Melt-coated lithium metal / lithium alloy composite strip production line
By setting the melt coating composite zone and cooling shaping zone in the metal lithium/lithium alloy composite belt production line, the contact time and temperature between molten metal and metal foil is controlled, and the problem of easy pull-off of metal foil and cooling zone affecting molding quality is solved. , improves the quality and stability of the product.
Patent Information
- Application Number
- CN202110334451.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-03-29
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-03-29
AI Technical Summary
When the existing composite metal belt continuous production equipment is used to produce metal lithium/lithium alloy composite belts, the metal foil is easily pulled out, and the cooling time and temperature of the cooling zone affect the forming quality, resulting in lithium dendrites growth and cracks, affecting energy storage. Equipment security.
A production line of melt-coated metal lithium/lithium alloy composite belt is designed, and the upper control roller and the lower control roller are arranged to form a melt-coated composite zone and a cooling shaping zone. The feeding channel and cold air channel are used to control the molten metal and metal foil. Contact time and temperature, the surface tension of metal lithium or lithium alloy is destroyed by melt coating composite rollers, and the cooling medium is used to shape it in the cooling setting zone.
It effectively avoids the metal foil being pulled out, improves the stability of the production equipment and the quality of the metal lithium/lithium alloy composite belt, and ensures the tensile strength of the product and the defect-free molding.
Smart Images

Figure CN115138825B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a metal strip production equipment, in particular to a melt-coated metal lithium / lithium alloy composite strip production line. Background Art
[0002] A Chinese patent application with publication number CN111822662A discloses a continuous production device for composite metal strips, comprising: an unwinding mechanism: for continuously unwinding a substrate; an extrusion molding device: for extruding a metal layer on at least one side of the substrate and obtaining a composite metal strip; a winding mechanism: for winding the prepared composite metal strip; the extrusion molding device comprises an extrusion roller group, the extrusion roller group comprises two extrusion rollers whose axes are parallel to each other; a feeding device for adding molten metal material is provided on the feed side of the two extrusion rollers; a high-temperature zone for keeping the molten metal material in a molten state is provided on the feed side of the extrusion roller group, and a cooling zone for cooling and shaping the composite metal strip is provided on the discharge side of the extrusion roller group; a guide mechanism for allowing the substrate to pass through between the two extrusion rollers is provided between the unwinding mechanism and the winding mechanism.
[0003] Although the composite metal strip continuous production equipment can meet the continuous production requirements of the composite metal strip to a certain extent, it still has the following problems when used to produce metal lithium / lithium alloy composite strips:
[0004] 1. Lithium metal / lithium alloy composite tape is generally used as the electrode of energy storage equipment, and its thickness is strictly controlled; specifically, the thickness of metal foil is generally 6um, and the melting point of lithium metal is 180℃. To achieve the technical purpose of making molten lithium metal or molten lithium alloy flow through two extrusion rollers, the molten lithium metal or molten lithium alloy must have a certain fluidity, and its temperature must be at least 200℃. The molten lithium metal or lithium alloy is in contact with the metal foil for a long time, which causes the metal foil to heat up and reduce its tensile strength. In addition, in the continuous production equipment of the composite metal tape, the tension of the metal foil when passing through the two extrusion rollers is relatively large, which can easily break the metal foil, resulting in production interruption;
[0005] 2. The cooling time and cooling temperature in the cooling zone affect the forming quality of the metal lithium / lithium alloy composite belt. In the continuous production equipment of the composite metal belt, if the cooling time of the metal lithium / lithium alloy composite belt in the cooling zone is too long, cracks will be generated in the metal lithium layer or the lithium alloy layer. The existence of cracks will easily lead to the growth of lithium dendrites, affecting the safety of the energy storage equipment.
[0006] 3. The molten lithium metal or molten lithium alloy droplets have a strong surface tension. It is impossible to coat the molten lithium metal or molten lithium alloy onto the metal foil simply by using an extrusion roller, that is, the quality of the produced lithium metal / lithium alloy composite strip cannot be guaranteed. Summary of the invention
[0007] In view of this, the object of the present invention is to provide a melt-coated metal lithium / lithium alloy composite strip production line, which can prevent the metal foil from being broken and improve the stability of the equipment.
[0008] In order to achieve the above object, the present invention provides the following technical solutions:
[0009] A production line for melt-coated lithium metal / lithium alloy composite strips, comprising:
[0010] Unwinding mechanism, used for continuously unwinding metal foil;
[0011] A melt coating composite forming device is used to melt-coat and composite a metal lithium layer or a lithium alloy layer on a metal foil to obtain a metal lithium / lithium alloy composite strip;
[0012] A winding mechanism, used for winding the prepared metal lithium / lithium alloy composite strip;
[0013] The melt-coating composite forming device comprises an upper control roller and a lower control roller which are arranged correspondingly and respectively located at the upper and lower sides of the metal foil material, wherein a feeding device is provided at the front side of the upper control roller and a cooling zone is provided at the rear side for cooling and shaping the metal lithium / lithium alloy composite strip;
[0014] The feeding device includes a feeding channel, and the feeding channel includes a front inner baffle plate arranged close to the metal foil and a front outer baffle plate located on the side of the front inner baffle plate facing away from the metal foil. A melt-coating composite zone is formed between the feeding channel, the metal foil and the upper control roller. A melt-coating composite roller is provided in the melt-coating composite zone for destroying the surface tension of molten lithium metal or molten lithium alloy and compounding the molten lithium metal or molten lithium alloy with the metal foil.
[0015] Furthermore, a cold air channel is provided in the cooling zone, and the cold air channel includes a rear inner baffle plate arranged close to the metal foil and a rear outer baffle plate located on the side of the rear inner baffle plate facing away from the metal foil. A cooling and molding zone is formed between the cold air channel and the metal lithium / lithium alloy composite strip and the upper control roller. The cooling medium blown in through the cold air channel reaches the cooling and molding zone and cools and molds the metal lithium / lithium alloy composite strip.
[0016] Furthermore, the lower control roller is fixedly installed, and the upper control roller can move relative to the lower control roller and adjust the distance between the upper control roller and the lower control roller.
[0017] Furthermore, a pressure roller is provided below the metal foil material and corresponding to the melt-coated composite roller, and the distance between the melt-coated composite roller and the metal foil material is adjustable.
[0018] Furthermore, the melt-coated composite roller is a brush roller or a scraper roller.
[0019] Furthermore, an overflow trough is provided in the feeding channel, and an overflow port is provided in the overflow trough for allowing the molten metal lithium or the molten lithium alloy to overflow onto the melt-coated composite roller.
[0020] Furthermore, a guide plate extending into the cooling and molding area is provided in the cold air channel, and the guide plate divides the cold air channel into an air inlet channel and an air outlet channel, and the air inlet channel and the air outlet channel are connected through the cooling and molding area.
[0021] Furthermore, it also includes a control roller heating device for heating the upper control roller; the control roller heating device uses a heating element arranged in the upper control roller; or, the control roller heating device uses an eddy current heating device or a radiation heating device for heating the surface of the upper control roller, and the control roller heating device is arranged between the front outer baffle and the rear outer baffle.
[0022] Furthermore, the front side of the melt-coated composite zone is provided with a front tension balancing roller group for applying a friction force to balance the tension of the metal foil, and the rear side of the cooling and shaping zone is provided with a rear tension balancing roller group for applying a friction force to balance the tension of the metal lithium / lithium alloy composite strip.
[0023] Furthermore, a front drive roller is provided in front of the front tension balancing roller group, and a rear drive roller is provided behind the rear tension balancing roller group. A transmission belt is provided between the front drive roller and the rear drive roller, and the metal foil and the metal lithium / lithium alloy composite belt move forward under the action of the transmission belt.
[0024] Furthermore, at least one thickness control section for controlling the thickness of the metal lithium layer or the lithium alloy layer is provided between the cooling and forming section and the winding mechanism, and the thickness control section includes a thickness control area, and the thickness control area is provided with an upper thickness control roller and a lower thickness control roller respectively located on the upper and lower sides of the metal lithium / lithium alloy composite strip;
[0025] The thickness control zone is divided into a first temperature zone located above and a second temperature zone located below with the metal lithium / lithium alloy composite belt as the interface; the first temperature zone is set as a high temperature zone and the second temperature zone is set as a low temperature zone, the temperature in the high temperature zone is higher than the temperature in the low temperature zone, and a roller heating device for heating the upper thickness control roller is provided in the high temperature zone.
[0026] Furthermore, the roller heating device adopts a heating element arranged in the upper thickness control roller; or, the roller heating device adopts an eddy current heating device or a radiation heating device for heating the surface of the upper thickness control roller, and a rolling insulation plate is provided between the roller heating device and the metal lithium / lithium alloy composite strip.
[0027] Furthermore, the thickness control section also includes a temperature control transition zone located in front of the thickness control zone.
[0028] Furthermore, a heat preservation section is provided between the thickness control section and the cooling and shaping area.
[0029] Furthermore, a finishing section for finishing the metal lithium / lithium alloy composite strip is provided between the thickness control section and the winding mechanism.
[0030] Furthermore, at least one finishing zone is provided in the finishing section, and finishing rollers are provided in the finishing zone respectively located on both sides of the metal lithium / lithium alloy composite belt, and finishing heating devices are also provided in the finishing zone respectively located on both sides of the metal lithium / lithium alloy composite belt and used to heat the corresponding finishing rollers.
[0031] Furthermore, the finishing roller in the finishing zone at the rear end is a surface finishing roller used to control the surface finish of the metal lithium / lithium alloy composite strip.
[0032] Furthermore, the finishing heating device adopts a heating element arranged in the finishing roller; or, the finishing heating device adopts an eddy current heating device or a radiation heating device for heating the surface of the finishing roller, and a finishing insulation plate is provided between the finishing heating device and the metal lithium / lithium alloy composite strip.
[0033] Furthermore, a tempering section for eliminating the internal stress of the metal lithium / lithium alloy composite strip is provided between the finishing section and the winding mechanism.
[0034] Furthermore, a covering film laminating mechanism for laminating covering films on both side edges of the metal foil is provided between the unwinding mechanism and the feeding channel.
[0035] Furthermore, a covering film winding mechanism is provided in front of the winding mechanism, and the covering film winding mechanism comprises a knife roller, and a cutting knife facing the inner edge of the covering film is provided on the knife roller.
[0036] Furthermore, a film laminating mechanism for laminating covering strips at intervals on the metal foil is provided between the unwinding mechanism and the feeding channel; or, a covering film laminating mechanism for laminating a covering film on the metal foil and a covering film winding mechanism for peeling the covering film off the metal foil so that the covering strips arranged at intervals on the covering film are adhered to the metal foil are provided between the unwinding mechanism and the feeding channel.
[0037] Furthermore, a brush roller mechanism for brushing molten metal lithium or molten lithium alloy on the metal foil is provided between the unwinding mechanism and the feeding channel.
[0038] Furthermore, a membrane winding composite mechanism for compositely winding a membrane on the surface of the metal lithium / lithium alloy composite belt is provided in front of the winding mechanism.
[0039] Furthermore, the front sides of the two upper control rollers and the lower control roller are provided with clamping mechanisms respectively used to clamp the edges of both ends of the metal foil, and the clamping mechanism includes a clamping groove, and a sealing strip is provided between the upper side wall of the clamping groove and the metal foil.
[0040] Furthermore, the clamping mechanism includes an upper clamping plate and a lower clamping plate, the clamping groove is formed between the upper clamping plate and the lower clamping plate, and a clamping adjustment mechanism for controlling the clamping force between the sealing strip and the metal foil is provided between the upper clamping plate and the lower clamping plate.
[0041] Furthermore, a side surface of the upper clamping plate close to the upper control roller is configured as an arc surface matching the upper control roller.
[0042] The beneficial effects of the present invention are:
[0043] The melt-coated metal lithium / lithium alloy composite belt production line of the present invention provides a feeding device on the front side of the upper control roller, provides a feeding channel in the feeding device, and forms a melt-coated composite zone between the feeding channel, the metal foil and the upper control roller. The front inner baffle plate can prevent the molten metal lithium or the molten lithium alloy from directly contacting the metal foil, so that the molten metal lithium or the molten lithium alloy contacts the metal foil only in the melt-coated composite zone, thereby reducing the contact time between the metal foil and the high-temperature molten metal lithium or the molten lithium alloy, so as to avoid the problem of the metal foil being broken due to the decrease of tensile strength due to the long-term contact between the metal foil and the molten metal lithium or the molten lithium alloy; the melt-coated composite roller is provided to destroy the surface tension of the molten metal lithium or the molten lithium alloy, so that the molten metal lithium or the molten lithium alloy can be better coated on the metal foil, thereby improving the production quality of the metal lithium / lithium alloy composite belt.
[0044] By arranging a cold air channel on the rear side of the upper control roller and forming a cooling and shaping zone between the cold air channel, the metal lithium / lithium alloy composite strip and the upper control roller, the cooling medium contacts the metal lithium / lithium alloy composite strip only in the cooling and shaping zone to cool it down and shape it, thereby being able to control the cooling and shaping temperature and time of the metal lithium / lithium alloy composite strip, avoiding defects such as cracks in the metal lithium layer or the lithium alloy layer, and improving product quality.
[0045] By arranging a front tension balancing roller group on the front side of the melt-coating composite zone, the tension balancing roller group applies friction force to the metal foil and is used to balance the tension required for unwinding the metal foil; by arranging a rear tension balancing roller group on the rear side of the cooling and shaping zone, the rear tension balancing roller group applies friction force to the metal foil and is used to balance the tension required for subsequent winding of the metal lithium / lithium alloy composite strip; in this way, the tension of the metal foil and the metal lithium / lithium alloy composite strip between the front tension balancing roller group and the rear tension balancing roller group can be reduced, thereby preventing the metal foil from being broken.
[0046] By providing a front drive roller and a rear drive roller, and providing a drive belt between the front drive roller and the rear drive roller, and utilizing the drive belt to drive the metal foil and the shaped metal lithium / lithium alloy composite belt to move, the tension requirement for the metal foil and the metal lithium / lithium alloy composite belt can be further reduced, thereby preventing the metal foil from being broken. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] In order to make the purpose, technical solution and beneficial effects of the present invention clearer, the present invention provides the following drawings for illustration:
[0048] Figure 1 It is a structural schematic diagram of an embodiment of a production line for melt-coated lithium metal / lithium alloy composite strips of the present invention;
[0049] Figure 2 for Figure 1 Detailed drawing A;
[0050] Figure 3 It is the structural schematic diagram of the thickness control section;
[0051] Figure 4 It is a structural schematic diagram of the finishing section;
[0052] Figure 5 It is a structural schematic diagram when a covering film laminating mechanism is provided;
[0053] Figure 6 It is a schematic diagram of the structure after the masking film is attached to the two side edges of the metal foil;
[0054] Figure 7 It is a structural schematic diagram when a strip sticking mechanism is provided;
[0055] Figure 8 It is a schematic diagram of the structure when a covering film laminating mechanism is provided;
[0056] Fig. 9 It is a schematic diagram of the structure after the masking strips are laminated on the metal foil at intervals;
[0057] Fig.10 It is a structural schematic diagram when a brush roller mechanism is provided;
[0058] Fig.11 It is a structural schematic diagram of the splint mechanism;
[0059] Fig.12 for Fig.11 Left view of;
[0060] Fig.13 This is a schematic structural diagram of Example 2 of the melt-coated metal lithium / lithium alloy composite strip production line of the present invention.
[0061] Description of reference numerals:
[0062] 1-metal foil; 2-metal lithium / lithium alloy composite strip; 3-masking film; 4-masking strip; 5-covering film; 6-rolled diaphragm;
[0063] 10-unwinding mechanism; 11-covering film laminating mechanism; 12-strip laminating mechanism; 13-covering film laminating mechanism; 14-covering film rewinding mechanism; 15-brush roller mechanism;
[0064] 20-melt coating composite forming device; 21-upper control roller; 22-lower control roller; 23-front inner baffle; 24-rear outer baffle; 25-melt coating composite area; 26-melt coating composite roller; 27-rear inner baffle; 28-rear outer baffle; 29-cooling and shaping area; 30-pressure roller; 31-overflow groove; 32-overflow port; 33-guide plate; 34-air inlet channel; 35-air outlet channel; 36-control roller heating device; 37-front tension balancing roller group; 38-rear tension balancing roller group; 37-tension balancing roller group; 39-front transmission roller; 40-rear transmission roller; 41-transmission belt;
[0065] 50-thickness control section; 51-upper thickness control roller; 52-lower thickness control roller; 53-first temperature zone; 54-second temperature zone; 55-roller heating device; 56-rolling insulation board; 57-temperature control transition zone;
[0066] 60-reeling mechanism; 61-covering film reeling mechanism; 62-knife roller; 63-reeling diaphragm composite mechanism; 64-heat preservation section;
[0067] 70-finishing section; 71-finishing roller; 72-finishing heating device; 73-finishing heat insulation board;
[0068] 80- clamping plate mechanism; 81- clamping groove; 82- sealing strip; 83- clamping plate; 84- arc surface; 85- pressing adjustment mechanism;
[0069] 90-Tempering section. DETAILED DESCRIPTION
[0070] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0071] Example 1
[0072] like Figure 1 The figure is a schematic diagram of the structure of an embodiment of the molten metal lithium / lithium alloy composite strip production line of the present invention. The molten metal lithium / lithium alloy composite strip production line of this embodiment includes:
[0073] An unwinding mechanism 10, used for continuously unwinding the metal foil material 1;
[0074] The melt coating composite forming device 20 is used to melt-coat and composite a metal lithium layer or a lithium alloy layer on the metal foil 1 to obtain a metal lithium / lithium alloy composite strip 2;
[0075] The winding mechanism 60 is used for winding the prepared metal lithium / lithium alloy composite strip 2.
[0076] The melt coating composite molding device 20 of this embodiment includes an upper control roller 21 and a lower control roller 22 which are correspondingly arranged and respectively located on the upper and lower sides of the metal foil 1. The front side of the upper control roller 21 is provided with a feeding device, and the rear side is provided with a cooling zone for cooling and shaping the metal lithium / lithium alloy composite strip 2.
[0077] The feeding device of this embodiment includes a feeding channel, which includes a front inner baffle 23 arranged close to the metal foil 1 and a front outer baffle 24 located on the side of the front inner baffle 23 facing away from the metal foil 1. A melt-coating composite area 25 is formed between the feeding channel, the metal foil 1 and the upper control roller 23. A melt-coating composite roller 26 is provided in the melt-coating composite area 25 for destroying the surface tension of the molten lithium metal or the molten lithium alloy and compounding the molten lithium metal or the molten lithium alloy with the metal foil 1.
[0078] like Figure 2 As shown, a cold air channel is provided in the cooling zone of the present embodiment, and the cold air channel includes a rear inner baffle 27 arranged near the metal foil and a rear outer baffle 28 located on the side of the rear inner baffle 27 facing away from the metal foil. A cooling and shaping zone 29 is formed between the cold air channel and the metal lithium / lithium alloy composite strip 2 and the upper control roller 21. The cooling medium blown in through the cold air channel reaches the cooling and shaping zone 29 and cools and shapes the metal lithium / lithium alloy composite strip 2. By arranging a cold air channel on the rear side of the upper control roller and forming a cooling and shaping zone between the cold air channel and the metal lithium / lithium alloy composite strip and the upper control roller, the cooling medium contacts the metal lithium / lithium alloy composite strip only in the cooling and shaping zone to cool and shape it, thereby controlling the temperature and time of cooling and shaping the metal lithium / lithium alloy composite strip, avoiding defects such as cracks in the metal lithium layer or the lithium alloy layer, and improving product quality.
[0079] Specifically, the front inner baffle 23 and the rear inner baffle 27 are made of heat insulation plates, the front outer baffle 24 is made of heat insulation plates or plates made of temperature-resistant materials; the rear outer baffle 28 is made of heat insulation plates or plates made of low-temperature resistant materials. The front inner baffle 23, the front outer baffle 24, the rear inner baffle 27 and the rear outer baffle 28 of this embodiment are all made of heat insulation plates, which can exchange heat with the outside through the side walls of the feeding channel and the cold air channel, thereby avoiding the heating of the metal foil 1 and the cooling of the metal lithium / lithium alloy composite belt 2 for too long. Specifically, the metal foil 1 can be made of copper foil, aluminum foil, steel foil, nickel foil, silver foil or gold foil. The metal foil 1 of this embodiment can be made of copper foil, which will not be repeated.
[0080] Specifically, the lower control roller 22 is fixedly installed, and the upper control roller 21 can move relative to the lower control roller 22 and adjust the distance between the upper control roller 21 and the lower control roller 22, so as to adjust the thickness of the metal lithium layer or lithium alloy layer composited on the metal foil 1. Specifically, the adjustment mechanism for the upper control roller 21 to move relative to the lower control roller 22 can be implemented in various existing ways, which will not be described again.
[0081] Furthermore, a pressure roller 30 is provided below the metal foil 1 in correspondence with the melt-coated composite roller 26, and the distance of the melt-coated composite roller 26 relative to the metal foil 1 is adjustable. The pressure roller 30 is mainly used to balance the pressure exerted by the melt-coated composite roller 26 on the metal foil 1. By setting the distance of the melt-coated composite roller 26 relative to the metal foil 1 to be adjustable, the surface tension of the molten lithium metal or molten lithium alloy can be better destroyed. Furthermore, the melt-coated composite roller 26 adopts a brush roller or a scraper roller. The melt-coated composite roller 26 of this embodiment adopts a brush roller. Those skilled in the art should know that the roller brush of the brush roller should be made of a high temperature resistant material.
[0082] Furthermore, an overflow groove 31 is provided in the feeding channel, and an overflow port 32 is provided in the overflow groove 31 for overflowing the molten metal lithium or molten lithium alloy to the melt-coated composite roller 26. By providing the overflow groove 31, the problem of uneven feeding in the axial direction of the upper control roller 21 can be avoided. At the same time, under the action of the cooling zone on the rear side, three different temperature zones are formed between the feeding channel and the melt-coated composite zone 25, that is, the temperature of the molten metal lithium or molten lithium alloy located above the overflow groove 31 is higher, the temperature of the molten metal lithium or molten lithium alloy located at the rear side of the melt-coated composite roller 25 is lower, and the temperature of the molten metal lithium or molten lithium alloy located between the melt-coated composite roller 26 and the overflow groove 31 is in the middle. In this way, it can be ensured that the molten metal lithium or molten lithium alloy above the overflow groove 31 has sufficient fluidity to overflow to the melt-coated composite roller 26, and the molten metal lithium or molten lithium alloy can be gradually cooled down to increase viscosity, and coated on the metal foil 1 under the action of the melt-coated composite roller 26.
[0083] Furthermore, a guide plate 33 extending into the cooling and shaping area is provided in the cold air channel, and the guide plate 33 divides the cold air channel into an air inlet channel 34 and an air outlet channel 35, and the air inlet channel 34 and the air outlet channel 35 are connected through the cooling and shaping area 29. Specifically, an air inlet channel 34 is formed between the guide plate 33 and the rear outer baffle 28, and an air outlet channel 35 is formed between the guide plate 33 and the rear inner baffle 27 in this embodiment. Of course, those skilled in the art should know that an air outlet channel 35 can also be formed between the guide plate 33 and the rear outer baffle 28, and an air inlet channel 34 can also be formed between the guide plate 33 and the rear inner baffle 27, which will not be repeated. By providing the guide plate 33 for guiding, the air wall effect formed by directly blowing the cooling medium on the metal lithium / lithium alloy composite strip 2 can be avoided, thereby improving the cooling effect.
[0084] Furthermore, the melt-coated metal lithium / lithium alloy composite strip production line of this embodiment further includes a control roller heating device 36 for heating the upper control roller 21; the control roller heating device 36 uses a heating element arranged in the upper control roller; or, the control roller heating device 36 uses an eddy current heating device or a radiation heating device for heating the surface of the upper control roller 21, and the control roller heating device 36 is arranged between the front outer baffle 24 and the rear outer baffle 28. The control roller heating device 36 of this embodiment uses an eddy current heating device for heating the surface of the control roller. By heating the upper control roller 21, the upper control roller 21 can be prevented from cooling the molten metal lithium or molten lithium alloy.
[0085] Furthermore, a front tension balancing roller group 37 is provided on the front side of the melt coating composite zone 25 and is used to apply a friction force to the metal foil 1 to balance its tension, and a rear tension balancing roller group 38 is provided on the rear side of the cooling and shaping zone 29 and is used to apply a friction force to the metal lithium / lithium alloy composite strip 2 to balance its tension. By arranging the front tension balancing roller group on the front side of the melt coating composite zone, the tension balancing roller group applies a friction force to the metal foil and is used to balance the tension required for the unwinding of the metal foil; by arranging the rear tension balancing roller group on the rear side of the cooling and shaping zone, the rear tension balancing roller group applies a friction force to the metal foil and is used to balance the tension required for the subsequent winding of the metal lithium / lithium alloy composite strip; in this way, the tension of the metal foil and the metal lithium / lithium alloy composite strip between the front tension balancing roller group and the rear tension balancing roller group can be reduced, thereby preventing the metal foil from being pulled apart.
[0086] Furthermore, at least one thickness control section 50 is provided between the cooling and forming area and the winding mechanism for controlling the thickness of the metal lithium layer or the lithium alloy layer. Figure 3As shown, the thickness control section 50 includes a thickness control zone, in which an upper thickness control roller 51 and a lower thickness control roller 52 are respectively provided, which are located on the upper and lower sides of the metal lithium / lithium alloy composite strip 2. The thickness control zone of this embodiment is divided into a first temperature zone 53 located at the upper side and a second temperature zone 54 located at the lower side, with the metal lithium / lithium alloy composite strip 2 as the interface; the first temperature zone 53 is set as a high temperature zone, and the second temperature zone 54 is set as a low temperature zone, the temperature in the high temperature zone is higher than the temperature in the low temperature zone, and a roller heating device 55 for heating the upper thickness control roller 51 is provided in the high temperature zone. The roller heating device 55 adopts a heating element provided in the upper thickness control roller; or, the roller heating device 55 adopts an eddy current heating device or a radiation heating device for heating the surface of the upper thickness control roller, and a rolling heat insulation plate 56 is provided between the roller heating device 55 and the metal lithium / lithium alloy composite strip 2. Specifically, the temperature of the first temperature zone 51 is a temperature suitable for plastic deformation of the metal lithium layer and the lithium alloy layer, and the temperature of the second temperature zone 52 is set to be relatively low, so that when the upper thickness control roller 51 and the lower thickness control roller 52 are rolled, only the thickness of the metal lithium layer or the lithium alloy layer located in the first temperature zone 51 will change significantly, and the thickness of the metal lithium layer or the lithium alloy layer located in the second temperature zone 52 will not change or will change slightly without affecting the product quality. The thickness control section 50 of this embodiment is set as one section, and this section of the thickness control section 50 is used to control the thickness of the metal lithium layer or the lithium alloy layer on the upper side of the metal foil 1. Preferably, the thickness control section 50 also includes a temperature control transition zone 57 located in front of the thickness control zone, which is used to achieve the transition of temperature change.
[0087] Furthermore, a heat preservation section 64 is provided between the thickness control section 50 and the cooling and shaping zone 29 to gradually restore the metal lithium / lithium alloy composite strip 2 that has been rapidly cooled in the cooling and shaping zone 29 to a suitable temperature to eliminate internal stress and improve product quality.
[0088] Furthermore, a finishing section 70 for finishing the metal lithium / lithium alloy composite strip 2 is provided between the thickness control section 50 and the winding mechanism 60. Figure 4 As shown, at least one finishing zone is provided in the finishing section 70, and finishing rollers 71 are provided in the finishing zone, which are respectively located on both sides of the metal lithium / lithium alloy composite belt 2, and finishing heating devices 72 are also provided in the finishing zone, which are respectively located on both sides of the metal lithium / lithium alloy composite belt and are used to heat the corresponding finishing rollers. The finishing heating device 72 uses a heating element arranged in the finishing roller; or, the finishing heating device 72 uses an eddy current heating device or a radiation heating device for heating the surface of the finishing roller, and a finishing heat insulation plate 73 is provided between the finishing heating device 72 and the metal lithium / lithium alloy composite belt. Preferably, the finishing roller in the finishing zone at the rear end of this embodiment is a surface finishing roller used to control the surface finish of the metal lithium / lithium alloy composite belt, so as to control the surface roughness of the metal lithium / lithium alloy composite belt and improve the product quality.
[0089] Furthermore, a tempering section 90 for eliminating the internal stress of the metal lithium / lithium alloy composite strip 2 is provided between the finishing section 70 and the winding mechanism 60, so as to eliminate the internal stress, prevent the metal lithium / lithium alloy composite strip from deforming, and improve product quality.
[0090] Furthermore, in order to use the produced metal lithium / lithium alloy composite strip for energy storage devices, it is also necessary to reserve an area for setting the tabs on the metal foil 1. There are many ways to reserve an area for setting the tabs on the metal foil 1, such as:
[0091] The first type: Figure 5 As shown, a covering film laminating mechanism 11 is provided between the unwinding mechanism 10 and the feeding channel for laminating the covering film 3 on both side edges of the metal foil 1. The covering film 3 is used to cover the both side edges of the metal foil 1 to prevent metal lithium or lithium alloy from being coated on both side edges of the metal foil 1, and to reserve both side areas for the tabs. The covering film 3 can be removed when manufacturing the energy storage device, or it can be removed before winding. That is, a covering film winding mechanism 61 is provided in front of the winding mechanism 40 of this embodiment. The covering film winding mechanism 61 includes a knife roller 62, and the knife roller 62 is provided with a cutter facing the inner edge of the covering film 3. Figure 6 , which is a schematic structural diagram after the covering films 3 are attached to the two side edges of the metal foil 1 .
[0092] The second type: a strip pasting mechanism 12 for pasting the covering strip 4 on the metal foil 1 is provided between the unwinding mechanism 10 and the feeding channel, that is, the covering strip 4 is pasted directly on the metal foil 1 at intervals, such as Figure 7 As shown; or, a covering film laminating mechanism 13 for laminating the covering film 5 on the metal foil 1 and a covering film reeling mechanism 14 for peeling the covering film 5 off the metal foil 1 so that the covering strips 4 arranged at intervals on the covering film are attached to the metal foil 1 are provided between the unwinding mechanism 10 and the feeding channel, as shown in FIG. Figure 8 That is, the masking strips 4 are first pasted on the covering film 5 at intervals, and then the covering film 5 is compounded on the metal foil 1 so that the masking strips 4 are pasted on the metal foil 1 at intervals, and then the covering film 5 is removed and the masking strips 4 are left on the metal foil 1. Fig. 9 , which is a schematic diagram of the structure after the covering strips 4 are laminated on the metal foil 1 at intervals.
[0093] Of course, in order to enhance the melting coating effect, a brush roller mechanism 15 for brushing molten lithium metal or molten lithium alloy on the metal foil 1 can also be provided between the unwinding mechanism 10 and the feeding channel, such as Fig.10 After a layer of metal lithium or lithium alloy is pre-coated on the metal foil 1, the metal lithium or lithium alloy is melt-coated by the melt-coating composite molding device 20, so as to improve the bonding performance between the molten metal lithium or molten lithium alloy and the metal foil 1.
[0094] Furthermore, a membrane winding composite mechanism 63 for compositely winding the membrane 6 on the surface of the metal lithium / lithium alloy composite strip is provided in front of the winding mechanism 10 to prevent the metal foil between adjacent winding layers from adhering to the metal lithium layer or lithium alloy layer after winding.
[0095] Furthermore, the front sides of the upper control roller 21 and the lower control roller 22 of this embodiment are provided with clamping plate mechanisms 80 for clamping the edges of both ends of the metal foil material 1. Fig.11 As shown, the clamping mechanism 80 includes a clamping groove 81, and sealing strips 82 are respectively provided between the two side walls of the clamping groove 81 and the metal foil 1. Specifically, the clamping mechanism of this embodiment includes two clamping plates 83, and the clamping groove 81 is formed between the two clamping plates 83, and a clamping adjustment mechanism 85 for controlling the clamping force between the sealing strip 82 and the metal foil 1 is provided between the two clamping plates 83. The clamping adjustment mechanism can be implemented in a variety of existing ways, which will not be repeated. The side surface of the clamping plate 83 of this embodiment close to the upper control roller 21 is set as an arc surface 84 that matches the control roller 21, which can prevent molten metal lithium or molten lithium alloy from flowing out from both ends of the upper control roller 21.
[0096] The melt-coated metal lithium / lithium alloy composite strip production line of this embodiment, by arranging a feeding device on the front side of the upper control roller, arranging a feeding channel in the feeding device, and forming a melt-coated composite zone between the feeding channel, the metal foil and the upper control roller, can prevent the molten metal lithium or the molten lithium alloy from directly contacting the metal foil by using the front inner baffle plate, so that the molten metal lithium or the molten lithium alloy contacts the metal foil only in the melt-coated composite zone, thereby reducing the contact time between the metal foil and the high-temperature molten metal lithium or the molten lithium alloy, so as to avoid the problem of the metal foil being broken due to the decrease of tensile strength due to the long-term contact between the metal foil and the molten metal lithium or the molten lithium alloy; by arranging the melt-coated composite roller, the surface tension of the molten metal lithium or the molten lithium alloy is destroyed, so that the molten metal lithium or the molten lithium alloy can be better coated on the metal foil, thereby improving the production quality of the metal lithium / lithium alloy composite strip.
[0097] Example 2
[0098] like Fig.13 The figure is a schematic diagram of the structure of an embodiment of the molten metal lithium / lithium alloy composite strip production line of the present invention. The molten metal lithium / lithium alloy composite strip production line of this embodiment includes:
[0099] An unwinding mechanism 10, used for continuously unwinding the metal foil material 1;
[0100] The melt coating composite forming device 20 is used to melt-coat and composite a metal lithium layer or a lithium alloy layer on the metal foil 1 to obtain a metal lithium / lithium alloy composite strip 2;
[0101] The winding mechanism 60 is used for winding the prepared metal lithium / lithium alloy composite strip 2.
[0102] The melt coating composite molding device 20 of this embodiment includes an upper control roller 21 and a lower control roller 22 which are correspondingly arranged and respectively located on the upper and lower sides of the metal foil 1. The front side of the upper control roller 21 is provided with a feeding device, and the rear side is provided with a cooling zone for cooling and shaping the metal lithium / lithium alloy composite strip 2.
[0103] The feeding device of this embodiment includes a feeding channel, which includes a front inner baffle 23 arranged close to the metal foil 1 and a front outer baffle 24 located on the side of the front inner baffle 23 facing away from the metal foil 1. A melt-coating composite area 25 is formed between the feeding channel, the metal foil 1 and the upper control roller 23. A melt-coating composite roller 26 is provided in the melt-coating composite area 25 for destroying the surface tension of the molten lithium metal or the molten lithium alloy and compounding the molten lithium metal or the molten lithium alloy with the metal foil 1.
[0104] In the cooling zone of the present embodiment, a cold air channel is provided, and the cold air channel includes a rear inner baffle 27 arranged near the metal foil and a rear outer baffle 28 located on the side of the rear inner baffle 27 facing away from the metal foil. A cooling and shaping zone 29 is formed between the cold air channel and the metal lithium / lithium alloy composite strip 2 and the upper control roller 21. The cooling medium blown in through the cold air channel reaches the cooling and shaping zone 29 and cools and shapes the metal lithium / lithium alloy composite strip 2. By arranging a cold air channel on the rear side of the upper control roller and forming a cooling and shaping zone between the cold air channel and the metal lithium / lithium alloy composite strip and the upper control roller, the cooling medium contacts the metal lithium / lithium alloy composite strip only in the cooling and shaping zone to cool and shape it, thereby controlling the temperature and time of cooling and shaping the metal lithium / lithium alloy composite strip, avoiding defects such as cracks in the metal lithium layer or the lithium alloy layer, and improving product quality.
[0105] Furthermore, a front tension balancing roller group 37 is provided on the front side of the melt coating composite zone 25 and is used to apply a friction force to the metal foil 1 to balance its tension, and a rear tension balancing roller group 38 is provided on the rear side of the cooling and shaping zone 29 and is used to apply a friction force to the metal lithium / lithium alloy composite strip 2 to balance its tension. By arranging the front tension balancing roller group on the front side of the melt coating composite zone, the tension balancing roller group applies a friction force to the metal foil and is used to balance the tension required for the unwinding of the metal foil; by arranging the rear tension balancing roller group on the rear side of the cooling and shaping zone, the rear tension balancing roller group applies a friction force to the metal foil and is used to balance the tension required for the subsequent winding of the metal lithium / lithium alloy composite strip; in this way, the tension of the metal foil and the metal lithium / lithium alloy composite strip between the front tension balancing roller group and the rear tension balancing roller group can be reduced, thereby preventing the metal foil from being pulled apart.
[0106] Furthermore, a front transmission roller 39 is provided in front of the front tension balance roller group 37, and a rear transmission roller 40 is provided behind the rear tension balance roller group 38. A transmission belt 41 is provided between the front transmission roller 39 and the rear transmission roller 40, and the metal foil 1 and the metal lithium / lithium alloy composite belt 2 move forward under the action of the transmission belt 41. By providing the front transmission roller and the rear transmission roller, and providing the transmission belt between the front transmission roller and the rear transmission roller, and using the transmission belt to drive the metal foil and the shaped metal lithium / lithium alloy composite belt to move, the tension required for the metal foil and the metal lithium / lithium alloy composite belt can be further reduced, thereby preventing the metal foil from being broken.
[0107] The other implementations of this embodiment are the same as those of Embodiment 1 and are not described one by one.
[0108] Note: The meaning of "metal lithium / lithium alloy" mentioned herein is "metal lithium" or "lithium alloy". According to the different added raw materials, the melt-coated metal lithium / lithium alloy composite belt production equipment of the present invention can produce "metal lithium composite belt" or "lithium alloy composite belt". The "melt coating" mentioned herein refers to melting metal lithium or lithium alloy and then coating it on the metal foil. The temperature of the molten metal lithium and the molten lithium alloy is between its melting point and boiling point.
[0109] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.
Claims
1. A production line for melt-coated lithium metal / lithium alloy composite strip, characterized in that: include: Unwinding mechanism, used for continuously unwinding metal foil; A melt coating composite forming device is used to melt-coat and composite a metal lithium layer or a lithium alloy layer on a metal foil to obtain a metal lithium / lithium alloy composite strip; A winding mechanism, used for winding the prepared metal lithium / lithium alloy composite strip; The melt-coating composite forming device comprises an upper control roller and a lower control roller which are arranged correspondingly and respectively located at the upper and lower sides of the metal foil material, wherein a feeding device is provided at the front side of the upper control roller and a cooling zone is provided at the rear side for cooling and shaping the metal lithium / lithium alloy composite strip; The feeding device comprises a feeding channel, the feeding channel comprises a front inner baffle plate arranged close to the metal foil and a front outer baffle plate located on the side of the front inner baffle plate facing away from the metal foil, a melt-coating composite zone is formed between the feeding channel, the metal foil and the upper control roller, and a melt-coating composite roller is arranged in the melt-coating composite zone for destroying the surface tension of molten lithium metal or molten lithium alloy and compounding the molten lithium metal or molten lithium alloy with the metal foil; A cold air channel is provided in the cooling zone, and the cold air channel includes a rear inner baffle plate arranged close to the metal foil and a rear outer baffle plate located on the side of the rear inner baffle plate facing away from the metal foil. A cooling and shaping zone is formed between the cold air channel, the metal lithium / lithium alloy composite strip and the upper control roller, and the cooling medium blown in through the cold air channel reaches the cooling and shaping zone to cool and shape the metal lithium / lithium alloy composite strip; The front side of the melt coating composite zone is provided with a front tension balancing roller group for applying a friction force to balance the tension of the metal foil, and the rear side of the cooling and shaping zone is provided with a rear tension balancing roller group for applying a friction force to balance the tension of the metal lithium / lithium alloy composite strip; A front transmission roller is provided in front of the front tension balance roller group, and a rear transmission roller is provided behind the rear tension balance roller group. A transmission belt is provided between the front transmission roller and the rear transmission roller, and the metal foil and the metal lithium / lithium alloy composite belt move forward under the action of the transmission belt. At least one thickness control section is provided between the cooling and forming section and the winding mechanism for controlling the thickness of the metal lithium layer or the lithium alloy layer, and the thickness control section includes a thickness control area, and the thickness control area is provided with an upper thickness control roller and a lower thickness control roller respectively located at the upper and lower sides of the metal lithium / lithium alloy composite strip; The thickness control zone is divided into a first temperature zone located above and a second temperature zone located below with the metal lithium / lithium alloy composite belt as the interface; the first temperature zone is set as a high temperature zone and the second temperature zone is set as a low temperature zone, the temperature in the high temperature zone is higher than the temperature in the low temperature zone, and a roller heating device for heating the upper thickness control roller is provided in the high temperature zone.
2. The production line for melt-coated lithium metal / lithium alloy composite strip according to claim 1, characterized in that: The lower control roller is fixedly installed, and the upper control roller can move relative to the lower control roller and adjust the distance between the upper control roller and the lower control roller.
3. The melt-coated lithium metal / lithium alloy composite strip production line according to claim 1, characterized in that: A pressure roller is provided below the metal foil material and corresponds to the melt-coated composite roller, and the distance between the melt-coated composite roller and the metal foil material is adjustable.
4. The production line for melt-coated lithium metal / lithium alloy composite strip according to claim 2, characterized in that: The melt-coated composite roller is a brush roller or a scraper roller.
5. The melt-coated lithium metal / lithium alloy composite strip production line according to claim 1, characterized in that: An overflow trough is provided in the feeding channel, and an overflow port is provided in the overflow trough for allowing molten metal lithium or molten lithium alloy to overflow onto the melt-coated composite roller.
6. The production line for melt-coated lithium metal / lithium alloy composite strip according to claim 1, characterized in that: The cold air channel is provided with a guide plate extending into the cooling and shaping area, and the guide plate divides the cold air channel into an air inlet channel and an air outlet channel, and the air inlet channel and the air outlet channel are connected through the cooling and shaping area.
7. The production line for melt-coated lithium metal / lithium alloy composite strip according to claim 1, characterized in that: It also includes a control roller heating device for heating the upper control roller; the control roller heating device uses a heating element arranged in the upper control roller; or, the control roller heating device uses an eddy current heating device or a radiation heating device for heating the surface of the upper control roller, and the control roller heating device is arranged between the front outer baffle and the rear outer baffle.
8. The production line for melt-coated lithium metal / lithium alloy composite strip according to claim 1, characterized in that: The roller heating device adopts a heating element arranged in the upper thickness control roller; or, the roller heating device adopts an eddy current heating device or a radiation heating device for heating the surface of the upper thickness control roller, and a rolling insulation plate is provided between the roller heating device and the metal lithium / lithium alloy composite strip.
9. The production line for melt-coated lithium metal / lithium alloy composite strip according to claim 1, characterized in that: The thickness control section also includes a temperature control transition zone located in front of the thickness control zone.
10. The melt-coated lithium metal / lithium alloy composite strip production line according to claim 1, characterized in that: A heat preservation section is also provided between the thickness control section and the cooling and shaping area.
11. The production line for melt-coated lithium metal / lithium alloy composite strip according to claim 1, characterized in that: A finishing section for finishing the metal lithium / lithium alloy composite strip is provided between the thickness control section and the winding mechanism.
12. The melt-coated lithium metal / lithium alloy composite strip production line according to claim 11, characterized in that: At least one finishing zone is provided in the finishing section, and finishing rollers are provided in the finishing zone respectively located on both sides of the metal lithium / lithium alloy composite belt, and finishing heating devices are also provided in the finishing zone respectively located on both sides of the metal lithium / lithium alloy composite belt and used to heat the corresponding finishing rollers.
13. The production line for melt-coated lithium metal / lithium alloy composite strip according to claim 12, characterized in that: The finishing roller in the finishing zone at the rearmost end is a surface finishing roller used to control the surface finish of the metal lithium / lithium alloy composite strip.
14. The production line for melt-coated lithium metal / lithium alloy composite strip according to claim 12, characterized in that: The finishing heating device adopts a heating element arranged in the finishing roller; or, the finishing heating device adopts an eddy current heating device or a radiation heating device for heating the surface of the finishing roller, and a finishing insulation plate is provided between the finishing heating device and the metal lithium / lithium alloy composite strip.
15. The production line for melt-coated lithium metal / lithium alloy composite strip according to claim 11, characterized in that: A tempering section for eliminating the internal stress of the metal lithium / lithium alloy composite strip is provided between the finishing section and the winding mechanism.
16. The production line for melt-coated lithium metal / lithium alloy composite strip according to claim 1, characterized in that: A covering film laminating mechanism for laminating covering films on both side edges of the metal foil is provided between the unwinding mechanism and the feeding channel.
17. The production line for melt-coated lithium metal / lithium alloy composite strip according to claim 16, characterized in that: A covering film winding mechanism is arranged in front of the winding mechanism, and the covering film winding mechanism comprises a knife roller, and a cutting knife facing the inner edge of the covering film is arranged on the knife roller.
18. The production line for melt-coated lithium metal / lithium alloy composite strip according to claim 1, characterized in that: A film laminating mechanism for laminating covering strips at intervals on the metal foil is provided between the unwinding mechanism and the feeding channel; or, a covering film laminating mechanism for laminating covering film on the metal foil and a covering film winding mechanism for peeling the covering film off the metal foil so that the covering strips arranged at intervals on the covering film are attached to the metal foil are provided between the unwinding mechanism and the feeding channel.
19. The production line for melt-coated lithium metal / lithium alloy composite strip according to claim 1, characterized in that: A brush roller mechanism for brushing molten metal lithium or molten lithium alloy on the metal foil is provided between the unwinding mechanism and the feeding channel.
20. The production line for melt-coated lithium metal / lithium alloy composite strip according to claim 1, characterized in that: A membrane winding composite mechanism for compositely winding a membrane on the surface of the metal lithium / lithium alloy composite belt is also provided in front of the winding mechanism.
21. The melt-coated lithium metal / lithium alloy composite strip production line according to claim 1, characterized in that: The front sides of the two upper control rollers and the lower control roller are provided with clamping mechanisms respectively used to clamp the edges of both ends of the metal foil. The clamping mechanism includes a clamping groove, and a sealing strip is provided between the upper side wall of the clamping groove and the metal foil.
22. The melt-coated lithium metal / lithium alloy composite strip production line according to claim 21, characterized in that: The clamping plate mechanism comprises an upper clamping plate and a lower clamping plate, the clamping groove is formed between the upper clamping plate and the lower clamping plate, and a clamping adjustment mechanism for controlling the clamping force between the sealing strip and the metal foil is provided between the upper clamping plate and the lower clamping plate.