Forming method for high-flatness ceramic substrate
Through dry preparation and dry pressure preforming combined with isostatic pretreatment and molding, linear boosting and step-type pressure relief methods are adopted to solve the problem of warpage of ceramic substrates and achieve high flatness of ceramic substrates. , reduces production costs and improves quality.
Patent Information
- Application Number
- CN202210849562.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-19
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-07-19
AI Technical Summary
In the existing ceramic substrate forming process, green body with severe warpage has poor effect on improving flatness through the leveling process, and the process is time-consuming and laborious, and energy consumption is high, making it difficult to meet the demand for high flatness.
The dry method is used to prepare pellets, dry pressure preforming, isostatic pressure pretreatment and isostatic pressure forming. Through linear boosting and step-by-step pressure relief, the maximum pressure value is 200~220MPa and the pressure holding is 6~ For 10 minutes, combined with dry preparation and dry pressure preforming, the moisture content is significantly reduced to improve flatness.
It significantly improves the flatness of the ceramic substrate, reduces water collection deformation, avoids re-leveling processes, reduces energy consumption and labor costs, and achieves efficient mass production and high-quality products.
Abstract
Description
Technical Field
[0001] The invention relates to a molding method, in particular to a molding method for a high-flatness ceramic substrate, and belongs to the technical field of electronic functional ceramic production technology. Background Art
[0002] In the field of ceramic production, the molding process is a key process in ceramic preparation. Ceramic substrates with high flatness can ensure the consistency and uniformity of the thickness of printed and sputtered circuits on the ceramic substrates, and can maximize the excellent properties of ceramics and metal packaging. Considering the changes in the international environment and the requirements of my country's national defense modernization and industrial transformation, the application of ceramic substrates is showing a trend of substantial increase, which puts higher requirements on the flatness process of the ceramic substrates themselves.
[0003] At present, the flatness of ceramic substrates is mainly controlled by leveling during sintering, also known as flattening. Although the flattening method is a relatively mature technology for improving the warpage of green bodies with severe warpage, it also has disadvantages such as unsatisfactory flattening effect, time-consuming and labor-intensive process, and high energy consumption. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a molding method for a high-flatness ceramic substrate which can effectively improve the flatness of a finished ceramic substrate.
[0005] The technical solution adopted to solve the above technical problems is: a molding method for a high-flatness ceramic substrate, the molding method at least comprising the steps of dry preparation of granulated materials, dry pressing preforming, isostatic pressing pretreatment, isostatic pressing molding and one-time sintering.
[0006] Among them, during isostatic pressing, a linear pressure increase and a stepped pressure release method are used, the maximum pressure value is 200-220 MPa and the pressure is maintained for 6-10 minutes.
[0007] Furthermore, during isostatic pressing, the pressure increasing rate is 20 MPa / min.
[0008] A preferred embodiment of the above scheme is that the stepped pressure relief during isostatic pressing includes the following steps: first, the pressure is relieved at a pressure relief rate of 10 MPa / min to 150 MPa and maintained for 3 to 5 minutes; then, the pressure is relieved at a pressure relief rate of 20 MPa / min to 90 MPa and maintained for 3 to 5 minutes; then, the pressure is relieved at a pressure relief rate of 20 MPa / min to 45 MPa and maintained for 5 to 10 minutes; and finally, the pressure is naturally relieved from 45 MPa.
[0009] Furthermore, the ceramic substrate is a beryllium oxide ceramic substrate, an aluminum oxide ceramic substrate or an aluminum nitride ceramic substrate.
[0010] The preferred embodiment of the above scheme is that when preparing the granulated material by dry method, the beryllium oxide granulated material, the aluminum oxide granulated material or the aluminum nitride granulated material are prepared respectively by spray granulation according to the formula.
[0011] The particle size of various granulated materials prepared is 80-120 μm, and the moisture content is 0.08%-0.1%.
[0012] Furthermore, the prepared granulated material is preformed into a preformed ceramic substrate by dry pressing at a pressure of 1 to 2 T / cm 3 control.
[0013] A preferred embodiment of the above scheme is that the consistency of the thickness of the preformed ceramic substrate formed by the dry pressing preforming process is controlled within ±0.05 mm, and the warpage of the preformed ceramic substrate does not exceed 0.4 mm.
[0014] Furthermore, when the dry-pressed preformed ceramic substrate is subjected to isostatic pressing pretreatment, a substrate with a thickness of 10 mm to 15 mm is used as a carrier, the bottom of the substrate is close to the sponge foam board, a layer of isolation film is attached to the top of the substrate, and then the pre-pressed ceramic substrate is placed on the isolation film. Finally, the entire foam board, substrate and ceramic substrate are wrapped with a vacuum film to form an integral plate of substrate + ceramic substrate, and then isostatic pressing pretreatment is performed.
[0015] A preferred embodiment of the above scheme is that the substrate carrier is a metal plate; the thickness of the metal plate is 10-15 mm; the corners of the metal plate are rounded and the edges are sealed; the roughness of the metal plate is 0.3-0.6 μm; and the flatness of the metal plate is ±0.2 mm.
[0016] Furthermore, after the entire foam board, substrate and ceramic substrate are wrapped with a vacuum film to form an integral board of substrate + ceramic substrate, vacuum treatment is required until no relative movement occurs between the ceramic substrate, metal plate and foam board.
[0017] The beneficial effects of the present invention are as follows: the technical solution provided by the present application prepares the ceramic substrate by setting at least several steps including dry preparation of granulation materials, dry pressing preforming, isostatic pressing pretreatment, isostatic pressing molding and one-time sintering, and adopts linear pressure increase and stepped pressure relief to form during isostatic pressing, with a maximum pressure value of 200-220MPa and pressure maintenance for 6-10 minutes. In this way, since the present application adopts dry preparation and dry pressing preforming for both granulation materials and preforming, and then successively performs isostatic pressing pretreatment and final isostatic pressing molding before one-time sintering, the water content in the process from raw materials to preforming can be significantly reduced, thereby reducing the deformation caused by water absorption, and at the same time, isostatic pressing pretreatment and isostatic pressing molding are assisted to obtain a green body with high flatness, and finally sintered and molded in one go, thereby achieving the purpose of effectively improving the flatness of the finished ceramic sheet. DETAILED DESCRIPTION
[0018] In order to solve the above technical problems existing in the prior art, the present invention provides a molding method for a high-flatness ceramic substrate that can effectively improve the flatness of the finished ceramic substrate. The molding method at least includes the steps of dry preparation of granulated materials, dry pressing preforming, isostatic pressing pretreatment, isostatic pressing molding, and one-time sintering.
[0019] Among them, during isostatic pressing, linear pressure rise and stepped pressure relief are used for forming, the maximum pressure value is 200-220MPa and the pressure is maintained for 6-10 minutes. The technical solution provided by the present application is prepared by setting at least several steps including dry preparation of granulation materials, dry pressing preforming, isostatic pressing pretreatment, isostatic pressing and one-time sintering, and linear pressure rise and stepped pressure relief are used for forming during isostatic pressing, the maximum pressure value is 200-220MPa and the pressure is maintained for 6-10 minutes. In this way, since the present application adopts dry preparation and dry pressing preforming for both granulation materials and preforming, and then isostatic pressing pretreatment and final isostatic pressing are carried out successively before one-time sintering, the water content in the process from raw materials to preforming can be significantly reduced, thereby reducing the deformation of water collection, and at the same time, isostatic pressing pretreatment and isostatic pressing are assisted to obtain a green body with high flatness, and finally sintered and formed in one go, thereby achieving the purpose of effectively improving the flatness of the finished ceramic sheet.
[0020] In the above-mentioned embodiment, the ceramic substrate described in the present application is mostly a beryllium oxide ceramic substrate, an alumina ceramic substrate or an aluminum nitride ceramic substrate. In order to maximize the flatness of the green body, corresponding control is required in each process, that is, during isostatic pressing, the pressure increase rate is 20MPa / min; and the step-by-step pressure relief during isostatic pressing includes the following steps: first, the pressure is relieved at a pressure relief rate of 10MPa / min to 150MPa and maintained for 3 to 5 minutes; then, the pressure is relieved at a pressure relief rate of 20MPa / min to 90MPa and maintained for 3 to 5 minutes; then, the pressure is relieved at a pressure relief rate of 20MPa / min to 45MPa and maintained for 5 to 10 minutes; finally, the pressure is naturally relieved from 45MPa. Accordingly, when preparing granules by dry method, beryllium oxide granules, aluminum oxide granules or aluminum nitride granules are prepared respectively by spray granulation according to the formula, wherein the particle size of each granule prepared is 80-120 μm, and the moisture content is 0.08%-0.1%. The dry pressing pressure of the prepared granules when pre-forming into a pre-formed ceramic substrate by dry pressing is 1-2 T / cm 3 control.
[0021] Furthermore, when the dry-pressed preformed ceramic substrate is subjected to isostatic pressing pretreatment, a 10mm to 15mm thick substrate is used as a carrier, the substrate is closely attached to the sponge foam board below, a layer of isolation film is attached to the substrate above, and then the preformed ceramic substrate is placed on the isolation film, and finally the entire foam board, substrate and ceramic substrate are wrapped with a vacuum film to form an integral plate of substrate + ceramic substrate, and then isostatic pressing is performed. At this time, the substrate carrier is a metal plate; the thickness of the metal plate is 10 to 15mm; the edges and corners of the metal plate are rounded, and the edges are sealed; the roughness of the metal plate is 0.3 to 0.6μm; the flatness of the metal plate is ±0.2mm. After the entire foam board, substrate and ceramic substrate are wrapped with a vacuum film to form an integral plate of substrate + ceramic substrate, it is still necessary to evacuate until there is no relative movement between the ceramic substrate, the metal plate and the foam board. The consistency of the thickness of the preformed ceramic substrate made by the dry pressing preforming process is controlled within ±0.05 mm, and the warpage of the preformed ceramic substrate does not exceed 0.4 mm.
[0022] In summary, the molding method provided in this application for preparing a ceramic substrate also has the following advantages:
[0023] 1. The ceramic substrate green body provided by the present invention has high flatness, and the flatness of the ceramic substrate after sintering is controlled within the range of ±0.05mm. Compared with the original process in which the substrate has a large warpage after sintering and can only improve the warpage after flattening, the flatness can be directly controlled from the source of the green body. The isostatic pressing method using a metal plate as a carrier can repair the cracks and burrs on the corners of the substrate after dry pressing, while reducing the gaps between the powder particles in the substrate and making the internal structure more consistent. The stepped pressure relief method can gradually release the stress inside the substrate without causing microcracks inside the substrate. In addition, the product fired once will not cause abnormal grain growth compared to flattening.
[0024] 2. The molding method of the present invention can not only realize the mass production of substrate products, effectively improve the production efficiency of enterprises, but also greatly improve the quality and qualified rate of ceramic substrate products, ensure the quality of subsequent packaged devices, and provide protection for the development of electronic devices. In addition, the present invention no longer requires additional flattening process, directly reducing labor costs, equipment costs, and energy consumption costs, which can increase profits and high price advantages for enterprises. Specific embodiments
[0026] The present invention provides a method for isostatic pressing of a high-flatness ceramic substrate, which comprises the following steps:
[0027] A. Dry method for preparing granules:
[0028] According to the formula, the granulated material is prepared by spray granulation;
[0029] B. Dry pressing preforming:
[0030] The prepared granules are dry pressed to preform into a preformed ceramic substrate, and the dry pressing pressure is 1-2T / cm 3 ;
[0031] C. Isostatic pressing pretreatment:
[0032] A 10mm to 15mm substrate is used as a carrier, a sponge foam board is closely attached to the bottom of the substrate, a layer of isolation film is attached to the top of the substrate, a dry-pressed preformed ceramic substrate is placed on the isolation film, and finally a vacuum film is used to wrap the entire foam board, substrate and ceramic substrate to form an integral board of substrate + ceramic substrate;
[0033] D. Isostatic Pressing:
[0034] The treated integral plate is placed in an isostatic pressing mold, and the pressure is increased linearly and released in a stepwise manner to 200-220 MPa, and the pressure is maintained for 6-10 minutes. After the pressure is released, the integral plate is taken out, the vacuum film is peeled off, and the ceramic substrate is taken out. The ceramic substrate at this time is the final formed substrate;
[0035] Among them, in the above-mentioned isostatic pressing method for high-flatness ceramic substrates, the ceramic substrates include but are not limited to beryllium oxide, aluminum oxide, and aluminum nitride ceramic substrates.
[0036] Wherein, in the above-mentioned high-flatness ceramic substrate isostatic pressing method, in step A, the particle size of the spray granulation material is 80-120 μm, and the water content is 0.08%-0.1%.
[0037] Among them, in the above-mentioned isostatic pressing method for high-flatness ceramic substrates, in step B, the thickness consistency of the preformed ceramic substrate is controlled at ±0.05mm, and the warpage of the ceramic substrate is 0.4mm.
[0038] Among them, in the above-mentioned high-flatness ceramic substrate isostatic pressing method, in step C, the substrate carrier is a metal plate; the thickness of the metal plate is 10 to 12 mm, so that it can withstand a pressure of more than 250 MPa without deformation; the corners of the metal plate are rounded and the edges are sealed; the roughness of the metal plate is 0.3 to 0.6 μm; the flatness of the metal plate is ±0.2 mm.
[0039] Among them, in the above-mentioned high-flatness ceramic substrate isostatic pressing method, in step C, the entire plate needs to be vacuumed until there is no relative movement between the substrate, the metal plate and the foam plate.
[0040] Wherein, in the above-mentioned isostatic pressing method for high-flatness ceramic substrates, in step D, the isostatic pressing pressure increase rate is 20 MPa / min.
[0041] Among them, in the above-mentioned high-flatness ceramic substrate isostatic pressing method, in step D, the step-by-step pressure release step of the isostatic pressing is to release the pressure from 10MPa / min to 150MPa, and hold the pressure for 3 to 5 minutes; then release the pressure from 20MPa / min to 90MPa and hold the pressure for 3 to 5 minutes; then release the pressure from 20MPa / min to 45MPa and hold the pressure for 5 to 10 minutes: and then naturally release the pressure from 45MPa.
Claims
1. Forming method for high flatness ceramic substrate, Features: The molding method at least comprises the steps of dry preparation of granulated materials, dry pressing preforming, isostatic pressing pretreatment, isostatic pressing molding and one-time sintering. Among them, during isostatic pressing, linear pressure increase and step-by-step pressure relief are used, with a maximum pressure of 200-220 MPa and pressure maintenance for 6-10 minutes. When the dry-pressed preformed ceramic substrate is subjected to isostatic pressing pretreatment, a 10mm to 15mm thick substrate is used as a carrier, the bottom of the substrate is closely attached to the sponge foam board, a layer of isolation film is attached to the top of the substrate, and then the pre-pressed ceramic substrate is placed on the isolation film. Finally, the entire foam board, substrate and ceramic substrate are wrapped with a vacuum film to form an integral plate of substrate + ceramic substrate, and then isostatic pressing pretreatment is performed. The substrate carrier is a metal plate; the thickness of the metal plate is 10-15 mm; the edges of the metal plate are rounded and the edges are sealed; the roughness of the metal plate is 0.3-0.6 μm; the flatness of the metal plate is ±0.2 mm, After the entire foam board, substrate and ceramic substrate are wrapped with a vacuum film to form an integral board of substrate + ceramic substrate, it is necessary to evacuate the foam board until there is no relative movement between the ceramic substrate, metal plate and foam board. The stepped pressure relief during isostatic pressing includes the following steps: first, the pressure is released at a pressure relief rate of 10 MPa / min to 150 MPa and maintained for 3 to 5 minutes; then, the pressure is released at a pressure relief rate of 20 MPa / min to 90 MPa and maintained for 3 to 5 minutes; then, the pressure is released at a pressure relief rate of 20 MPa / min to 45 MPa and maintained for 5 to 10 minutes; finally, the pressure is naturally relieved from 45 MPa.
2. The forming method for a high-flatness ceramic substrate according to claim 1, Features: During isostatic pressing, the pressure increase rate is 20MPa / min.
3. The forming method for a high-flatness ceramic substrate according to claim 1 or 2, Features: The ceramic substrate is a beryllium oxide ceramic substrate, an aluminum oxide ceramic substrate or an aluminum nitride ceramic substrate.
4. The forming method for a high-flatness ceramic substrate according to claim 3, Features: When preparing granules by dry method, beryllium oxide granules, aluminum oxide granules or aluminum nitride granules are prepared respectively by spray granulation according to the formula. The particle size of various granulated materials prepared is 80-120 μm, and the moisture content is 0.08%-0.1%.
5. The forming method for a high-flatness ceramic substrate according to claim 4, Features: The prepared granules are preformed into preformed ceramic substrates by dry pressing at a pressure of 1 to 2 T / cm 3 control.
6. The forming method for a high-flatness ceramic substrate according to claim 5, Features: The consistency of the thickness of the preformed ceramic substrate made by the dry pressing preforming process is controlled within ±0.05 mm, and the warpage of the preformed ceramic substrate does not exceed 0.4 mm.