A copper refining slag depletion method

By using new depleting agents and oxidizing gases for high-temperature smelting reduction during the copper pyrometallurgical smelting process, and using matte for deep depletion, the problem of high copper components in copper refining slag is solved and low-cost, low-temperature The deep depletion and effective utilization of copper resources reduce environmental pollution and waste of copper resources.

CN115141935BActive Publication Date: 2024-10-22NORTHEASTERN UNIV CHINA
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202110331473.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-29
Publication Date
2024-10-22
Estimated Expiration
2041-03-29

AI Technical Summary

Technical Problem

The copper refining slag produced during the pyrometallurgical smelting process of copper sulfide ore and recycled copper contains high copper component, which leads to waste of physical heat, environmental pollution and waste of copper resources. The existing dilution method has heating requirements, high cost, long process and The problem of unusable tailings.

Method used

After the oxidation period of copper fire refining is completed, a new type of composite depletion agent and oxidizing gas are added for high-temperature smelting reduction to deeply deplete the copper refining slag, and copper matte is used for deep depletion to achieve effective reduction and reduction of copper components. Utilizes resources without requiring additional equipment or heating.

Benefits of technology

It achieves low-cost, low-temperature and deep depletion of copper refining slag, reduces the copper content in the slag, improves resource utilization, reduces environmental pollution, simplifies the process, and promotes the effective recovery and economic benefits of copper.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A copper refining slag depletion method belongs to the field of environment, slag metallurgy and comprehensive resource utilization. After the copper pyrometallurgical refining oxidation period is over, the method directly adds a new depletion agent to the copper refining slag in the copper pyrometallurgical refining furnace, or adds the depletion agent and the copper refining slag to a high-temperature furnace, and introduces an oxidizing gas to achieve the reduction of the copper component in the copper refining slag and the deep depletion of the slag. The deep depletion slag is used as a raw material for reducing ironmaking or cement raw material or a raw material for flotation separation of copper. The new depletion agent has the advantages of high specific gravity, controllable reaction, small addition amount, no need for heating, no need for additional equipment, clean, low cost, good depletion effect, etc., and is a composite depletion agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the fields of environment, slag metallurgy and comprehensive utilization of resources, and in particular relates to a copper refining slag depletion method. Background Art

[0002] During the pyrometallurgical smelting of copper sulfide ore and recycled copper, a large amount of copper refining slag is produced, and the copper content in the slag is as high as 45wt%. During the smelting of copper sulfide ore, the copper refining slag is returned to the blowing process for treatment. This method reduces the amount of cold material processed in the blowing process, reduces the efficiency of the enterprise, and causes waste of physical heat in the refining slag. The slag contains high copper, serious smoke leakage, and pollutes the environment. After the copper refining slag produced during the pyrometallurgical smelting of recycled copper is treated by high-temperature furnace depletion, the depleted slag contains more than 1wt% copper, which is much higher than the optional grade of copper ore 0.1wt%, resulting in a waste of copper resources.

[0003] In order to solve the above problems, it is necessary to develop new copper refining slag depletion methods and depletion reagents, which must meet the following requirements: (1) Utilize the physical heat of copper refining slag without heating or with a small amount of heating; (2) Develop a reasonable process route to reduce the copper content in the slag; (3) Develop new depletion reagents to reduce the copper content in the slag; (4) Realize the utilization of the physical heat and iron components of the slag; (5) It should be clean, short in process, low in cost, not affect subsequent production and tailings utilization, and have no solid waste emissions. Summary of the invention

[0004] In view of the problems existing in the prior art, a method for utilizing copper refining slag is provided. After the oxidation period of copper pyrometallurgical refining is completed, the method directly adds a new type of depletion agent to the copper refining slag in the copper pyrometallurgical refining furnace, or adds the depletion agent and the copper refining slag to a high-temperature furnace, and introduces an oxidizing gas to achieve the reduction of the copper component in the copper refining slag and the deep depletion of the slag, and the deep depletion of the slag is used as a raw material for reducing ironmaking or cement raw material or a raw material for flotation separation of copper. The new type of depletion agent has the advantages of high specific gravity, controllable reaction, small addition amount, no need for heating, no need for additional equipment, clean, low cost, good depletion effect, etc., and is a composite depletion agent.

[0005] This method has short reaction time, low copper content in slag, low production cost, short process, large processing volume, environmental friendliness, high economic benefits, and can effectively solve problems such as environmental pollution, efficient utilization of heat energy and resources, and realize the utilization of copper refining slag.

[0006] A method for utilizing copper refining slag of the present invention specifically comprises the following steps:

[0007] A copper refining slag depletion method specifically comprises the following steps:

[0008] Step (1) Reduction and depletion of reagents

[0009] After the oxidation period of copper pyro-refining is over, the depleting agent and the reducing agent are directly added to the copper refining slag in the copper pyro-refining furnace; or the depleting agent, the reducing agent and the copper refining slag are added to a high-temperature furnace for heating; then an oxidizing gas is introduced to perform high-temperature melting reduction depletion, so that the copper oxide in the copper refining slag is reduced to metallic copper, and after sedimentation and depletion, a copper-rich phase and depleted slag are obtained;

[0010] The reduction depletion temperature is 1150-1450°C;

[0011] Step (2) Depletion of slag matte

[0012] Adding matte to the depleted slag in step (1) for deep depletion, so that the residual copper oxide in the slag is converted into metallic copper, which is then precipitated and depleted to obtain a copper-rich phase and deeply depleted slag;

[0013] The specific gravity of the depleted agent is greater than 2.6 g / cm 3 .

[0014] Furthermore, the depletion agent is one or a combination of two or more of ferroalloy, coal-fired slag, coal gangue, fly ash, carbide, coal gasification slag, oil shale, and oil shale slag, or one or more of TiO2, FeO, SiO2, CaCO3, CaO, blast furnace slag, and steel slag is added to a combination of one or more of ferroalloy, coal-fired slag, coal gangue, fly ash, carbide, coal gasification slag, oil shale, and oil shale slag.

[0015] Furthermore, the carbide is one or a combination of two or more of iron carbide, manganese carbide, chromium carbide, titanium carbide, silicon carbide, and vanadium carbide; the ferroalloy is one or a combination of two or more of ferrosilicon, silicon manganese, silicon calcium iron, silicon aluminum iron, silicon calcium aluminum iron, silicon carbon iron, and silicon carbon alloy.

[0016] Furthermore, based on the total amount of copper refined slag being 100wt%, the added amount of the depleted agent is ≤2wt%; and the particle size of the depleted agent is 30μm to 4mm.

[0017] Furthermore, the reducing agent is one or a combination of two or more of diesel, heavy oil, firewood, coal powder, natural gas, and coal gas; based on the total amount of copper refining slag as 100wt%, the amount of reducing agent added is 100wt% of the stoichiometric ratio of copper oxide in the slag to reduce the copper oxide to metallic copper.

[0018] Furthermore, the oxidizing gas is one or a combination of two or more of air, oxygen-enriched air, oxygen, and carbon dioxide.

[0019] Furthermore, the amount of copper matte added is 100wt% of the stoichiometric ratio of the residual copper oxides in the slag converted into metallic copper.

[0020] Furthermore, the sedimentation time in step (1) and step (2) is ≥30 min.

[0021] Furthermore, the copper-rich phase in step (1) is sent to a converting furnace; and the copper-rich phase in step (2) is sent to a copper refining process or a converting process.

[0022] Furthermore, after the high-temperature molten reduction depletion in step (1), the copper content of the slag is ≤2.0wt%; after the deep depletion in step (2), the copper content of the slag is ≤0.3wt%; the slag after the deep depletion is used as molten reduction ironmaking or as cement raw material after water quenching or as raw material for flotation separation of copper after being poured into a slag bag and slowly cooled, and the copper content of the tailings after flotation is ≤0.18wt%.

[0023] Furthermore, the high temperature furnace is an electric furnace, an ore-fired furnace, a reverberatory furnace or a rotary furnace; the matte is in a cold state, a hot state or a molten state, and the molten state comes directly from a copper smelting furnace.

[0024] Principles and advantages of the present invention:

[0025] (1) Principles and advantages of reduction depletion

[0026] Principles and advantages: ① The new depletion agent is a composite agent with a high specific gravity, which is similar to or greater than the specific gravity of the slag. It has a large contact area with the slag, does not float, has a long reaction time, reacts completely, and reduces the copper content in the slag; ② The new depletion agent can provide a composite reducing agent to accelerate the reduction of Cu2O; ③ The new depletion agent can release Cu2O from the silicate phase to a free state, accelerate the reduction, and reduce the copper content in the slag; ④ The reducing agent and the new depletion agent work together to reduce the use of the new depletion agent and reduce costs.

[0027] For example, adding iron carbide to react with Cu2O, FeC+Cu2O=Cu+FeO+CO, Cu2O+CO=Cu+CO2, 2FeO+2Cu2O·SiO2=2Cu2O+2FeO·SiO2

[0028] (2) Principle and advantages of deep depletion of slag by adding copper matte

[0029] Principle: ① The melting point of matte is low, it melts quickly and reacts quickly; ② The Cu2S in matte reacts with the residual Cu2O in the slag, Cu2S+Cu2O=Cu+SO2, generating metallic copper with high specific gravity and low melting point, which accelerates the sedimentation of metallic copper; ③ The FeS in matte makes the sulfur component in the slag excessive, causing the Cu2O and magnetite phase to disappear, thus promoting the sedimentation and flotation separation of the copper component;

[0030] Advantages: ① The product is metallic copper, which has great economic benefits; ② The metallic copper is easy to settle and the slag contains low copper; ③ The melting point of matte is low, no or little heating is required, and the energy consumption is low; ④ The matte can be processed at the same time, which has great benefits; ⑤ The molten matte is directly used without heating. DETAILED DESCRIPTION

[0031] The present invention will be further described below based on a specific embodiment of the present invention. Of course, this embodiment is only a part of the embodiments of the present invention and does not represent all the embodiments of the present invention.

[0032] Example 1

[0033] A copper refining slag impoverishment method and a novel impoverishment agent, specifically comprising the following steps:

[0034] Step (1) Reduction and depletion of reagents

[0035] After the oxidation period of the copper reverberatory refining furnace is over, ferrosilicon powder (specific gravity 3.0 g / cm2) with a particle size of 140-180 μm and an addition amount of 1.3 wt% of the total slag is added. 3 ) and firewood are added to the copper refining slag (the slag contains 27.95wt% copper) in the copper reverberatory refining furnace, and air is introduced to carry out high-temperature melting reduction and depletion. The reduction and depletion temperature is 1230-1300°C, so that the copper oxides in the slag are reduced to metallic copper, and the slag is depleted for 30 minutes to obtain a copper-rich phase and a depleted slag. The copper content of the depleted slag is 1.6wt%, and the molten copper-rich phase is sent to the converter for blowing. The amount of firewood added is 100wt% of the stoichiometric ratio of the copper oxides in the slag to be reduced to metallic copper.

[0036] Step (2) Depletion of slag matte

[0037] Adding molten copper matte to the slag after depletion in step (1) for deep depletion, so that the residual copper oxide in the slag is converted into metallic copper, and the slag is depleted by sedimentation for 30 minutes, and a copper-rich phase and deeply depleted slag are obtained, and the copper content of the deeply depleted slag is 0.28wt%; the molten copper matte comes directly from a copper flash smelting furnace, and the amount of copper matte added is 100wt% of the stoichiometric ratio of the residual copper oxide in the slag converted into metallic copper;

[0038] Example 2

[0039] A copper refining slag impoverishment method and a novel impoverishment agent, specifically comprising the following steps:

[0040] Step (1) Reduction and depletion of reagents

[0041] The particle size is 120-160 μm, and the amount of iron carbide added is 0.8 wt% of the total slag (specific gravity is 7.7 g / cm 3), CaO (specific gravity 3.35 g / cm 3 ), heavy oil and recycled copper refining slag (the slag contains 38.23wt% copper) are added to the electric arc furnace, and air is introduced to carry out high-temperature melting reduction and depletion. The reduction and depletion temperature is 1200-1280°C, so that the copper oxides in the slag are reduced to metallic copper, and the slag is depleted by sedimentation. The depletion time is 40min, and a copper-rich phase and a depleted slag are obtained. The copper content of the depleted slag is 1.5wt%, and the molten copper-rich phase is sent to the converter for blowing; the amount of heavy oil added is 100wt% of the stoichiometric ratio of metallic copper to reduce the copper oxides in the slag.

[0042] Step (2) Depletion of slag matte

[0043] Adding cold copper matte to the slag after depletion in step (1) for deep depletion, so that the residual copper oxide in the slag is converted into metallic copper, and the slag is depleted by sedimentation for 80 minutes, and a copper-rich phase and deeply depleted slag are obtained, and the copper content of the deeply depleted slag is 0.24wt%; the molten copper matte comes directly from the copper side-blown smelting furnace, and the amount of copper matte added is 100wt% of the stoichiometric ratio of the residual copper oxide in the slag converted into metallic copper;

[0044] Example 3

[0045] A copper refining slag impoverishment method and a novel impoverishment agent, specifically comprising the following steps:

[0046] Step (1) Reduction and depletion of reagents

[0047] The coal gangue (specific gravity: 3.0 g / cm2) with a particle size of 100-140 μm and an addition amount of 1.6 wt% of the total slag is added. 3 ), heavy oil and recycled copper refining slag (the slag contains 37.19wt% copper) are added to the electric furnace, and air is introduced to carry out high-temperature melting reduction and depletion. The reduction and depletion temperature is 1220-1290°C, so that the copper oxides in the slag are reduced to metallic copper, and the slag is depleted for 60 minutes to obtain a copper-rich phase and a depleted slag. The copper content of the depleted slag is 1.7wt%. The molten copper-rich phase is sent to the converter for blowing; the amount of heavy oil added is to reduce the copper oxides in the slag to 100wt% of the stoichiometric ratio of metallic copper.

[0048] Step (2) Depletion of slag matte

[0049] Adding cold copper matte to the slag after depletion in step (1) for deep depletion, so that the residual copper oxide in the slag is converted into metallic copper, and the slag is depleted by sedimentation for 80 minutes, and a copper-rich phase and deeply depleted slag are obtained. The deeply depleted slag contains 0.22wt% copper, and the tailings are used as raw materials for ironmaking; the molten copper matte comes directly from a copper low-blowing smelting furnace, and the amount of copper matte added is 100wt% of the stoichiometric ratio of the residual copper oxide in the slag converted into metallic copper;

[0050] Comparative Example 1

[0051] A copper refining slag depletion method and a novel depletion agent are provided, which are the same as those in Example 1, except that: no ferrosilicon powder is added, the reduction is incomplete, the copper content in the slag after depletion in step (1) is 24.19wt%, and after deep depletion in step (2), the copper content in the slag is 1.98wt%, which is much higher than the optional grade of copper ore 0.1wt%, resulting in a waste of copper resources and the tailings cannot be used.

[0052] Comparative Example 2

[0053] A copper refining slag dilution method and a novel dilution agent are provided, which are the same as those in Example 1, except that: the deep dilution of the matte in step (2) is not performed, and after reduction dilution in step (1), the dilution slag contains 1.6wt% copper, which is much higher than the optional grade of copper ore of 0.1wt%, resulting in a waste of copper resources and the tailings cannot be used.

[0054] Comparative Example 3

[0055] A copper refining slag depletion method and a novel depletion agent are the same as those in Example 2, except that: no iron carbide powder is added, the reduction is incomplete, the copper content in the slag after depletion in step (1) is 25.28wt%, and after deep depletion in step (2), the copper content in the slag is 2.89wt%, which is much higher than the optional grade of copper ore 0.1wt%, resulting in a waste of copper resources and the tailings cannot be used.

Claims

1. A method for depleting copper refining slag, characterized in that: The specific steps include: Step (1) Reduction and depletion of reagents After the oxidation period of copper pyro-refining is over, the depletion agent and the reducing agent are directly added to the copper refining slag in the copper pyro-refining furnace; then, an oxidizing gas is introduced to carry out high-temperature melting reduction depletion, so that the copper oxide in the copper refining slag is reduced to metallic copper, and after sedimentation and depletion, a copper-rich phase and depleted slag are obtained; The reduction depletion temperature is 1150-1450°C; Step (2) Depletion of slag matte Adding matte copper to the depleted slag in step (1) for deep depletion, so that the residual copper oxide in the slag is converted into metallic copper, which is then precipitated and depleted to obtain a copper-rich phase and deeply depleted slag; The specific gravity of the depleted agent is greater than 2.6 g / cm 3 ; The depletion agent is one or a combination of two or more selected from ferroalloy, coal-fired slag, coal gangue, fly ash, carbide, coal gasification slag, oil shale, and oil shale slag, or one or a combination of two or more selected from ferroalloy, coal-fired slag, coal gangue, fly ash, carbide, coal gasification slag, oil shale, and oil shale slag is added to a combination of one or more selected from ferroalloy, coal-fired slag, coal gangue, fly ash, carbide, coal gasification slag, oil shale, and oil shale slag, and then one or a combination of two or more selected from TiO2, FeO, SiO2, CaCO3, CaO, blast furnace slag, and steel slag is added; The amount of copper matte added is 100wt% of the stoichiometric ratio of residual copper oxides in the slag converted into metallic copper; Based on the total amount of copper refined slag being 100wt%, the addition amount of the depletion agent is ≤2wt%; the particle size of the depletion agent is 30μm~4mm; After high-temperature molten reduction and depletion in step (1), the slag contains ≤2.0wt% copper; after deep depletion in step (2), the slag contains ≤0.3wt% copper; the slag after deep depletion is used as molten reduction ironmaking or as cement raw material after water quenching or as raw material for flotation separation of copper after being poured into a slag bag and slowly cooled, and the tailings after flotation contain ≤0.18wt% copper.

2. The copper refining slag depletion method according to claim 1, characterized in that: The carbide is one or a combination of two or more of iron carbide, manganese carbide, chromium carbide, titanium carbide, silicon carbide, and vanadium carbide; the ferroalloy is one or a combination of two or more of ferrosilicon, silicon manganese, silicon calcium iron, silicon aluminum iron, silicon calcium aluminum iron, and silicon carbon iron.

3. The copper refining slag depletion method according to claim 1, characterized in that: The reducing agent is one or a combination of two or more of diesel, heavy oil, firewood, coal powder, natural gas, and coal gas; based on the total amount of copper refining slag as 100wt%, the amount of reducing agent added is 100wt% of the stoichiometric ratio of copper oxide in the slag to metallic copper.

4. The copper refining slag depletion method according to claim 1, characterized in that: The oxidizing gas is one or a combination of two or more of air, oxygen-enriched air, oxygen and carbon dioxide.

5. The copper refining slag depletion method according to claim 1, characterized in that: The sedimentation time in step (1) and step (2) is ≥30 min.

6. The copper refining slag depletion method according to claim 1, characterized in that: The matte is in a cold, hot or molten state, and the molten state comes directly from a copper smelting furnace; the copper-rich phase in step (1) is sent to a converting furnace; and the copper-rich phase in step (2) is sent to a copper refining process or a converting process.

Citation Information

Cited By

  • Short-process comprehensive recovery method for copper refining slag

    CN122503641A