be confirmed that the strength is improved. This means that even if the oxygen enrichment is carried out for 4.8 minutes from 10.6 minutes after the start of ignition (9.6 minutes after the completion of ignition), the effect will not be weakened. That is, the effect of improving the strength brought about by oxygen enrichment of the lower layer of the sintering raw material layer (63.5%-61.6%=1.9) is equivalent to 53% of the effect of improving the strength brought about by oxygen enrichment of the middle layer (65.2%-61.6%=3.6).
[0046] This is considered to be due to the fact that heat becomes excessive in the lower layer, especially in the lower part, and the strength increase brought about by the progress of sintering and the strength reduction caused by overheating offset each other. Therefore, when oxygen enrichment is carried out in the lower layer, it is expected to stop within 2.5 minutes (4.8 minutes × 53%) from 10.6 minutes after the start of ignition (9.6 minutes after the completion of ignition), that is, oxygen enrichment is carried out from the ignition of the upper surface of the raw material loading layer to 13 minutes (10.6 minutes + 2.5 minutes).
[0047] [Table 2]
[0048] Comparative Example 1 Comparative Example 2 Invention Example 1 Invention Example 2 Oxygen-rich locations - Upper part Middle level Lower part Yield rate (%) 70.4 72.0 68.8 66.7 Firing time (min) 15.5 15.2 14.7 14.6 <![CDATA[Productivity (t / h / m 2 )]]> 1.43 1.49 1.48 1.44 TI strength (%) 61.6 62.0 65.2 63.5
[0049] Example
[0050] The example described below verifies the influence of oxygen enrichment time on the middle layer of the sintering raw material layer. The raw material used in this example uses a sintering raw material adjusted to SiO2: 4.9 mass%, basicity: 2.0 (Table 1). While adding water to the sintering raw material in such a way that the water content reaches 7.5 mass%, granulation is carried out by a tumble mixer, and a sintering test is carried out on the obtained granulated sintering raw material using a sintering pot. During the sintering, the wind pressure is set to a constant (6 kPa), and the oxygen concentration of the granulated sintering raw material is adjusted to 30 vol.% and provided for the test. The sintering time of the basis (Comparative Example 1) without oxygen enrichment is 15.5 minutes. In addition, in this test, the timing of oxygen enrichment is set to the period of 5.8 to 10.6 minutes after ignition (middle layer), and the oxygen enrichment time at this time is changed to 0.3 to 4.8 minutes.
[0051] As a result, as shown in Table 3, when the oxygen enrichment time for the middle layer is ensured to be 1.0 minute or more, at least the productivity and the sintered ore strength (TI strength) are greatly improved. It should be noted that there is no particular limitation on the oxygen enrichment time, and as mentioned above, it can be considered that the enrichment time for the middle layer is 4.8 minutes and the enrichment time for the lower layer is 2.5 minutes, which is 53% of the 4.8 minutes, which is a total of 7 minutes, is effective.
[0052] [Table 3]
[0053] Comparative Example 1 Example 1 Example 2 Example 3 Oxygen enrichment time (min) 0 0.3 1 4.8 Yield rate (%) 70.4 69.7 69.7 68.8 Firing time (min) 15.5 15.3 15.1 14.7 <![CDATA[Productivity (t / h / m 2 )]]> 1.43 1.46 1.46 1.48 TI strength (%) 61.6 62.0 63.7 65.2
[0054] Next, the example described below verifies the effect of oxygen concentration during oxygen enrichment treatment on the middle layer of the sintering raw material layer. The raw material used in this example uses a sintering raw material adjusted to SiO2: 4.9 mass%, basicity: 2.0 (Table 1). While adding water to the sintering raw material in a manner that the water content reaches 7.5 mass%, granulation is carried out by a tumble mixer, and a sintering test is carried out on the obtained granulated sintering raw material using a sintering pot. During the sintering, the wind pressure is set to a constant (6 kPa), and oxygen-enriched air adjusted in a manner that the oxygen concentration of the granulated sintering raw material reaches 30 vol.% is used for the test. In this test, oxygen enrichment was carried out 5.8 minutes after the start of ignition, that is, from 4.8 minutes after the completion of ignition to the next 4.8 minutes, as in Example 3. The oxygen concentration during oxygen enrichment was changed in the range of 30 to 40 vol.%. The results show that, as shown in Table 4, the strength is improved before the concentration of the oxygen-enriched air reaches 40 vol.%.
[0055] [Table 4]
[0056] Example 3 Example 6 Example 7 Oxygen enrichment time (min) 4.8 4.8 4.8 Yield rate (%) 68.8 71.7 72.1 Firing time (min) 14.7 14.6 13.9 Productivity (t / h / m2) 1.48 1.56 1.64 Oxygen concentration of oxygen-enriched air (vol.%) 30 35 40 TI strength (%) 65.2 66.9 67.4
[0057] Industrial Applicability
[0058] The above description of the present invention is mainly based on the premise of the operation of the sintering machine without using the gas fuel, but it can also be applied to the case of combining the operation of the sintering machine with using the gas fuel.
Claims
1. A method for producing sintered ore, which is a method for producing sintered ore without using gas fuel in the operation of a sintering machine, the method comprising: The sintering raw materials including iron ore and carbon material are loaded into the raw material supply section on the circulating trolley of the sintering machine to form a raw material loading layer. Then, the carbon material on the upper surface of the raw material loading layer is ignited using an ignition furnace arranged at the downstream side of the raw material supply section. In addition, the gas above the raw material loading layer is sucked by a bellows arranged under the trolley, and the gas is introduced into the raw material loading layer to cause the carbon material in the raw material loading layer to burn in sequence, thereby sintering the raw materials to produce sintered ore, wherein: When oxygen enrichment is performed from above the raw material loading layer on the sintering machine, oxygen enrichment treatment is performed at a position closer to the discharge part than the position of the raw material loading layer when 4 minutes have passed since the upper surface of the raw material loading layer was ignited, and sintering is performed. The upper surface is an upper layer portion that divides the raw material loading layer into three equal parts in the height direction. The time for enriching the raw material loading layer with oxygen is set to be 4 to 13 minutes from the time when the upper surface of the raw material loading layer is ignited.
2. The method for producing sintered ore according to claim 1, wherein: The time for oxygen enrichment of the raw material loading layer is set to 1 to 7 minutes in terms of the passage time of the sintering compound raw material.
3. The method for producing sintered ore according to claim 1 or 2, wherein: Oxygen enrichment did not occur until 4 minutes had passed since the upper surface of the loading layer was ignited.
4. The method for producing sintered ore according to claim 1 or 2, which is not used in combination with an exhaust gas recycling process.
5. The method for producing sintered ore according to claim 1 or 2, wherein: The oxygen concentration of the oxygen-enriched air introduced into the raw material loading layer exceeds 25 vol.%.