A PE wood-plastic wallboard and preparation method thereof
By using polyethylene-methyl acrylate copolymer and diatomite as a binder, combined with silicone surface material and three-layer co-extrusion process, the problem of insufficient bonding performance of PE wood-plastic wallboards is solved and high strength is achieved and weather-resistant PE wood-plastic wall panel products.
Patent Information
- Application Number
- CN202210847018.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-07
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-07-07
AI Technical Summary
Existing PE wood-plastic wall panels are prone to bubbling and delamination when used outdoors, and have insufficient bonding performance. The hot melt adhesive flows unevenly in the co-extrusion channels, leading to product quality problems and increased costs.
Polyethylene-methyl acrylate copolymer is used as the adhesive base material, diatomaceous earth and siloxane are added, and the wall panels are made through a three-layer co-extrusion process to ensure the stable flow and high viscosity of the adhesive in the co-extruder. Strengthen the bond and prevent the adhesive from affecting the performance of the surface material.
It improves the bonding strength and weather resistance of PE wood-plastic wall panels, avoids delamination and bubbling, reduces product costs, and ensures high-quality appearance and performance.
Smart Images

Figure HDA0003734300550000011 
Figure HDA0003734300550000012 
Figure HDA0003734300550000021
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of wood-plastic products, in particular to a PE wood-plastic wallboard and a preparation method thereof. Background Art
[0002] PE (polyethylene) wood plastic wallboard is a product that integrates function and decoration. It can not only decorate the building entity and improve the quality of the application environment, but also give the building good application functions and diverse choices, fully showing the decorative aesthetic effect of wood plastic materials and the building itself. Therefore, the application of PE wood plastic wallboard in the field of outdoor wall decoration has rapidly emerged.
[0003] When PE wood plastic wall panels are used on exterior walls, scaffolding is required during the installation process. If there are quality problems with the product, the repair process will require a lot of manpower and material resources. Existing PE wood plastic wall panels are generally made by bonding the surface layer to the core layer. However, the bonding performance of the co-extruded surface layer material and the core layer material is not good, and the product is prone to bubbling and delamination during outdoor use (such as Figure 1 ), which seriously affects the appearance of the product. The bonding performance of the surface layer and the core layer of the PE wood-plastic wallboard needs to be improved.
[0004] At present, the main way to solve the above problems is to add the binder to the surface material by melt blending, such as introducing esters and maleic anhydride grafted compatibilizers to improve the bonding strength between the co-extruded surface composite material and the core material of the wood-plastic composite material. However, this method has high requirements on the material mixing process. If the mixing is not uniform, it will cause local debonding. In addition, in order to achieve the ideal bonding effect, the amount of binder will be increased during the blending modification, which will increase the cost of the product.
[0005] Commercially available hot melt adhesive products such as EVA hot melt adhesive or EAA hot melt adhesive are prone to uneven flow and unstable discharge in complex co-extrusion flow channels (such as Figure 2 ), so there is no report on using hot melt adhesive as a co-extrusion material to increase adhesion. The prior art still mainly uses the method of blending and modifying the surface material to improve the bonding problem. Summary of the invention
[0006] Based on this, it is necessary to provide a PE wood-plastic wallboard to address the above problems, wherein the adhesive layer makes the base material layer and the surface layer bond tightly, thereby improving the stability and weather resistance of the product.
[0007] A PE wood-plastic wallboard comprises a substrate layer, an adhesive layer and a surface layer which are stacked in sequence; the adhesive layer is made of an adhesive, and the adhesive is made of the following raw materials in parts by weight: 50 to 87 parts of polyethylene-methyl acrylate copolymer, 1 to 3 parts of low-density polyethylene, 5 to 15 parts of petroleum resin, 0 to 28 parts of diatomaceous earth, and 0.1 to 1 part of an antioxidant; the surface layer is made of a surface material containing siloxane.
[0008] In the above-mentioned PE wood-plastic wallboard, the adhesive uses EMA as the base material. Compared with hot melt adhesives such as EVA and EAA, EMA has lower viscosity to metal, which can improve the processing performance of the adhesive in the co-extruder and stably flow in the complex co-extrusion flow channel; at the same time, diatomaceous earth filler is added to the adhesive. Diatomaceous earth has strong water absorption performance, which can absorb moisture entering the adhesive, prevent moisture from breaking the structure of the adhesive, and maintain the performance of the adhesive; moreover, the surface material for making the surface layer contains siloxane components, and the diatomaceous earth in the adhesive contains components such as silicon dioxide, which can improve the bonding strength between the adhesive layer and the surface layer, thereby avoiding the influence of the addition of adhesive to the surface material for blending and modification on the performance of the surface material.
[0009] In one embodiment, the amount of diatomaceous earth used is 6 to 16 parts.
[0010] In one embodiment, the amount of the polyethylene-methyl acrylate copolymer is 71 to 81 parts.
[0011] In one embodiment, the content of methyl acrylate in the ethylene methyl acrylate copolymer is 28-32%, and the melt flow index of the ethylene methyl acrylate copolymer is 2.8-3.2 g / 10 min.
[0012] In one embodiment, the melt flow index of the low-density polyethylene is 3 to 8 g / 10 min.
[0013] In one embodiment, the petroleum resin is C5 petroleum resin.
[0014] In one of the embodiments, the diatomaceous earth has a 300-mesh sieve residue of ≤17.6% and an oil absorption of 105-190 g / 100 g.
[0015] In one embodiment, the antioxidant is selected from: one or two of antioxidant 1010 and antioxidant 168.
[0016] In one embodiment, the preparation method of the binder comprises the following steps: uniformly mixing polyethylene-methyl acrylate copolymer, low-density polyethylene, petroleum resin and antioxidant, blending and melt-extruding, and cooling to obtain the binder.
[0017] In one embodiment, a parallel twin-screw extruder is used for blending and melt extrusion.
[0018] In one embodiment, the temperatures of each section from the hopper to the die are: 80-100°C, 130-150°C, 130-150°C, 140-160°C, 140-160°C, 140-160°C, 160-180°C, 160-180°C, 160-180°C, 170-190°C.
[0019] In one embodiment, the screw speed of the main machine is 200-350 r / min, and the feed screw speed is 10-30 r / min.
[0020] In one embodiment, the substrate layer is made of a base material comprising wood powder and polyethylene.
[0021] The base material in the present invention is a material commonly used in the market for preparing wood powder polyethylene composite boards (such as wood powder / low-density polyethylene composite boards, wood powder / high-density polyethylene composite boards, etc.).
[0022] In one of the embodiments, the surface material is made of the following raw materials in parts by weight: 50-80 parts of high-density polyethylene, 10-25 parts of polyamide, 5-15 parts of anti-scratch agent, 4-12 parts of compatibilizer, 0.1-1 part of antioxidant, and 0.1-1 part of ultraviolet light absorber; the anti-scratch agent is polypropylene grafted with siloxane.
[0023] The above-mentioned surface material adopts an anti-scratch agent with silicone grafted on the polypropylene molecular chain. Even if a large amount of it is added to the surface material, it will not precipitate on the surface of the product. At the same time, it can increase the scratch resistance of the surface material, improve the whitening phenomenon of the product surface after polishing, and the color and texture are natural and soft. Moreover, the anti-scratch agent adopts PP as the main material, which can reduce the toughness of the surface material, effectively improve the phenomenon of burrs after polishing, and improve the appearance of the product.
[0024] In one embodiment, the amount of the high-density polyethylene is 55 to 72 parts. Preferably, the amount of the high-density polyethylene is 55 to 62 parts.
[0025] In one embodiment, the amount of the polyamide is 18 to 25 parts.
[0026] In one embodiment, the amount of the anti-scratch agent is 12 to 15 parts.
[0027] In one embodiment, the melt flow index of the high-density polyethylene is 0.8 to 1.2 g / 10 min.
[0028] In one embodiment, the polyamide is polyamide 6 (ie, nylon 6), and the relative viscosity of the polyamide 6 is 2.85±0.03.
[0029] In one embodiment, the compatibilizer is maleic anhydride grafted high-density polyethylene, the grafting rate is 0.8% to 1.2%, and the melt flow index is 3 to 5 g / 10 min.
[0030] In one embodiment, the antioxidant is selected from: one or two of antioxidant 1010 and antioxidant 168.
[0031] In one embodiment, the ultraviolet light absorber is selected from: one or two of UV-531 and UV-327.
[0032] In one embodiment, the anti-scratch agent is made of the following raw materials in parts by weight: 90-95 parts of polypropylene, 1-4 parts of siloxane, 0.1-0.3 parts of initiator, and 0.1-0.5 parts of antioxidant.
[0033] In one embodiment, the polypropylene is homopolymer polypropylene with a melt flow index of 10 to 14 g / 10 min.
[0034] In one embodiment, the siloxane is selected from: one or two of vinyl trimethoxy silane and vinyl triethoxy silane.
[0035] In one embodiment, the initiator is selected from: one or two of diisopropylbenzene peroxide and 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane.
[0036] In one embodiment, the antioxidant is selected from: one or two of antioxidant 1010 and antioxidant 168.
[0037] In one embodiment, the preparation method of the anti-scratch agent is: siloxane and an initiator are mixed evenly to obtain a mixture A; polypropylene and a second antioxidant are mixed to obtain a mixture B; the mixture A and the mixture B are blended, melt-extruded, and cooled to obtain the anti-scratch agent.
[0038] In one embodiment, the anti-scratch agent is prepared by a parallel twin-screw extruder, a mixture of siloxane and initiator is placed in a side feeding tank, polypropylene is placed in a main feeding hopper, the screw speed of the main machine is 200-350 r / min, and the speed of the feeding screw of the main feeding hopper is 10-30 r / min; the mixed melt is added to the twin-screw extruder by side feeding to mix with the polypropylene melt, and the flow rate of the mixed melt is 0.5-0.8 kg / h.
[0039] In one embodiment, the temperatures of each section from the hopper to the die are: 100-130°C, 150-170°C, 160-180°C, 170-190°C, 180-200°C, 180-200°C, 180-200°C, 180-200°C, 190-200°C, 200-210°C.
[0040] In one embodiment, the preparation method of the surface layer material is: mixing the raw materials evenly, melt-extruding, cooling, and pelletizing to obtain the surface layer material.
[0041] In one embodiment, the melt extrusion step is specifically as follows: placing the mixed raw materials in a feeding hopper of a parallel twin-screw extruder, and blending and melt-extruding the raw materials.
[0042] In one embodiment, the temperatures of each section from the hopper to the die are: 100-130°C, 150-180°C, 180-200°C, 190-210°C, 190-210°C, 190-220°C, 200-220°C, 200-220°C, 200-230°C, 200-230°C.
[0043] In one embodiment, the screw speed of the main machine is 200-350 r / min, and the screw speed of the main feeding hopper is 10-30 r / min.
[0044] The present invention also provides a method for preparing the PE wood-plastic wallboard of the present invention, wherein the PE wood-plastic wallboard is prepared by a three-layer co-extrusion method.
[0045] The PE wood-plastic wallboard is prepared by three-layer co-extrusion. Compared with adding adhesive to the surface material for blending and modification, the three-layer co-extrusion method can ensure that the bonding performance of the adhesive is not interfered by other layers of materials, and the adhesive will not affect the basic performance of the surface material.
[0046] The co-extrusion is carried out by an extruder, the channel of the extruder is made of metal. The adhesive in the PE wood-plastic wall of the present invention has low viscosity to metal, can flow stably in the channel, and has good processing performance.
[0047] In one embodiment, the substrate layer raw material, the adhesive layer raw material and the surface layer raw material are melt-extruded separately, stacked in sequence, pressed and shaped to obtain the PE wood-plastic wallboard.
[0048] In one embodiment, the melt extrusion of the substrate layer raw material is carried out in a conical twin-screw extruder, and the temperatures of each section from the hopper to the confluence core are 190-210°C, 170-190°C, 170-150°C, 160-140°C, and 150-130°C, respectively; the temperatures of the upper zone, lower zone, left zone, and right zone of the front section of the mold are 150-170°C, 150-170°C, 150-170°C, and 150-170°C, respectively; the temperatures of the upper zone, lower zone, left zone, and right zone of the rear section of the mold are 190-220°C, 190-220°C, 190-220°C, and 190-220°C, respectively; the screw speed of the main machine is 10-15r / min, and the speed of the feeding screw of the main feeding hopper is 18-25r / min.
[0049] In one embodiment, the melt extrusion of the bonding layer raw material is carried out in the first single-screw co-extruder, and the temperatures of each section from the hopper to the confluence core are 110-130°C, 140°C-170°C, 180°C-200°C, 180°C-200°C, respectively, and the screw speed of the main machine is 5-8r / min.
[0050] In one embodiment, the surface layer raw material is melt-extruded in a second single-screw co-extruder, and the temperatures of each section from the hopper to the confluence core are 110-130°C, 160°C-180°C, 180°C-200°C, 200°C-220°C, and the main screw speed is 9-14r / min.
[0051] Compared with the prior art, the present invention has the following beneficial effects:
[0052] The PE wood-plastic wallboard of the present invention uses EMA as a base material as an adhesive. Compared with hot melt adhesives such as EVA and EAA, EMA has lower viscosity to metals, which can improve the processing performance of the adhesive in a co-extruder and stably flow in a complex co-extrusion flow channel. At the same time, diatomaceous earth filler is added to the adhesive. Diatomaceous earth has strong water absorption performance and can absorb moisture entering the adhesive to prevent the moisture from breaking the structure of the adhesive and maintain the use performance of the adhesive. Moreover, the surface material for making the surface layer contains siloxane components, and the diatomaceous earth in the adhesive contains components such as silicon dioxide, which can improve the bonding strength between the adhesive layer and the surface layer, thereby avoiding the influence of the surface material performance on the surface material by adding the adhesive to the surface material for blending and modification. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] Figure 1 It is a schematic diagram of the delamination and bubbling phenomenon of the existing PE wood-plastic products mentioned in the background technology after use.
[0054] Figure 2 It is a schematic diagram of the product obtained by uneven extrusion of hot melt adhesive mentioned in the background technology.
[0055] Figure 3 This is the appearance of the product of Example 2 after weather resistance test. DETAILED DESCRIPTION
[0056] For the convenience of understanding the present invention, the preferred embodiments will be given below to describe the present invention in more detail. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0057] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0058] In the following examples and comparative examples, unless otherwise specified, reagents, materials, and equipment are commercially available, and the experimental methods are conventional experimental methods in the art. The following parts are all parts by weight.
[0059] The substrate layers in the following examples and comparative examples are all prepared using commercially available wood powder and high-density polyethylene granules as raw materials, wherein the mass ratio of wood powder to high-density polyethylene is about 65:35.
[0060] Example 1
[0061] A PE wood plastic wallboard includes a base layer, an adhesive layer and a surface layer which are stacked in sequence. The adhesive layer is prepared by using an adhesive having a raw material composition as shown in Table 1, and the surface layer is prepared by using a surface material. The preparation method of the PE wood plastic wallboard is as follows, wherein the weight ratio of the surface material to the adhesive is 93:7.
[0062] (1) Preparation of binder
[0063] Add the raw materials of the adhesive into the mixer and stir for 15 minutes, then add them into the feeding hopper of the parallel twin-screw extruder. Set the temperature of each section of the extruder from the hopper to the die head to be 80℃, 130℃, 150℃, 160℃, 160℃, 160℃, 180℃, 180℃, 180℃, 190℃. The screw speed of the main machine is 230r / min, and the speed of the feeding screw of the main feeding hopper is 12r / min. Then, the materials are blended and melted and extruded through the extruder. The extruded granules are cooled in a water tank, air-dried, and then enter the pelletizer for pelletizing to obtain the bonding layer material.
[0064] (2) Preparation of surface material
[0065] The surface material is prepared from the following raw materials in parts by weight: 72 parts of high-density polyethylene with a melt flow index of 1 g / 10 min, 18 parts of nylon 6 with a relative viscosity of 2.85±0.03, 5 parts of maleic anhydride grafted high-density polyethylene with a grafting rate of 1% and a melt flow index of 4 g / 10 min, 5 parts of anti-scratch agent, 0.5 parts of antioxidant 1010, 0.5 parts of antioxidant 168, and 0.5 parts of ultraviolet light absorber UV-531. Among them, the anti-scratch agent is prepared from the following raw materials in parts by weight: 99 parts of polypropylene (homopolymer polypropylene, melt flow index 12 g / 10 min), 1 part of vinyl trimethoxysiloxane, 0.1 parts of diisopropylbenzene peroxide, and 0.3 parts of antioxidant 1010.
[0066] The preparation method of the anti-scratch agent is as follows: vinyl trimethoxysiloxane and diisopropylbenzene peroxide are added to a liquid mixer and stirred for 15 minutes, and then the uniformly stirred materials are added to the side feed tank of the parallel twin-screw extruder, and polypropylene is added to the main feed hopper. The temperatures of each section of the extruder from the hopper to the die are set to be 100°C, 150°C, 180°C, 190°C, 200°C, 200°C, 200°C, 200°C, 200°C, 210°C. The screw speed of the main machine is 250r / min, and the speed of the feeding screw of the main feed hopper is 18r / min. The siloxane and initiator mixed liquid is added to the twin-screw extruder by a melt pump by side feeding, and the flow rate is set to 0.6kg / h. The materials are blended and melted and extruded through the extruder. The extruded pellets are cooled by conveyor belt wind and then enter the pelletizer for pelletizing and sealed for storage.
[0067] The preparation method of the surface material is as follows: (i) Add the weighed raw materials into a mixer and stir for 15 minutes, then add the evenly stirred materials into the feeding hopper of a parallel twin-screw extruder. (ii) Set the temperature of each section of the extruder from the hopper to the die head to be 110°C, 180°C, 200°C, 200°C, 210°C, 220°C, 220°C, 220°C, 230°C, 230°C. The screw speed of the main machine is 200r / min, and the speed of the feeding screw of the main feeding hopper is 15r / min. The materials are blended and melted and extruded through the extruder. (iii) The extruded pellets are cooled in a water tank, air-dried, and then pelletized in a pelletizer to obtain the obtained pellets.
[0068] (3) Three-layer co-extrusion
[0069] S1. Add the granular material for preparing the substrate layer into the material hopper of the conical twin-screw extruder.
[0070] S2. Add the adhesive to the material hopper of the single screw co-extruder 1, turn on the material drying switch, set the temperature to 80°C, and dry the material for 2 hours. Add the surface material to the material hopper of the single screw co-extruder 2, turn on the material drying switch, set the temperature to 80°C, and dry the material for 2 hours.
[0071] S3. Set the temperature of each section of the conical twin-screw extruder from the hopper to the confluence core to 200℃, 170℃, 160℃, 150℃, 145℃ respectively; the temperature of the four zones of the front section of the mold (up, down, left, and right) are 150℃, 150℃, 150℃, 150℃ respectively; the temperature of the four zones of the rear section of the mold (up, down, left, and right) are 220℃, 220℃, 220℃, 220℃ respectively. The screw speed of the main machine is 12r / min, and the speed of the feeding screw of the main feeding hopper is 18r / min.
[0072] S4. Set the temperatures of each section of the single-screw co-extruder 1 from the hopper to the confluence core to 110°C, 160°C, 200°C, and 200°C, respectively, and the screw speed of the main machine to 6r / min.
[0073] S5. Set the temperatures of each section of the single-screw co-extruder 2 from the hopper to the confluence core to 130°C, 180°C, 200°C, and 210°C, respectively, and the main screw speed to 11r / min.
[0074] S6, start the conical twin-screw extruder, the single screw co-extruder 1 and the single screw co-extruder 2 to perform three-layer co-extrusion. After the extruded product is subjected to the online deep embossing process, it is cut and transported to the cooling and shaping vehicle, and after natural cooling and shaping, the PE wood-plastic co-extruded wallboard semi-finished product can be obtained, and after grinding and fixed-length cutting, the PE wood-plastic wallboard finished product can be obtained.
[0075] Example 2
[0076] A PE wood-plastic wallboard, whose structure and preparation method are basically the same as those of Example 1, except that the binder is replaced with an equal weight of the binder in this embodiment. The composition of the binder raw materials in this embodiment is shown in Table 1.
[0077] Example 3
[0078] A PE wood-plastic wallboard, whose structure and preparation method are basically the same as those of Example 1, except that the binder is replaced with an equal weight of the binder in this embodiment. The composition of the binder raw materials in this embodiment is shown in Table 1.
[0079] Example 4
[0080] A PE wood-plastic wallboard, whose structure and preparation method are basically the same as those of Example 1, except that the binder is replaced with an equal weight of the binder in this embodiment. The composition of the binder raw materials in this embodiment is shown in Table 1.
[0081] Example 5
[0082] A PE wood-plastic wallboard, whose structure and preparation method are basically the same as those of Example 1, except that the binder is replaced with an equal weight of the binder in this embodiment. The composition of the binder raw materials in this embodiment is shown in Table 1.
[0083] Comparative Example 1
[0084] A PE wood plastic wallboard comprises a substrate layer and a surface layer which are stacked in sequence, and does not include an adhesive layer. The preparation method of the PE wood plastic wallboard is as follows.
[0085] (1) Preparation of surface material
[0086] The raw materials and preparation method of the surface layer material are the same as those in Example 1.
[0087] (2) Double-layer co-extrusion
[0088] S1. Add the granular material for preparing the substrate layer into the material hopper of the conical twin-screw extruder.
[0089] S2. Add the surface material into the material hopper of the single-screw co-extruder, turn on the material drying switch, set the temperature to 80°C, and dry the material for 2 hours.
[0090] S3. Set the temperature of each section of the conical twin-screw extruder from the hopper to the confluence core to 200℃, 170℃, 160℃, 150℃, 145℃ respectively; the temperature of the four zones of the front section of the mold (up, down, left, and right) are 150℃, 150℃, 150℃, 150℃ respectively; the temperature of the four zones of the rear section of the mold (up, down, left, and right) are 220℃, 220℃, 220℃, 220℃ respectively. The screw speed of the main machine is 12r / min, and the speed of the feeding screw of the main feeding hopper is 18r / min.
[0091] S4. Set the temperature of each section of the single-screw co-extruder from the hopper to the confluence core to 130℃, 180℃, 200℃, and 210℃ respectively, and the main screw speed to 11r / min.
[0092] S5, start the conical twin-screw extruder and the single-screw co-extruder to perform double-layer co-extrusion. After the extruded product undergoes the online deep embossing process, it is cut and transported to the cooling and shaping vehicle. After natural cooling and shaping, the PE wood-plastic co-extruded wallboard semi-finished product can be obtained. After grinding and fixed-length cutting, the PE wood-plastic wallboard finished product can be obtained.
[0093] Comparative Example 2
[0094] A PE wood-plastic wallboard, whose structure and preparation method are basically the same as those of comparative example 1, except that the surface material in comparative example 1 is replaced by a commercially available surface material, and its raw material components are: 48 parts of HDPE, 15 parts of PP, 30 parts of sarling resin, 7 parts of EVA, 0.6 parts of antioxidant 1010, and 0.6 parts of antioxidant 168.
[0095] Comparative Example 3
[0096] A PE wood plastic wallboard, the structure and preparation method of which are basically the same as those of Example 1, except that EMA in the binder is replaced by EAA of equal mass. The binder layer is discharged unevenly during the extrusion process, and the product is unqualified.
[0097] Comparative Example 4
[0098] A PE wood-plastic wallboard, whose structure and preparation method are basically the same as those of Example 1, except that no siloxane is added to the surface material.
[0099] Comparative Example 5
[0100] A PE wood plastic wallboard comprises a substrate layer and a surface layer which are stacked in sequence, and does not include an adhesive layer. The preparation method of the PE wood plastic wallboard is as follows.
[0101] (1) Surface material blending modification
[0102] The surface layer material in Example 1 and the adhesive in Example 1 were mixed in a mass ratio of 80:20.
[0103] (2) Double-layer co-extrusion
[0104] The double-layer co-extrusion method is basically the same as that of Comparative Example 1, except that the surface layer material in Comparative Example 1 is replaced by the blended modified surface layer material in S2.
[0105] Table 1 Types and amounts of raw materials of binders in the examples
[0106] Test Project Example 1 Example 2 Example 3 Example 4 Example 5 EMA 81 75 71 65 59 LDPE 3 3 3 3 3 C5 Petroleum Resin 10 10 10 10 10 diatomite 6 12 16 22 28 Antioxidant 1010 0.3 0.3 0.3 0.3 0.3 Antioxidant 168 0.3 0.3 0.3 0.3 0.3
[0107] The weight content of methyl acrylate in EMA is 30%, the melt flow index is 3.0 g / 10 min, the melt flow index of low-density polyethylene is 5 g / 10 min, the 300-mesh sieve residue of diatomaceous earth is 16%, and the oil absorption is 150 g / 100 g.
[0108] Experimental Example 1
[0109] The surface bonding strength test of the PE wood-plastic wallboards of the above embodiments and comparative examples was carried out, and the results are shown in Table 2.
[0110] Table 2 Surface bonding strength results
[0111] project Surface bonding strength / MPa Test Standards GB / T 17657-2016 Example 1 1.16 Example 2 1.27 Example 3 1.13 Example 4 0.92 Example 5 0.82 Comparative Example 1 0.56 Comparative Example 2 0.75 Comparative Example 3 1.02 Comparative Example 4 0.95 Comparative Example 5 1.06
[0112] Experimental Example 2
[0113] The product of Example 2 was subjected to a weather resistance test by boiling it in 5 wt % salt water at 100°C for 240 hours to observe whether the product had surface delamination, bulging, and other undesirable phenomena. Figure 3 As shown, the results show that after the weather resistance test, the surface layer material of the product of Example 2 did not show any debonding phenomenon, and no delamination and bubbling phenomenon occurred.
[0114] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0115] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A PE wood-plastic wallboard, characterized in that: It comprises a substrate layer, an adhesive layer and a surface layer which are stacked in sequence; the adhesive layer is made of an adhesive, and the adhesive is made of the following raw materials in parts by weight: 71-81 parts of polyethylene-methyl acrylate copolymer, 1-3 parts of low-density polyethylene, 10-15 parts of petroleum resin, 6-16 parts of diatomaceous earth, and 0.6-1 part of antioxidant; the weight content of methyl acrylate in the polyethylene-methyl acrylate copolymer is 28-32%; The surface layer is made of a surface material containing siloxane; the surface material is made of the following raw materials in parts by weight: 50-80 parts of high-density polyethylene, 10-25 parts of polyamide, 5-15 parts of anti-scratch agent, 4-12 parts of compatibilizer, 0.1-1 part of antioxidant, and 0.1-1 part of ultraviolet light absorber; the anti-scratch agent is polypropylene grafted with siloxane; the anti-scratch agent is made of the following raw materials in parts by weight: 90-95 parts of polypropylene, 1-4 parts of siloxane, 0.1-0.3 parts of initiator, and 0.1-0.5 parts of antioxidant; The substrate layer is made of a base material comprising wood powder and polyethylene.
2. The PE wood-plastic wallboard according to claim 1, characterized in that: The melt flow index of the polyethylene-methyl acrylate copolymer is 2.8-3.2 g / 10 min; the melt flow index of the low-density polyethylene is 3-8 g / 10 min; the petroleum resin is C5 petroleum resin; the diatomaceous earth sieve residue of 300 mesh is ≤17.6%, and the oil absorption is 105-190 g / 100 g; the antioxidant is selected from: one or two of antioxidant 1010 and antioxidant 168.
3. The PE wood-plastic wallboard according to claim 1 or 2, characterized in that: The preparation method of the binder comprises the following steps: uniformly mixing various raw materials, blending, melting and extruding, and cooling to obtain the binder.
4. The PE wood-plastic wallboard according to claim 3, characterized in that: A parallel twin-screw extruder is used for blending and melt extrusion; the temperatures of each section from the hopper to the die head are: 80-100°C, 130-150°C, 130-150°C, 140-160°C, 140-160°C, 140-160°C, 160-180°C, 160-180°C, 160-180°C, 170-190°C; the screw speed of the main machine is 200-350r / min, and the speed of the feed screw is 10-30r / min.
5. The method for preparing the PE wood-plastic wallboard according to any one of claims 1 to 4, characterized in that: The PE wood-plastic wallboard is manufactured by a three-layer co-extrusion method.
6. The preparation method according to claim 5, characterized in that: The raw materials of the substrate layer, the raw materials of the adhesive layer and the raw materials of the surface layer are melt-extruded respectively, stacked in sequence, pressed and shaped to obtain the PE wood-plastic wallboard.
7. The preparation method according to claim 5, characterized in that: The substrate layer raw material is melt-extruded in a conical twin-screw extruder. The temperatures of the sections from the hopper to the confluence core are 190-210°C, 170-190°C, 170-150°C, 160-140°C, and 150-130°C, respectively. The temperatures of the upper zone, lower zone, left zone, and right zone of the front section of the mold are 150-170°C, 150-170°C, 150-170°C, and 150-170°C, respectively. The temperatures of the upper zone, lower zone, left zone, and right zone of the rear section of the mold are 190-220°C, 190-220°C, 190-220°C, and 190-220°C, respectively. The screw speed of the main machine is 10-15r / min, and the speed of the feeding screw of the main feeding hopper is 18-25r / min. The melt extrusion of the adhesive layer raw material is carried out in the first single screw co-extruder, and the temperatures of each section from the hopper to the confluence core are 110-130°C, 140-170°C, 180-200°C, 180-200°C, and the screw speed of the main machine is 5-8r / min; The surface layer raw material melt extrusion is carried out in the second single-screw co-extruder. The temperatures of each section from the hopper to the confluence core are 110-130°C, 160-180°C, 180-200°C, 200-220°C, and the main screw speed is 9-14r / min.
Citation Information
Patent Citations
Wood-plastic composite board and manufacturing method thereof
CN104070710A
Co-extruded wood-plastic composite material
CN105150644A
High strength wood-plastic coated coextruded composite material and preparation method thereof
CN105644074A
Wood-plastic coextruded fabric
CN106832548A