A method for improving the ionic conductivity of solid electrolyte LATP

By doping gallium and silicon in the solid electrolyte LATP, changing its crystal structure and generating LiTiOPO4, the low grain boundary conductivity and brittleness of LATP is solved, significantly improving the migration ability and overall conductivity of lithium ions, and improving battery performance .

CN115172884BActive Publication Date: 2024-11-26GUANGZHOU BOYUE NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210683655.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-17
Publication Date
2024-11-26
Estimated Expiration
2042-06-17

AI Technical Summary

Technical Problem

The solid electrolyte LATP has a low grain boundary conductivity, high electrolyte brittleness, and contacts with the positive and negative electrode materials of the battery to produce a large interface resistance, which affects the performance of lithium-ion batteries.

Method used

Gallium and silicon are used as doping elements to promote the generation of LiTiOPO4 by changing the lattice structure of LATP, reducing the resistance to lithium ion movement and improving grain boundary conductivity, thereby improving ionic conductivity. Specific steps include ball milling, calcining, and sintering after mixing the raw materials to form a high-performance solid electrolyte sheet.

Benefits of technology

It significantly improves the ion conductivity of solid electrolytes, improves the migration ability of lithium ions, enhances the electrochemical performance of the battery, is easy to operate and low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115172884B_ABST
    Figure CN115172884B_ABST
Patent Text Reader

Abstract

The invention discloses a method for improving the ionic conductivity of a solid electrolyte LATP, comprising the following steps: taking required raw materials of lithium carbonate, aluminum oxide, titanium dioxide and ammonium dihydrogen phosphate and doping raw materials of gallium oxide and silicon oxide, mixing them uniformly in a certain atomic ratio, then ball milling, drying and sieving; placing the mixed raw materials in a muffle furnace for calcining to obtain Li 1.35 Al 0.3‑x Ga x Ti 1.7 Si 0.05 P3O 12 (LAGTSP, x = 0.01, 0.03, 0.05) precursor, wherein; the LAGTSP precursor powder obtained after calcination is ball-milled, dried and sieved again; the dried and sieved LAGTSP precursor powder is placed in a mold and pressed into a disc, the disc is placed in a muffle furnace for sintering, and after sintering, it is polished with sandpaper to remove surface residues. The advantage of the scheme provided by the present invention is that the overall ionic conductivity of LATP can be improved only by the synergistic effect of different doping elements, the operation is simple, and the cost is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of solid lithium ion electrolyte materials, and in particular to a method for improving the ionic conductivity of a solid electrolyte LATP. Background Art

[0002] With the rapid development of science and technology and industrial industries, energy issues have gradually been put on the agenda of sustainable development of mankind. In the era of "carbon peak" and "carbon neutrality", the large-scale exploitation and use of traditional fossil energy represented by oil, coal and natural gas have aggravated the energy crisis. Although wind energy, solar energy, tidal energy, biomass energy and geothermal energy are renewable energy sources, they are all decentralized and intermittent, resulting in energy loss. In order to make full use of these energy sources, a good energy storage system is particularly important. Lithium-ion batteries have become the first choice for electrochemical energy storage devices due to their advantages such as high energy density, long cycle life, fast charging and discharging, convenient use and high technical maturity. However, most of the commercial lithium-ion batteries currently use liquid electrolytes, which are prone to dangerous accidents such as combustion and explosion caused by short circuits and leakage. In contrast, solid electrolytes have become a research hotspot due to their advantages such as high chemical stability, non-flammability and high elastic modulus.

[0003] Li 1.3 Al 0.3 Ti 1.7 P3O 12 (LATP) is a material that has been studied more in oxide solid electrolytes. It belongs to the NASICON structure derived from LiTi2 (PO4) 3 (LiTi2 (PO4) 3 is referred to as LTP). By sharing O atoms, TiO6 octahedrons are connected with PO4 tetrahedrons to form a three-dimensional framework. In LTP, due to the Ti 4+ Partly Al 3+ The obtained LATP has a well-structured skeleton, which is beneficial to Li + Among them, LATP (x = 0.3) has the highest ion conductivity, the least impurities, the lowest porosity and the best skeleton size of lithium ion insulators related to aluminum; however, there are still problems such as low grain boundary conductivity, high electrolyte brittleness and large interface resistance in contact with positive and negative electrode materials of the battery.

[0004] As a common method to change the crystal structure of materials, doping plays an important role in the modification of solid electrolytes, such as silicon (Journal of Power Sources, 2009, 189: 371-377). In LATP, it is possible to form a synergistic effect of doping elements and achieve the effect of improving ionic conductivity through co-doping at multiple sites. Summary of the invention

[0005] In view of the above problems, the present invention aims to provide a method for improving the ionic conductivity of the solid electrolyte LATP.

[0006] To achieve the technical purpose, the scheme of the present invention is: a method for improving the ionic conductivity of a solid electrolyte LATP, using gallium and silicon as doping elements to change the lattice of LATP to a certain extent, and promote the formation of LiTiOPO4, thereby reducing the resistance to the movement of lithium ions and improving the grain boundary conductivity, thereby improving the ionic conductivity, comprising the following steps:

[0007] S1: Take the required raw materials of lithium carbonate, aluminum oxide, titanium dioxide and ammonium dihydrogen phosphate and the doping raw materials of gallium oxide and silicon oxide, mix them in proportion, then ball mill, dry and sieve to obtain raw material powder;

[0008] S2: placing the mixed raw material powder into a muffle furnace and calcining it for a specified time to obtain a LAGTSP precursor;

[0009] S3: ball milling, drying and sieving the LAGTSP precursor obtained after calcination again to obtain LAGTSP precursor powder;

[0010] S4: The LAGTSP precursor powder obtained after drying and sieving is placed in a mold and pressed into a thin sheet, and the thin sheet is placed in a muffle furnace for further sintering. After the sintering is completed, the surface impurities are removed by grinding with sandpaper to obtain a solid electrolyte sheet.

[0011] Preferably, in step S1, the atomic ratio of lithium, aluminum, titanium and phosphorus is 1.3:0.3:1.7:3, and the atomic ratio of doping elements gallium and silicon is Ga=0.01, or 0.05 and Si=0.05 respectively.

[0012] Preferably, in step S1, the raw materials are mixed evenly and then ball milled for 8 h, the ball mill speed is 280 r / min, and ethanol is used as a dispersant;

[0013] The raw powder after ball milling was dried in a drying oven at 80 °C for 10 h, ground for 1 h after the ethanol was completely evaporated, and sieved with a 160-mesh fine powder sieve.

[0014] Preferably, in step S2, the raw material powder is calcined at 1200° C. for 2 h.

[0015] Preferably, in step S4, the LAGTSP precursor powder is pressed into a circular sheet with a diameter of 8 mm and a thickness of 2.5 mm at a pressure of 18 MPa for 5 min, and then the sheet is sintered in a muffle furnace at 950°C for 4 h at a heating rate of 5°C / min.

[0016] Preferably, in step S4, the atomic ratio of lithium, aluminum, titanium, phosphorus, gallium and silicon in the raw material is Li:Al:Ti:P:Ga:Si=1.3:0.7:1.7:3:0.03:0.05.

[0017] A solid-state battery comprises a solid-state electrolyte sheet prepared by a method for improving the ionic conductivity of a solid-state electrolyte LATP.

[0018] The beneficial effects of the present invention are as follows: the scheme described in the present application is to find a simple method for improving the ionic conductivity of LATP. The advantage of this design is that the key electrochemical properties of LATP can be improved only by doping, which is simple to operate and low in cost. While keeping the process steps of the LATP solid phase sintering method unchanged, the microscopic crystal structure of LATP is changed by the synergistic effect of different doping elements, and the generation of the second phase LiTiOPO4 is regulated at the same time, the migration of lithium ions in the LATP solid electrolyte is promoted, and the grain boundary conductivity is improved, thereby improving the overall ionic conductivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is the SEM image of Example 1 of the present application;

[0020] Figure 2 This is the SEM image of Example 2 of the present application;

[0021] Figure 3 This is the SEM image of Example 3 of the present application;

[0022] Figure 4 This is a SEM image of a comparative example of the present application;

[0023] Figure 5 This is the AC impedance diagram of Example 1 of the present application;

[0024] Figure 6 This is the AC impedance diagram of Example 2 of the present application;

[0025] Figure 7 This is the AC impedance diagram of Example 3 of the present application;

[0026] Figure 8 This is the AC impedance diagram of the comparative example of this application. DETAILED DESCRIPTION

[0027] The present invention is described in detail through the following specific examples, but the protection scope of the present invention is not limited to these embodiments.

[0028] like Figure 1-8As shown, a method for improving the ionic conductivity of a solid electrolyte LATP is provided, wherein gallium and silicon are used as doping elements to change the lattice of LATP to a certain extent and promote the formation of LiTiOPO4, thereby reducing the resistance to the movement of lithium ions and improving the grain boundary conductivity, thereby improving the ionic conductivity, and comprising the following steps:

[0029] S1: Take the required raw materials of lithium carbonate, aluminum oxide, titanium dioxide and ammonium dihydrogen phosphate and the doping raw materials of gallium oxide and silicon oxide, according to the atomic ratio of lithium, aluminum, titanium and phosphorus of 1.3:0.3:1.7:3, and the atomic ratio of doping elements gallium and silicon is Ga=0.01, or 0.03, or 0.05 and Si=0.05 respectively;

[0030] After the raw materials were evenly mixed, they were ball milled for 8 h at a speed of 280 r / min, and ethanol was used as a dispersant;

[0031] The ball-milled raw powder was dried in a drying oven at 80 °C for 10 h, ground for 1 h after the ethanol was completely evaporated, and sieved with a 160-mesh fine powder sieve;

[0032] S2: calcining the mixed raw material powder at 1200 °C for 2 h to obtain LAGTSP precursor;

[0033] S3: ball milling, drying and sieving the LAGTSP precursor obtained after calcination again to obtain LAGTSP precursor powder;

[0034] S4: The LAGTSP precursor powder was pressed into a circular sheet with a diameter of 8 mm and a thickness of 2.5 mm at a pressure of 18 MPa for 5 min.

[0035] The thin sheet was then placed in a muffle furnace and sintered at 950 °C for 4 h with a heating rate of 5 °C / min. After sintering, the surface impurities were removed by grinding with sandpaper to obtain a solid electrolyte sheet.

[0036] A solid-state battery comprises a solid-state electrolyte sheet prepared by a method for improving the ionic conductivity of a solid-state electrolyte LATP. Example

[0037] The solid electrolyte sheet preparation process of Example 1 is as follows, specifically comprising the following steps:

[0038] Step 1: Take the required raw materials lithium carbonate, aluminum oxide, titanium dioxide and ammonium dihydrogen phosphate and the doping raw materials gallium oxide and silicon oxide, with the atomic ratio being:

[0039] Li:Al:Ti:P:Ga:Si=1.3:0.7:1.7:3:0.01:0.05, after mixing, ball milling, drying and sieving;

[0040] Step 2: Place the mixed raw materials in a muffle furnace and calcine at 1200 °C for 2 h to obtain a LAGTSP (Ga=0.01) precursor;

[0041] Step 3: ball milling, drying and sieving the LATP precursor powder obtained after calcination again;

[0042] Step 4: Place the dried and sieved LAGTSP (Ga=0.01) precursor powder obtained in step 3 into a mold, hold the pressure at 18 MPa for 5 min, press into a disc with a diameter of 8 mm and a thickness of 2.5 mm, and then sinter at 950 ° C in a muffle furnace for 4 h at a heating rate of 5 ° C / min. After sintering, polish with sandpaper to remove surface residues to obtain the solid electrolyte sheet of Example 1. Example

[0043] The preparation process of the solid electrolyte sheet of Example 2 is as follows, and specifically comprises the following steps:

[0044] Step 1: Take the required raw materials lithium carbonate, aluminum oxide, titanium dioxide and ammonium dihydrogen phosphate and the doping raw materials gallium oxide and silicon oxide, with the atomic ratio being:

[0045] Li:Al:Ti:P:Ga:Si=1.3:0.7:1.7:3:0.03:0.05, after mixing, ball milling, drying and sieving;

[0046] Step 2: Place the mixed raw materials in a muffle furnace and calcine at 1200 °C for 2 h to obtain a LAGTSP (Ga=0.03) precursor;

[0047] Step 3: ball milling, drying and sieving the LAGTSP (Ga=0.03) precursor powder obtained after calcination again;

[0048] Step 4: Place the dried and sieved LAGTSP (Ga=0.03) precursor powder obtained in step 3 into a mold, hold the pressure at 18 MPa for 5 min, press into a disc with a diameter of 8 mm and a thickness of 2.5 mm, and then sinter at 950 ° C in a muffle furnace for 4 h at a heating rate of 5 ° C / min. After sintering, polish with sandpaper to remove surface residues to obtain the solid electrolyte sheet of Example 2. Example

[0049] The solid electrolyte sheet preparation process of Example 3 is as follows, specifically comprising the following steps:

[0050] Step 1: Take the required raw materials lithium carbonate, aluminum oxide, titanium dioxide and ammonium dihydrogen phosphate and the doping raw materials gallium oxide and silicon oxide, with the atomic ratio being:

[0051] Li:Al:Ti:P:Ga:Si=1.3:0.7:1.7:3:0.05:0.05, after mixing, ball milling, drying and sieving;

[0052] Step 2: Place the mixed raw materials in a muffle furnace and calcine at 1200 °C for 2 h to obtain a LAGTSP (Ga=0.05) precursor;

[0053] Step 3: ball milling, drying and sieving the LAGTSP (Ga=0.05) precursor powder obtained after calcination again;

[0054] Step 4: Place the dried and sieved LAGTSP (Ga=0.05) precursor powder obtained in step 3 into a mold, hold the pressure at 18 MPa for 5 min, press into a disc with a diameter of 8 mm and a thickness of 2.5 mm, and then sinter at 950°C in a muffle furnace for 4 h at a heating rate of 5°C / min. After sintering, polish with sandpaper to remove surface residues to obtain the solid electrolyte sheet of Example 3.

[0055] Comparative Example

[0056] The solid electrolyte sheet preparation process of the comparative example is as follows, specifically comprising the following steps:

[0057] Step 1: Take the required raw materials lithium carbonate, aluminum oxide, titanium dioxide and ammonium dihydrogen phosphate, with an atomic ratio of Li:Al:Ti:P = 1.3:0.7:1.7:3, mix them, ball mill, dry and sieve;

[0058] Step 2: Place the mixed raw materials in a muffle furnace and calcine at 1200 ° C for 2 h to obtain a LATP precursor;

[0059] Step 3: ball milling, drying and sieving the LATP precursor powder obtained after calcination again;

[0060] Step 4: Place the dried and sieved LATP precursor powder obtained in step 3 into a mold, hold the pressure at 18 MPa for 5 min, press it into a disc with a diameter of 8 mm and a thickness of 2.5 mm, and then sinter it at 950 ° C in a muffle furnace for 4 hours with a heating rate of 5 ° C / min. After sintering, polish it with sandpaper to remove surface residues to obtain a solid electrolyte sheet of the comparative example.

[0061] Ion conductivity test: After the two ends of the solid electrolyte sheets obtained in Examples 1-3 and the comparative example were covered with conductive silver paste, they were placed in a battery mold and pressed to obtain test samples, and the ionic conductivity of the test samples at room temperature was tested by the AC impedance method, that is, the ionic conductivity of the lithium-ion solid-state battery at 25°C was tested. The specific test results are shown in Table 1:

[0062] Table 1 Product performance test results

[0063] Test items Example 1 Example 2 Example 3 Comparative Example 25℃ ionic conductivity (mS / cm) 0.77 1.58 0.62 0.47

[0064] This application has greatly improved the key electrochemical performance of LATP, ionic conductivity, only by doping gallium and silicon. The method of this application is simple to operate and has low cost. While effectively retaining the process steps of the LATP solid-phase sintering method, the microscopic crystal structure of LATP can be changed by doping gallium and silicon in a suitable proportion and then acting synergistically. At the same time, the generation of the second phase LiTiOPO4 can be regulated. The solid electrolyte sheet prepared by this method can promote the migration of lithium ions in the LATP solid electrolyte, improve the grain boundary conductivity, and thus improve the overall ionic conductivity of the solid electrolyte sheet.

[0065] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any slight modification, equivalent substitution and improvement made to the above embodiment based on the technical essence of the present invention should be included in the protection scope of the technical solution of the present invention.

Claims

1. A method for improving the ionic conductivity of solid electrolyte LATP, Features: Gallium and silicon are used as doping elements to change the lattice of LATP to a certain extent and promote the formation of LiTiOPO 4 , thereby reducing the resistance to lithium ion movement and improving grain boundary conductivity, thereby improving ion conductivity, including the following steps: S1: Take the required raw materials of lithium carbonate, aluminum oxide, titanium dioxide and ammonium dihydrogen phosphate and the doping raw materials of gallium oxide and silicon oxide, mix them in proportion, then ball mill, dry and sieve to obtain raw material powder; the atomic ratio of lithium, aluminum, titanium, phosphorus, gallium and silicon in the raw materials is Li:Al:Ti:P:Ga:Si=1.3:0.7:1.7:3:0.01:0.05, or Li:Al:Ti:P:Ga:Si=1.3:0.7:1.7:3:0.03:0.05, or Li:Al:Ti:P:Ga:Si=1.3:0.7:1.7:3:0.05:0.05; S2: placing the mixed raw material powder into a muffle furnace and calcining it for a specified time to obtain a LAGTSP precursor; S3: ball milling, drying and sieving the LAGTSP precursor obtained after calcination again to obtain LAGTSP precursor powder; S4: The LAGTSP precursor powder obtained after drying and sieving is placed in a mold and pressed into a thin sheet, and the thin sheet is placed in a muffle furnace for further sintering. After the sintering is completed, the surface impurities are removed by grinding with sandpaper to obtain a solid electrolyte sheet.

2. The method for improving the ionic conductivity of the solid electrolyte LATP according to claim 1, Features: In the step S1, the raw materials are mixed evenly and then ball milled for 8 h, the ball mill speed is 280 r / min, and ethanol is used as a dispersant; The raw powder after ball milling was dried in a drying oven at 80 °C for 10 h, ground for 1 h after the ethanol was completely evaporated, and sieved with a 160-mesh fine powder sieve.

3. The method for improving the ionic conductivity of the solid electrolyte LATP according to claim 1, Features: In the step S2, the raw material powder is calcined at 1200° C. for 2 h.

4. The method for improving the ionic conductivity of the solid electrolyte LATP according to claim 1, Features: In the step S4, the LAGTSP precursor powder is pressed into a circular sheet with a diameter of 8 mm and a thickness of 2.5 mm at a pressure of 18 MPa for 5 minutes, and then the sheet is placed in a muffle furnace and sintered at 950° C. for 4 hours at a heating rate of 5° C. / min.

5. A solid-state battery, Features: The solid-state battery adopts a solid electrolyte sheet prepared by the method for improving the ionic conductivity of the solid electrolyte LATP according to any one of claims 1 to 4.