A kind of polyimide chopped fiber and preparation method thereof

By modifying the sizing agent and processing technology, the problem of poor length uniformity of polyimide fiber chopped fibers is solved, high-performance chopped fibers are prepared, and the mechanical properties and application value of fiber reinforced materials are improved.

CN115162004BActive Publication Date: 2024-10-29JIANGSU XIANNUO NEW MATERIAL TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210831974.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-15
Publication Date
2024-10-29
Estimated Expiration
2042-07-15

AI Technical Summary

Technical Problem

Polyimide fiber chopped fibers are difficult to cut evenly, resulting in poor length uniformity and affecting the mechanical properties of fiber-reinforced composite materials.

Method used

Modified sizing agents are used to surface treat polyimide fibers, and through clustering and chopped equipment processing, combined with ultrasonic washing and drying processes, chopped fibers with uniform length, uniform diameter and uniform dispersion are prepared.

Benefits of technology

It achieves length uniformity and dispersion of chopped fibers, improves the mechanical properties of fiber-reinforced materials, and is suitable for high and low temperature resistance, flame retardant, ablation resistance and other environments. The process is controllable and easy to be produced in batches or customized.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115162004B_ABST
    Figure CN115162004B_ABST
Patent Text Reader

Abstract

The present invention relates to a polyimide chopped fiber and a preparation method thereof. The prepared chopped fibers have uniform and controllable length, are evenly dispersed, have a length range of 0.2 to 10 mm, and a diameter of 1 to 30 μm, and can be mass-produced or customized. First, a special sizing agent is used to surface treat the polyimide fibers, and then the fibers are processed by a chopped device to obtain polyimide chopped fibers with uniform length. Finally, the sizing agent is removed by a water washing process to obtain the desired polyimide chopped fibers. The polyimide chopped fibers prepared by the method of the present invention have high use value in special fields, especially in environments such as high and low temperature resistance, flame retardancy, ablation resistance, low water absorption, UV resistance, insulation, etc. The method of the present invention is easy to implement and has controllable length, and can be used in rubber, papermaking, resin and other fields to enhance ablation resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high-performance fibers, and in particular to a polyimide fiber and a preparation method thereof. Background Art

[0002] Polyimide (PI) fiber is a type of fiber containing an imide ring structure in the main chain of the molecule. It has excellent comprehensive properties such as high temperature resistance (initial decomposition temperature>520℃), low temperature resistance (-269℃ will not break), solvent resistance, UV radiation resistance, flame retardancy and self-extinguishing, high dimensional stability, high electrical insulation, low dielectric, low creep, and low vacuum volatility. In extreme environments (aerospace, deep-sea operations, disaster relief, national defense and military industries, etc.), it can be used as a reinforcement for reinforced composite materials, and is expected to replace other high-performance fibers and improve the use of reinforced composite materials, lifespan and reliability of material performance.

[0003] The broad application prospects of polyimide fibers have promoted the development boom of polyimide fibers in China, but there are various problems in the application process. For example, the processing method of polyimide fiber reinforced composite materials includes surface treating or modifying the polyimide fibers, and then cutting them into chopped fibers through a chopped machine for melt blending and extrusion of thermoplastic materials. However, since the polyimide fibers are too soft, they are easy to bend when passing through the chopped machine, resulting in the cut fibers being of different lengths. The length uniformity of the chopped fibers will affect the mechanical properties of subsequent products such as fiber-reinforced resin-based composite materials, so this problem affects the application of downstream products of polyimide fibers. In view of this, how to improve the length uniformity of polyimide chopped fibers is an urgent problem to be solved. Summary of the invention

[0004] In view of the problem in the prior art that polyimide chopped fibers are difficult to cut uniformly, resulting in poor length uniformity, the present invention aims to provide a polyimide chopped fibers and a preparation method thereof.

[0005] Another object of the present invention is to provide a polyimide fiber reinforced material, which has better mechanical properties and the like due to the inclusion of the polyimide chopped fibers of the present invention.

[0006] According to the purpose of the present invention, the present invention provides a polyimide chopped short fiber, wherein the target length is any length L in the range of 0.2 mm to 10 mm, 100 fibers are randomly selected, and the percentage of the number of fibers with a length of L±0.5 mm to the total number of fibers is greater than 90%, preferably greater than 95%, and more preferably greater than 99%. In other words, the percentage of ultra-long fibers or ultra-short fibers (exceeding L±0.5 mm) to the total number of fibers does not exceed 10%, preferably does not exceed 5%, and more preferably does not exceed 1%.

[0007] The chopped fibers provided by the present invention have uniform length and uniform dispersion, and have no strand adhesion phenomenon, and therefore can be better applied to downstream products of polyimide fibers, such as polyimide fiber reinforced resin-based composite materials.

[0008] In the present invention, preferably, the target diameter of the polyimide chopped fibers is any diameter d in the range of 1 to 30 μm, preferably any diameter d in the range of 10 to 18 μm, and the effective diameter range is d±3 μm. The effective diameter range refers to the diameter variation range, and the test method is to randomly select 100 chopped fibers, test the diameter under an optical microscope, and calculate the average value. The water absorption rate of the polyimide chopped fibers is less than 1%, and the long-term use temperature is 300°C.

[0009] In the present invention, preferably, the target length of the polyimide chopped fibers is any length L in the range of 0.5 mm to 6 mm.

[0010] On the other hand, the present invention also provides a method for preparing polyimide chopped fibers, which comprises the following steps:

[0011] Step 1: using a sizing agent to perform surface sizing treatment on polyimide fiber filaments to obtain sized polyimide fibers, wherein the sizing agent is selected from one or more of polyvinyl alcohol solution, aqueous polyimide solution, polyacrylate emulsion, epoxy emulsion, polyurethane emulsion, and resorcinol-formaldehyde-latex (RFL emulsion), and a dispersant is added for modification;

[0012] Step 2: Bunching and flattening the sizing polyimide fibers through a bundling device to obtain flattened polyimide fibers;

[0013] Step 3: sending the flattened polyimide fiber to a short-cutting device for processing, cutting it into a target length, and obtaining polyimide short-cut fibers;

[0014] Step 4: Place the obtained polyimide chopped fibers in an ultrasonic washing tank for cleaning to remove the sizing agent, and then place them in an oven for drying.

[0015] The method of the present invention first uses a special sizing agent to surface treat the polyimide fiber, then processes it through a short-cutting device to obtain polyimide short-cut fibers of uniform length, and finally removes the sizing agent through a water washing process to obtain polyimide short-cut fibers of target length. The polyimide short-cut fibers prepared by the method of the present invention have uniform and controllable length, are evenly dispersed, have no doubling adhesion phenomenon, have a length range of 0.2 to 10 mm, a diameter of 1 to 30 μm, and a water absorption rate of less than 1%, which can achieve mass production or customized production. In addition, the polyimide short-cut fibers prepared by the method of the present invention have high use value in special fields, especially in environments such as high and low temperature resistance, flame retardancy, ablation resistance, low water absorption, UV resistance, insulation, etc. The method of the present invention is easy to implement and has controllable length, and can be used in rubber, papermaking, resin and other fields to enhance ablation resistance.

[0016] The sizing agent used in the present invention has the functions of a dispersant and a stiffener after being modified, so that the stiffness of the polyimide fiber can be increased without affecting the dispersibility of the fiber bundle. The polyimide fiber is too soft and is easily bent when passing through a short cut machine, resulting in the cut fibers being of different lengths. Therefore, the modified sizing agent can be used to produce polyimide short cut fiber products of uniform length.

[0017] In the above step 1, if "polyvinyl alcohol solution, aqueous polyimide solution, polyacrylate emulsion, epoxy emulsion, polyurethane emulsion" is called liquid A, then the sizing agent is a mixture of liquid A and a dispersant. The weight percentage concentration of liquid A is 0.1% to 10%, and the solvent used is deionized water. Liquid A mainly plays the role of stiffening the fiber, while the dispersant is a substance with dispersing function, which plays the role of dispersing the fiber. If only liquid A is used in the sizing agent without a dispersant, it will cause adhesion of fibers between fiber bundles, affecting the dispersion performance of the fiber.

[0018] In the present invention, the above liquid A is preferably an aqueous polyimide solution. This is because a low concentration of aqueous polyimide solution can act as a stiffening agent, and the cleaning process is water-soluble; even if the cleaning is not thorough, the temperature resistance remains unchanged after heating and drying.

[0019] In the present invention, the amount of dispersant should be appropriately selected to ensure that the sizing agent can have the functions of both dispersant and stiffener. Preferably, the weight percentage of the dispersant in the sizing agent is 0.1%≤w%≤10%, preferably 0.1%≤w%≤5%. If the amount of dispersant is too large and exceeds the upper limit, it will affect the bundling performance of the fiber and make the subsequent cleaning process difficult; if the amount is too small and below the lower limit, it will not have the desired dispersing effect during use.

[0020] In the present invention, the dispersant is an organic dispersant or an inorganic dispersant. Preferably, the inorganic dispersant is selected from triethylhexyl phosphate, sodium pyrophosphate, sodium lauryl sulfate, polyacrylamide, cellulose derivatives, etc. The above dispersant is preferably an organic dispersant, and more preferably fatty acid polyethylene glycol ester and methyl amyl alcohol. This is because in inorganic dispersants containing phosphorus and sodium, ions have a greater probability of diffusing into the fiber, thereby affecting the bulk properties of the fiber, while organic dispersants such as fatty acid polyethylene glycol ester and methyl amyl alcohol can avoid this problem.

[0021] In the present invention, preferably, the drying temperature is 60° C. to 200° C., and the drying time is 1 min to 120 min.

[0022] According to another object of the present invention, the present invention provides a polyimide fiber reinforced material, which is a polyimide fiber reinforced rubber-based material, a polyimide fiber reinforced paper-based material or a polyimide fiber reinforced resin-based material, and comprises the polyimide chopped fibers of the present invention. The polyimide fiber reinforced material of the present invention can have better mechanical properties, etc. because it comprises the polyimide chopped fibers of the present invention that are uniform in length and uniformly dispersed.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) The chopped fibers prepared by the method of the present invention have uniform and controllable length and are evenly dispersed. The length ranges from 0.2 to 10 mm and the diameter ranges from 1 to 30 μm, and batch production or customized production can be achieved.

[0025] (2) The polyimide chopped fibers prepared by the method of the present invention have high use value in special fields, especially in environments such as high and low temperature resistance, flame retardancy, ablation resistance, low water absorption, UV resistance, and insulation.

[0026] (3) The method of the present invention is easy to implement and has controllable length, and can be used in rubber, papermaking, resin and other fields to enhance ablation resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a photograph of polyimide chopped fibers obtained by the method of Example 1 of the present invention.

[0028] Figure 2 This is an optical microscope photograph of the length of polyimide chopped fibers obtained by the method of Example 1 of the present invention.

[0029] Figure 3 This is an optical microscope photograph of the diameter of polyimide chopped fibers obtained by the method of Example 1 of the present invention. DETAILED DESCRIPTION

[0030] The present invention is further described below in conjunction with specific examples, but the present invention is not limited to the following examples. If the specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially. The polyimide fiber filaments used in the experiment were provided by Jiangsu Xiannuo.

[0031] Example 1

[0032] The polyimide fiber filaments are subjected to surface sizing treatment. The sizing agent is an aqueous polyimide solution. After diluting it with deionized water to a mass fraction of 1%, 0.1% of fatty acid polyethylene glycol ester is added and mixed. Then, the sizing polyimide fibers are bundled and flattened through a bundling device, and the flattened polyimide fibers are sent to a short-cut device for processing to produce short-cut fibers with a target length of 1 mm. The short-cut fibers are ultrasonically cleaned in deionized water for 10 minutes, then pressed dry, and placed in a 120°C oven for drying for 2 hours to obtain polyimide short-cut fiber products.

[0033] Figure 1 is a photograph of polyimide chopped fibers obtained by the method of Example 1; Figure 2 An optical microscope photograph of the length of polyimide chopped fibers obtained by the method of Example 1; Figure 3 This is an optical microscope photograph of the diameter of the polyimide chopped fibers obtained by the method of Example 1.

[0034] Depend on Figure 2 and Figure 3 It can be seen that the length of the obtained polyimide chopped fibers is uniform, all about 1mm, the diameter is 12-15μm, and the dispersion is uniform, without the phenomenon of strand adhesion. It should be noted that each small grid under the microscope is 25μm. For example, the length test in Figure 2 is 36 small grids, with a total length of 900μm. Figure 3 The diameter of the test is 5 grids, totaling 12.5μm. 100 roots are randomly selected, and the percentage of roots with a length of 1mm±0.5mm accounts for 97% of the total number of roots.

[0035] Example 2

[0036] The polyimide fiber filaments are subjected to surface sizing treatment. The sizing agent is an aqueous polyimide solution, which is diluted with deionized water to a mass fraction of 1%, and then 0.5% of fatty acid polyethylene glycol ester is added and mixed. Then, the sizing polyimide fibers are bundled and flattened through a bundling device, and the flattened polyimide fibers are sent to a short-cut device for processing to produce short-cut fibers with a target length of 1 mm. The short-cut fibers are ultrasonically cleaned in deionized water for 10 minutes, then pressed dry, and placed in a 120°C oven for drying for 2 hours to obtain polyimide short-cut fiber products.

[0037] The obtained polyimide chopped fibers have uniform length, all about 1mm, and diameter of 12-15μm, and are evenly dispersed without the phenomenon of strand adhesion. It should be noted that each small grid under the microscope is 25μm, for example: the length of the test in the figure is 45 small grids, with a total length of 1125μm, and the diameter of the test is 6 grids, with a total length of 15μm (not shown in the figure). 100 strands were randomly selected, and the percentage of strands with a length of 1mm±0.5mm accounted for 95% of the total number of strands.

[0038] Example 3

[0039] The polyimide fiber filaments are subjected to surface sizing treatment. The sizing agent is a polyacrylate emulsion, which is diluted with deionized water to a mass fraction of 1%, and then 0.1% of fatty acid polyethylene glycol ester is added and mixed. Then, the sizing polyimide fibers are bundled and flattened through a bundling device, and the flattened polyimide fibers are sent to a short-cut device for processing to produce short-cut fibers with a target length of 1 mm. The short-cut fibers are ultrasonically cleaned in deionized water for 10 minutes, then pressed dry, and placed in a 120°C oven for drying for 2 hours to obtain polyimide short-cut fiber products.

[0040] The obtained polyimide chopped fibers have uniform length, all about 1mm, and diameter of 12-15μm, and are evenly dispersed without the phenomenon of strand adhesion. It should be noted that each small grid under the microscope is 25μm, for example: the length of the test in the figure is 40 small grids, with a total length of 1000μm, and the diameter is tested for 5 grids, with a total length of 12.5μm (not shown in the figure). 100 strands were randomly selected, and the percentage of strands with a length of 1mm±0.5mm accounted for 96% of the total number of strands.

[0041] Comparative Example 1

[0042] The polyimide fiber filaments were subjected to surface sizing treatment, and the sizing agent was an aqueous polyimide solution with a mass fraction of 1%. Then, the sizing polyimide fibers were bundled and flattened by a bundling device, and then the flattened polyimide fibers were sent to a short-cut device for processing to produce short-cut fibers with a target length of 1 mm. The short-cut fibers were ultrasonically cleaned in deionized water for 10 minutes, then pressed dry, and placed in a 120°C oven for 2 hours to obtain a polyimide short-cut fiber product. In the short-cut fiber product, there was a phenomenon of strand adhesion between the fibers, which affected the subsequent normal application, so the length uniformity was not measured.

[0043] Comparative Example 2

[0044] The polyimide fiber filaments were subjected to surface sizing treatment. The sizing agent was an aqueous polyimide solution. After diluting the solution with deionized water to a mass fraction of 1%, 20% of fatty acid polyethylene glycol ester was added and mixed. Then, the sizing polyimide fibers were bundled and flattened by a bundling device, and the flattened polyimide fibers were sent to a short-cut device for processing to produce short-cut fibers with a target length of 1 mm. The short-cut fibers were ultrasonically cleaned in deionized water for 10 minutes, then pressed dry, and dried in an oven at 120°C for 2 hours to obtain a polyimide short-cut fiber product. During the preparation process, the fiber bundling performance was poor. 100 fibers were randomly selected, and the percentage of roots with a length of 1 mm±0.5 mm accounted for 85% of the total number of roots.

[0045] From the comparison between the above embodiments and the comparative examples, it can be seen that the short-cut fibers prepared by the method of the present invention in embodiments 1 to 3 are uniform in length and uniformly dispersed, while no dispersant is added in comparative example 1, so there is a phenomenon of fiber adhesion between the fibers, which affects the subsequent normal application. The dispersant content in comparative example 2 exceeds the upper limit, so during the preparation process, the fiber bundling performance is poor, which affects the length uniformity of the prepared short-cut fibers.

[0046] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing polyimide chopped fibers, It is characterized in that The target length of the polyimide chopped fibers is any length L in the range of 0.5 mm to 10 mm, 100 fibers are randomly selected, and the percentage of fibers with a length of L±0.5 mm to the total number of fibers is greater than 90%, the target diameter of the polyimide chopped fibers is any diameter d in the range of 1 to 30 μm, and the effective diameter range is d±3 μm, The preparation method comprises the following steps: Step 1: using a sizing agent to perform surface sizing treatment on polyimide fiber filaments to obtain sized polyimide fibers, wherein the sizing agent is one or more selected from polyvinyl alcohol solution, aqueous polyimide solution, and polyacrylate emulsion, and the weight percentage concentration is 0.1% to 10%, and a dispersant is added for modification, wherein the dispersant is fatty acid polyethylene glycol ester and / or methyl amyl alcohol, and the weight percentage of the dispersant in the sizing agent is 0.1%≤w%≤10%; Step 2: Bunching and flattening the sizing polyimide fibers through a bundling device to obtain flattened polyimide fibers; Step 3: sending the flattened polyimide fiber to a short-cutting device for processing, cutting it into a target length, and obtaining polyimide short-cut fibers; Step 4: Place the obtained polyimide chopped fibers in an ultrasonic washing tank for cleaning to remove the sizing agent, and then place them in an oven for drying.

2. The preparation method according to claim 1, It is characterized in that The drying temperature is 60°C to 200°C, and the drying time is 1min to 120min.

3. The preparation method according to claim 1, It is characterized in that The target length of the polyimide chopped fibers is any length L between 1 mm and 6 mm, 100 fibers are randomly selected, and the percentage of fibers with a length of L±0.5 mm to the total number of fibers is greater than 95%; and / or The target diameter of the polyimide chopped fibers is any diameter d between 10 and 18 μm, and the effective diameter range is d±3 μm.

4. A polyimide chopped fiber prepared by the preparation method according to any one of claims 1 to 3.

5. A polyimide fiber reinforced material, It is characterized in that It is a polyimide fiber reinforced rubber-based material, a polyimide fiber reinforced paper-based material or a polyimide fiber reinforced resin-based material, and contains the polyimide chopped fibers according to claim 4.

Citation Information

Patent Citations

  • Polyimide ultra-short fiber and preparation method thereof

    CN107675288A

  • Sizing process of polyimide fibers

    CN110295494A