Polyoxymethylene composition

By adding boron nitride with specific particle sizes and specific polymers into polyformaldehyde, a new polyformaldehyde composition with high stress creep resistance, impact resistance, acid resistance and thermal stability is formed, which solves the high problems in the existing technology. The problem of insufficient performance under stress is achieved and better material properties are achieved.

CN115197531BActive Publication Date: 2024-10-01ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210338530.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-04-08
Filing Date
2022-04-01
Publication Date
2024-10-01
Estimated Expiration
2042-04-01

AI Technical Summary

Technical Problem

Existing polyoxymethylene compositions have room for improvement in terms of creep properties and impact strength under high stress, and have insufficient acid resistance and thermal stability, especially when used under high temperatures and acidic conditions.

Method used

By preparing a boron nitride and polyoxymethylene composition within a specific average particle size range, and adding a poly-β-alanine polymer containing a primary amide group and a polyamide polymer with a moderate melting point on its basis, a polyamide polymer with a moderate melting point is formed. A new polyoxymethylene composition with excellent creep resistance, impact resistance, acid resistance and thermal stability.

Benefits of technology

It achieves high creep resistance and high impact strength under high stress, while improving the acid resistance and thermal stability of the polyoxymethylene composition, solving the contradictory relationship and insufficient performance problems in the existing technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003577714350000141
    Figure BDA0003577714350000141
  • Figure BDA0003577714350000301
    Figure BDA0003577714350000301
  • Figure BDA0003577714350000311
    Figure BDA0003577714350000311
Patent Text Reader

Abstract

The present invention relates to a polyoxymethylene composition. An object of the present invention is to provide a polyoxymethylene composition having high high stress creep resistance, impact resistance, acid resistance and thermal stability. A polyoxymethylene composition, characterized in that the polyoxymethylene composition comprises 100 parts by mass of (A) polyoxymethylene and 0.001 to 0.5 parts by mass of (B) boron nitride, wherein the average particle size of at least 100 particles in a field of view image of (B) boron nitride obtained by a scanning electron microscope at a magnification of 50,000 times and obtained using image processing analysis software ("A-image Kun" manufactured by Asahi Kasei Engineering Corporation) is 10 nm to 800 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to polyoxymethylene compositions. Background Art

[0002] In the past, polyoxymethylene has been widely used as a material for many molded products, such as mechanical parts of automobiles, electrical products, and machinery, due to its high mechanical strength and excellent rigidity, creep resistance, solvent resistance, and sliding properties. However, as the scope of use of polyoxymethylene has expanded in recent years, represented by its use as a substitute for metal materials, there is a trend of gradually requiring higher properties. In addition, resistance to use under severe conditions such as high temperature and acidic conditions is also required.

[0003] For example, the resin material of the power window gear, which is a mechanical part of the car, is being miniaturized, and creep resistance is required under higher torque. On the other hand, a material with high impact resistance is desired so that good working durability can be ensured even when a starting torque greater than the rated torque is applied instantaneously during operation. In addition, tolerance to deterioration caused by the acidic components contained in the grease during gear operation and thermal degradation caused by frictional heat is also required.

[0004] To date, as a measure to improve the creep resistance of polyoxymethylene, research has been conducted on the use of boron nitride as a crystal nucleating agent. For example, Patent Document 1 lists the effects of improving high-temperature low-stress creep properties and suppressing fluctuations in Charpy impact strength by adding boron nitride at a specific concentration.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2019-183080 Summary of the invention

[0008] Problems to be solved by the invention

[0009] However, although the technology disclosed in Patent Document 1 improves the creep properties under low stress, the creep properties under high stress still have room for improvement. In addition, although the variation of Charpy impact strength itself is suppressed, further improvement is expected in terms of ensuring sufficient impact strength. Generally, polyoxymethylene to which a crystallization nucleating agent is added has improved rigidity as the polyoxymethylene brought about by the crystallization nucleating agent has a high degree of crystallinity, but on the other hand, it becomes brittle and thus has a tendency to reduce impact strength. Therefore, there is a contradictory relationship between the creep resistance and impact resistance in the system to which a crystallization nucleating agent is added. In addition, the technology disclosed in Patent Document 1 is not expected to contribute to improving the thermal stability and acid resistance of the polyoxymethylene composition.

[0010] Therefore, an object of the present invention is to provide a polyoxymethylene composition having high high stress creep resistance and Charpy impact strength and excellent acid resistance and thermal stability.

[0011] Methods used to solve problems

[0012] The present inventors have conducted intensive studies on the above-mentioned problems and, as a result, have found that the above-mentioned problems can be solved by preparing a polyoxymethylene composition containing boron nitride having an average particle size within a specific range, thereby completing the present invention.

[0013] That is, the present invention is as follows. [1]

[0015] A polyoxymethylene composition, characterized in that the polyoxymethylene composition comprises 100 parts by mass of (A) polyoxymethylene and 0.001 to 0.5 parts by mass of (B) boron nitride,

[0016] The boron nitride (B) has an average particle size of 100 to 800 nm of at least 100 particles in a field of view image of 3.0 μm×3.0 μm obtained by a scanning electron microscope at a magnification of 50,000 times, obtained using image processing analysis software. [2]

[0018] The polyoxymethylene composition according to [1], wherein the average particle size of the (B) boron nitride is 80 nm to 500 nm. [3]

[0020] The polyoxymethylene composition according to [1] or [2], wherein the content of the (B) boron nitride is 0.02 to 0.5 parts by mass. [4]

[0022] The polyoxymethylene composition according to any one of [1] to [3], further comprising 0.01 to 3.0 parts by mass of (C) a poly-β-alanine polymer containing 30 to 70 mol % of primary amide groups. [5]

[0024] The polyoxymethylene composition according to any one of [1] to [4], further comprising 0.001 to 0.1 parts by mass of (D) a polyamide polymer, wherein the melting point of the (D) polyamide polymer is 140°C to 230°C. [6]

[0026] The polyoxymethylene composition according to [5], wherein a mass ratio (D) / (B) of the polyamide polymer (D) to the boron nitride (B) is 0.04 to 1.0.

[0027] Effects of the Invention

[0028] According to the present invention, a polyoxymethylene composition having high high-stress creep resistance, impact resistance, acid resistance and thermal stability can be provided. DETAILED DESCRIPTION

[0029] Hereinafter, a mode for carrying out the present invention (hereinafter referred to as "this embodiment") will be described in detail. The present invention is not limited to the following this embodiment, and can be carried out with various modifications within the scope of the gist thereof.

[0030] [Polyoxymethylene composition]

[0031] The polyoxymethylene composition of the present embodiment includes (A) polyoxymethylene and (B) boron nitride. The polyoxymethylene composition of the present embodiment may further include (C) a poly-β-alanine polymer containing 30 mol% to 70 mol% of primary amide groups (hereinafter also referred to as "(C) poly-β-alanine polymer"), (D) a polyamide polymer having a melting point of 140°C to 230°C (hereinafter also referred to as "(D) polyamide polymer"), and other various additives.

[0032] <(A) Polyoxymethylene>

[0033] The (A) polyoxymethylene contained in the polyoxymethylene composition of the present embodiment is not particularly limited, and may be any of a polyoxymethylene homopolymer, a polyoxymethylene copolymer, and a mixture of a polyoxymethylene homopolymer and a polyoxymethylene copolymer. Among them, a polyoxymethylene homopolymer is preferred.

[0034] (A) The polyoxymethylene may be used alone or in combination of two or more.

[0035] -Polyoxymethylene Homopolymer-

[0036] The polyoxymethylene homopolymer is a polymer whose main chain substantially only contains oxymethylene units, and preferably 99.8 mol% or more of the main chain excluding both terminals is composed of oxymethylene units, and more preferably the main chain excluding both terminals is composed of only oxymethylene units. In addition, it is particularly preferred that the polyoxymethylene homopolymer has both terminals capped by esterification.

[0037] The polyoxymethylene homopolymer can be obtained by homopolymerizing a formaldehyde monomer or a cyclic oligomer of formaldehyde such as a trimer (trimer) or a tetramer (tetramer) thereof, and can be produced, for example, by supplying formaldehyde as a monomer, a chain transfer agent (molecular weight regulator) and a polymerization catalyst to a polymerization reactor into which a hydrocarbon polymerization solvent has been introduced and polymerizing by a slurry polymerization method.

[0038] At this time, the raw material monomers, chain transfer agents, and polymerization catalysts may contain components that can cause chain transfer (components that generate unstable terminal groups) such as water, methanol, and formic acid. Therefore, it is preferred to first adjust the content of these components that can cause chain transfer.

[0039] The content of these components capable of chain transfer is preferably in the range of 1 to 1000 ppm by mass, more preferably 1 to 500 ppm by mass, and even more preferably 1 to 300 ppm by mass, relative to the total mass of formaldehyde.

[0040] By adjusting the content of the component capable of chain transfer to fall within the above range, a polyoxymethylene homopolymer having excellent thermal stability can be obtained.

[0041] The molecular weight of the polyoxymethylene homopolymer can be adjusted by using a molecular weight modifier such as carboxylic anhydride or carboxylic acid to cause chain transfer. As the molecular weight modifier, propionic anhydride and acetic anhydride are particularly preferred, and acetic anhydride is more preferred.

[0042] The molecular weight modifier may be used alone or in combination of two or more.

[0043] The amount of the molecular weight modifier introduced is adjusted and determined according to the properties (particularly the melt flow rate) of the target polyoxymethylene homopolymer. For example, it is preferred that the melt flow rate (MFR value (according to ISO1133, 190°C, 2.16 kg load)) of the polyoxymethylene homopolymer be within the range of 0.1 g / 10 min to 100 g / 10 min, and it is more preferred that the melt flow rate of the polyoxymethylene homopolymer be within the range of 1.0 g / 10 min to 70 g / 10 min. By adjusting the MFR value of the polyoxymethylene homopolymer to the above range, a polyoxymethylene homopolymer having excellent mechanical strength can be obtained.

[0044] As the polymerization catalyst, an anionic polymerization catalyst is preferred, and more preferably a catalyst represented by the following general formula (1): Salt polymerization catalysts.

[0045] [R1R2R3R4M] + X - ……(1)

[0046] (In formula (1), R1, R2, R3 and R4 each independently represent an alkyl group, M represents an element having a lone pair of electrons, and X represents a nucleophilic group. R1, R2, R3 and R4 may be the same as or different from each other.)

[0047] The polymerization catalyst may be used alone or in combination of two or more.

[0048] Among the salt polymerization catalysts, tetraethyl iodide is preferred. Tributyl ethyl iodide Waiting for the season Salt compounds; quaternary ammonium salt compounds such as tetramethylammonium bromide and dimethyl distearyl ammonium acetate.

[0049] Relative to 1 mol of formaldehyde, these quaternary Salt compounds and quaternary ammonium salt compounds, etc. The amount of the salt-based polymerization catalyst added is preferably 0.0003 mol to 0.01 mol, more preferably 0.0008 mol to 0.005 mol, and even more preferably 0.001 mol to 0.003 mol.

[0050] The hydrocarbon polymerization solvent is not particularly limited as long as it is a solvent that does not react with formaldehyde. Examples thereof include pentane, isopentane, hexane, cyclohexane, heptane, octane, nonane, decane, benzene and the like, and hexane is particularly preferred.

[0051] These hydrocarbon polymerization solvents may be used alone or in combination of two or more.

[0052] In the production of the polyoxymethylene homopolymer, it is preferred that a crude polyoxymethylene homopolymer is first obtained by polymerization, and then the unstable terminal groups are subjected to a stabilization treatment as described later.

[0053] The polymerization reactor used for producing the crude polyoxymethylene homopolymer is not particularly limited as long as it can simultaneously supply formaldehyde as a monomer, a chain transfer agent (molecular weight modifier), a polymerization catalyst, and a hydrocarbon polymerization solvent, but is preferably a continuous polymerization reactor from the viewpoint of productivity.

[0054] The terminal groups of the crude polyoxymethylene homopolymer obtained by polymerization are thermally unstable, and therefore, it is preferred to perform a stabilization treatment by capping the unstable terminal groups with an esterifying agent or an etherifying agent.

[0055] The stabilization treatment of the terminal groups of the crude polyoxymethylene homopolymer by esterification can be performed, for example, by charging the crude polyoxymethylene homopolymer, the esterification agent and / or the esterification catalyst into a terminal stabilization reactor into which a hydrocarbon polymerization solvent is introduced and reacting them.

[0056] As the reaction temperature and reaction time at this time, the preferred reaction temperature is 130°C to 155°C and the reaction time is 1 minute to 100 minutes, the more preferred reaction temperature is 135°C to 155°C and the reaction time is 5 minutes to 100 minutes, and the further preferred reaction temperature is 140°C to 155°C and the reaction time is 10 minutes to 100 minutes.

[0057] As an esterifying agent for sealing and stabilizing the terminal groups of the crude polyoxymethylene homopolymer, an acid anhydride represented by the following general formula (2) can be used.

[0058] R5COOCOR6……(2)

[0059] (In formula (2), R5 and R6 each independently represent an alkyl group. R5 and R6 may be the same as or different from each other.)

[0060] Examples of the esterifying agent include benzoic anhydride, succinic anhydride, maleic anhydride, glutaric anhydride, phthalic anhydride, propionic anhydride, and acetic anhydride, and acetic anhydride is preferred.

[0061] These esterifying agents may be used alone or in combination of two or more.

[0062] The esterification catalyst is preferably an alkali metal salt of a carboxylic acid having 1 to 18 carbon atoms. The amount of the esterification catalyst added can be appropriately selected within the range of 1 to 1000 ppm by mass relative to the mass of the polyoxymethylene homopolymer.

[0063] Examples of alkali metal salts of carboxylic acids having 1 to 18 carbon atoms include alkali metal salts of carboxylic acids such as formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, heptanoic acid, octanoic acid, nonanoic acid, capric acid, lauric acid, myristic acid, palmitic acid, heptadecanoic acid, and stearic acid, and examples of the alkali metal include lithium, sodium, potassium, rubidium, and cesium. Among these alkali metal salts of carboxylic acids, alkali metal salts such as lithium acetate, sodium acetate, and potassium acetate are preferred.

[0064] The crude polyoxymethylene homopolymer can also be stabilized by capping the terminal groups thereof by etherification.

[0065] The etherifying agent can be selected from orthoesters of aliphatic or aromatic acids and aliphatic, alicyclic or aromatic alcohols, such as methyl orthoformate or ethyl orthoformate, methyl orthoacetate or ethyl orthobenzoate, and orthocarbonates, specifically ethyl orthocarbonate, and can be stabilized using medium-strength organic acids such as p-toluenesulfonic acid, acetic acid and oxalic acid, and Lewis acid catalysts such as dimethyl sulfate and diethyl sulfate.

[0066] As the solvent used in the etherification reaction when the terminal groups of the crude polyoxymethylene homopolymer are capped and stabilized by etherification, there can be mentioned, for example: low-boiling aliphatic organic solvents such as pentane, hexane, cyclohexane and benzene, alicyclic and aromatic hydrocarbon organic solvents; halogenated lower aliphatic hydrocarbon organic solvents such as dichloromethane, chloroform and carbon tetrachloride; and other organic solvents.

[0067] The polyoxymethylene homopolymer whose terminal groups are stabilized by the above method is dried by sealing air or nitrogen adjusted to 100° C. to 150° C. using a dryer such as a hot air dryer or a vacuum dryer to remove moisture, thereby obtaining the target polyoxymethylene homopolymer.

[0068] -Polyoxymethylene copolymer-

[0069] The polyoxymethylene copolymer can be produced by using, for example, a diol such as 1,3-dioxolane or 1,4-butanediol formal, a cyclic ether such as cyclic formal of dimer glycol, or a cyclic formal as a comonomer and copolymerizing it with a monomer such as trioxymethylene.

[0070] The ratio of the copolymerized comonomer to 1 mol of the above-mentioned trioxymethylene is preferably 0.03 mol% to 20 mol%, more preferably 0.03 mol% to 15 mol%, and further preferably 0.04 mol% to 5 mol%. When the ratio of the comonomer is within the above range, polyoxymethylene particles having better mechanical strength can be obtained.

[0071] Examples of the polymerization catalyst used in the polymerization of the polyoxymethylene copolymer include cation-active catalysts such as Lewis acids, protonic acids, and esters and anhydrides thereof.

[0072] Examples of the Lewis acid include halides of boron, tin, titanium, phosphorus, arsenic, and antimony. Specifically, examples include boron trifluoride, tin tetrachloride, titanium tetrachloride, phosphorus pentafluoride, phosphorus pentachloride, antimony pentafluoride, and complexes or salts thereof.

[0073] Examples of protonic acids and their esters or anhydrides include perchloric acid, trifluoromethanesulfonic acid, tert-butyl perchlorate, acetyl perchlorate, trimethylol Hexafluorophosphate, etc.

[0074] Among these substances, boron trifluoride, boron trifluoride hydrate, and coordination complexes of boron trifluoride and an organic compound containing an oxygen atom or a sulfur atom are preferred. For example, boron trifluoride diethyl ether and boron trifluoride di-n-butyl ether can be mentioned as preferred examples.

[0075] The amount of boron trifluoride added is preferably 0.10×10 -4 mol or less, more preferably 0.07×10 -4 mol or less, more preferably 0.03×10 -4 Mole~0.05×10 -4 When the amount of boron trifluoride added is within the above range, a polyoxymethylene composition having excellent thermal stability can be provided.

[0076] As a method for polymerizing the polyoxymethylene copolymer exemplified above, in addition to the above-mentioned slurry polymerization method, for example, a bulk polymerization method may be used, and any of a batch method and a continuous method can be applied.

[0077] Examples of the polymerization apparatus include self-cleaning extrusion kneading machines such as a co-kneader, a twin-screw continuous extrusion kneading machine, and a twin-screw paddle continuous mixer.

[0078] The monomers in a molten state are supplied to the above-mentioned polymerization apparatus, and a polyoxymethylene copolymer in a solid block form is obtained while polymerization proceeds.

[0079] In the polyoxymethylene copolymer obtained by the above polymerization, there may be thermally unstable terminal parts [-(OCH2) n -OH group], therefore, it is preferable to perform a decomposition and removal treatment of the unstable terminal portion. The decomposition and removal method of the unstable terminal portion can be carried out by a known method.

[0080] <(B) Boron nitride>

[0081] The polyoxymethylene composition of the present embodiment contains (B) boron nitride as a crystal nucleating agent.

[0082] The average particle size of the boron nitride (B) is 10 nm to 800 nm, preferably 80 nm to 500 nm, and more preferably 100 nm to 500 nm, from the viewpoint of the spherulite size of the polyoxymethylene (A) formed by functioning as a crystal nucleating agent.

[0083] It should be noted that the average particle size of the boron nitride (B) is obtained as follows: particles of the boron nitride (B) are taken out from the polyoxymethylene composition, and a field of view image of a range of 3.0 μm×3.0 μm is obtained by a scanning electron microscope at a magnification of 50,000 times using an image processing analysis software ("A-image Kun" manufactured by Asahi Kasei Engineering Corporation) to obtain the average value of the longest particle size of at least 100 particles in the above field of view image as the average particle size of the boron nitride (B). Specifically, it is obtained by the method described in the examples described later.

[0084] Examples of a method for removing the (B) boron nitride particles from the polyoxymethylene composition include a method of decomposing and removing organic components in the polyoxymethylene composition by incineration or heat treatment in a nitrogen atmosphere.

[0085] Regarding the (B) boron nitride, the (B) boron nitride having an average particle size within the above range can be used directly, or the boron nitride having a large particle size can be crushed and processed into the above average particle size range before use. That is, the particle size of the (B) boron nitride can be controlled by the crushing process.

[0086] Examples of the machine for pulverizing include a dry jet mill, a wet jet mill, a hammer mill, a vibration mill, a roll mill, a tumble mill, a roller mill, a bead mill, an impact shear mill, a high-pressure fluid impact mill, a dry ball mill, and a wet ball mill.

[0087] In addition, as a pulverization method, only a dry method may be used, a method combining a wet method and a dry method may be used, or only a wet method may be used.

[0088] (B) Boron nitride may be in any shape such as scale, flat, disc, or spherical.

[0089] The crystal structure of the boron nitride (B) includes a hexagonal graphite structure, a cubic sphalerite structure, and a hexagonal wurtzite structure. As a crystal nucleating agent for polyoxymethylene, the boron nitride (B) is preferably a hexagonal boron nitride having a hexagonal graphite structure.

[0090] (B) Boron nitride not only functions as a crystal nucleating agent, but also contributes to improving the thermal conductivity, heat resistance, corrosion resistance, electrical insulation, lubricity, and mold release properties of the polyoxymethylene composition.

[0091] There are no particular restrictions on the type of (B) boron nitride, and examples thereof include XGP (manufactured by Denka Co., Ltd.), SGP (manufactured by Denka Co., Ltd.), MGP (manufactured by Denka Co., Ltd.), GP (manufactured by Denka Co., Ltd.), HGP (manufactured by Denka Co., Ltd.), SP-2 (manufactured by Denka Co., Ltd.), SP-3 (manufactured by Denka Co., Ltd.), SGPS (manufactured by Denka Co., Ltd.), AP-10S (manufactured by Maruka Co., Ltd.), AP-20S (manufactured by Maruka Co., Ltd.), AP-100S (manufactured by Maruka Co., Ltd.), SL-170-20OG (manufactured by Maruka Co., Ltd.), SL-170-20-WA (manufactured by Maruka Co., Ltd.), UHP-S2 (manufactured by Showa Denko Co., Ltd.), )、UHP-1K (manufactured by Showa Denko Co., Ltd.), UHP-2 (manufactured by Showa Denko Co., Ltd.), UHP-G1H (manufactured by Showa Denko Co., Ltd.), PCT-UFB (manufactured by Saint-Gobain Co., Ltd.), PCTP2 (manufactured by Saint-Gobain Co., Ltd.), PCTF5 (manufactured by Saint-Gobain Co., Ltd.), PCTP8 (manufactured by Saint-Gobain Co., Ltd.), PCTL30 (manufactured by Saint-Gobain Co., Ltd.), PCTP12 (manufactured by Saint-Gobain Co., Ltd.), PCTP16 (manufactured by Saint-Gobain Co., Ltd.), PCTP30 (manufactured by Saint-Gobain Co., Ltd.), (manufactured by Saint-Gobain), PCTP30D (manufactured by Saint-Gobain), PCTL5MHF (manufactured by Saint-Gobain), PCTL7MHF (manufactured by Saint-Gobain), PCTL20MHF (manufactured by Saint-Gobain), PCTH7MHF (manufactured by Saint-Gobain), PCTH10MHF (manufactured by Saint-Gobain), CTS7M (manufactured by Saint-Gobain), CTS25M (manufactured by Saint-Gobain), IDL100 (manufactured by Saint-Gobain), IDL200 (manufactured by Saint-Gobain), IDL300 (manufactured by Saint-Gobain), IDL400 (manufactured by Saint-Gobain), IDL500 (manufactured by Saint-Gobain), IDL600 (manufactured by Saint-Gobain), IDL700 (manufactured by Saint-Gobain), IDL800 (manufactured by Saint-Gobain), IDL900 (manufactured by Saint-Gobain), PHPP325 (manufactured by Saint-Gobain), PHPP325B (manufactured by Saint-Gobain),MCFP (manufactured by Saint-Gobain), PSHP325 (manufactured by Saint-Gobain), PSHP605 (manufactured by Saint-Gobain), PCPS3005 (manufactured by Saint-Gobain), PCPS302 (manufactured by Saint-Gobain), PCPS308 (manufactured by Saint-Gobain), PCPS3012 (manufactured by Saint-Gobain), PCPS3016 (manufactured by Saint-Gobain), PCPS330 (manufactured by Saint-Gobain), PUHP3008J (manufactured by Saint-Gobain), PUHP1109J (manufactured by Saint-Gobain), PT110 (manufactured by Momentive), PT120 (manufactured by Momentive), PT350 (manufactured by Momentive), PT670 (manufactured by Momentive), PTX25 (manufactured by Momentive), PTX60 (manufactured by Momentive), ZSA-200 (manufactured by Zikusu Industries), ZSA-20 (manufactured by Zikusu Industries), ZSA-5 (manufactured by Zikusu Industries), SCP1 (manufactured by ESK Ceramics), SX (manufactured by ESK Ceramics), S1 (manufactured by ESK Ceramics), S3 (manufactured by ESK Ceramics), SRF (manufactured by ESK Ceramics) CERAMICS Co., Ltd.), SHP-2 (Mizushima Alloy Iron Co., Ltd.), SHP-3 (Mizushima Alloy Iron Co., Ltd.), SHP-4 (Mizushima Alloy Iron Co., Ltd.), SHP-5 (Mizushima Alloy Iron Co., Ltd.), SHP-5L (Mizushima Alloy Iron Co., Ltd.), SHP-6 (Mizushima Alloy Iron Co., Ltd.), SHP-7 (Mizushima Alloy Iron Co., Ltd.), SHP-9 (Mizushima Alloy Iron Co., Ltd.), HP-1 (Mizushima Alloy Iron Co., Ltd.), HP-P1 (Mizushima Alloy Iron Co., Ltd.), HP-2 (Mizushima Alloy Iron Co., Ltd.), HP-4W (Mizushima Alloy Iron Co., Ltd.), HP-6 (Mizushima Alloy Iron Co., Ltd.), HP40J (Mizushima Alloy Iron Co., Ltd.), HP40MF (Mizushima Alloy Iron Co., Ltd.), FS-1 (Mizushima Alloy Iron Co., Ltd.), FS-3 (Mizushima Alloy Iron Co., Ltd.), Platelets 001 (3M Co., Ltd.), Platelets 003E (manufactured by 3M Company), Platelets 003SF (manufactured by 3M Company), Platelets 003 (manufactured by 3M Company), Platelets 006 (manufactured by 3M Company),Platelets 007HS (manufactured by 3M), Platelets 0075 (manufactured by 3M), Platelets 009 (manufactured by 3M), Platelets 012 (manufactured by 3M), Platelets 012P (manufactured by 3M), Flakes 500-3 (manufactured by 3M), L551 (manufactured by HONGWUNEWMA TERIAL), L553 (manufactured by HONGWUNEWMA TERIAL), L556 (manufactured by HONGWUNEWMA TERIAL), Hex-Boron Nitride Powder (hBN, purity 99%, APS: 70nm) (manufactured by Lower Friction), Hex-Boron Nitride Powder (hBN, purity 98%, APS: 0.5μm) (manufactured by Lower Friction), Hex-Boron Nitride Powder (hBN, purity 98%, APS: 1.5μm) (manufactured by Lower Friction), FRICTION), Hex-Boron Nitride Powder (hBN, purity 98%, APS: 5 microns) (Lower Friction), Hex-Boron Nitride Powder (hBN, purity 98%, APS: 30 microns) (Lower Friction), etc.

[0092] (B) Boron nitride may be used alone or in combination of two or more.

[0093] Representative methods for producing (B) boron nitride include a method of reacting molten boric anhydride (B2O3) with nitrogen or ammonia in the presence of a calcium phosphate (Ca3(PO4)2) catalyst. Other methods include a method of reacting boric acid or an alkali metal boride with an organic nitrogen compound such as urea, guanidine, or melamine in a high-temperature nitrogen-ammonia atmosphere, a method of reacting molten sodium borate (Na3BO3) with ammonium chloride in an ammonia atmosphere, a method of reacting boron trichloride (BCl3) with ammonia at high temperatures, a CVD (chemical vapor deposition) method, a thermal CVD method, a PVD (physical vapor deposition) method, and the like.

[0094] The (B) boron nitride used in the present embodiment may contain impurities such as B2O3, boric acid, and carbon components, but the purity of the (B) boron nitride is preferably 60% or more, more preferably 80% or more, and most preferably 90% or more.

[0095] The boron nitride (B) may be added in the form of a solid or dispersed in a dispersion medium in the production of the polyoxymethylene composition of the present embodiment. In addition, a pretreatment such as surface oxidation or surface modification, calcination, insertion of a dopant, or cleavage treatment may be appropriately applied.

[0096] The content of the boron nitride (B) in the polyoxymethylene composition of the present embodiment can be measured by quantitative analysis of the boron element by inductively coupled plasma mass spectrometry (ICP-MS), and specifically, can be measured by the method described in Examples described later.

[0097] As a pretreatment for ICP-MS measurement, it can be listed that any one of the particles, powders, and formed cutting pieces of the polyoxymethylene composition and a mixed acid of hydrofluoric acid and nitric acid are added to a pressurizable container, and pressurized acid decomposition of the closed system is performed by microwave radiation, thereby completely decomposing the (B) boron nitride in the polyoxymethylene composition, and the boron element can be quantitatively analyzed by ICP-MS.

[0098] From the viewpoint of the effective amount of the crystal nucleating agent, the content of the boron nitride (B) in the polyoxymethylene composition of the present embodiment is 0.001 parts by mass or more, preferably 0.002 parts by mass or more, more preferably 0.005 parts by mass or more, further preferably 0.007 parts by mass or more, still further preferably 0.01 parts by mass or more, and most preferably 0.02 parts by mass or more, relative to 100 parts by mass of the polyoxymethylene (A). On the other hand, from the viewpoint of thermal stability and the influence of being a fracture starting point as a foreign matter, the content of the boron nitride (B) is 0.5 parts by mass or less, preferably 0.3 parts by mass or less, and more preferably 0.2 parts by mass or less.

[0099] By using the boron nitride (B) within the above-mentioned specific particle size and content range, the spherulite size of the polyoxymethylene (A) can be reduced as much as possible, the creep resistance under high stress can be improved, and surprisingly, a polyoxymethylene composition with excellent impact resistance and acid resistance can be provided. The detailed principle is not clear, but with respect to impact resistance, it is believed that the anisotropy of the crystal structure of the surface layer of the molded product is eliminated by increasing the crystallization rate, and with respect to acid resistance, it is believed that the nitrogen atoms in the boron nitride (B) act as a base.

[0100] <(C) Poly-β-alanine polymer>

[0101] The polyoxymethylene composition of the present embodiment may contain (C) a poly-β-alanine polymer containing 30 mol % to 70 mol % of a primary amide group.

[0102] (C) The poly-β-alanine polymer mainly comprises a structural unit (3) represented by the following formula (3) and a structural unit (4) represented by the following formula (4).

[0103]

[0104] It should be noted that “mainly comprising the structural unit (3) and the structural unit (4)” means that the total content of the structural unit (3) and the structural unit (4) in the (C) poly-β-alanine polymer is 95 mol% or more.

[0105] (C) The poly-β-alanine polymer may be used alone or in combination of two or more.

[0106] As described above, the structural unit (4) contains a primary amide group, and the content of the primary amide group in the poly-β-alanine polymer (C) is 30 mol% to 70 mol%, more preferably 35 mol% to 65 mol%, and more preferably 40 mol% to 60 mol%. When the content of the primary amide group is within this range, the productivity is excellent.

[0107] As a method for determining the content of primary amide groups, first, a sample polymer and a 40% by mass potassium hydroxide aqueous solution are added to a flask equipped with a stirrer, and heated at 105° C. to 110° C. for 20 minutes while stirring, thereby hydrolyzing the primary amide groups into ammonia. Next, the contents of the flask are cooled to below 50° C., and then methanol is added to extract ammonia together with the methanol. The extract is absorbed in a 0.1 normal sulfuric acid aqueous solution, and neutralization titration is performed using methyl red as an indicator with a 0.1 normal sodium hydroxide aqueous solution to determine the content of the primary amide groups.

[0108] As the (C) poly-β-alanine polymer, a poly-β-alanine polymer ranging from a low molecular weight poly-β-alanine polymer soluble in formic acid to a high molecular weight poly-β-alanine polymer insoluble in formic acid can be used. Preferably, the poly-β-alanine polymer has a molecular weight equivalent to a reduced viscosity (ηsp / c) of 0.5 dL / g to 15 dL / g, more preferably, a poly-β-alanine polymer has a molecular weight equivalent to a reduced viscosity (ηsp / c) of 1 dL / g to 10 dL / g, and further preferably, a poly-β-alanine polymer has a molecular weight equivalent to a reduced viscosity (ηsp / c) of 2 dL / g to 5 dL / g.

[0109] As a method for determining reduced viscosity (ηsp / c), first, 5g of polymer is added to 100mL of formic acid and stirred at room temperature for 2 hours to dissolve it. Then, it is filtered under reduced pressure to obtain a formic acid solution. 500mL of methanol is added to the formic acid solution to precipitate the formic acid solution, the precipitate is filtered, and then dried under reduced pressure at 80°C for 10 hours in a vacuum dryer. The obtained sample is dissolved in formic acid with a purity of more than 99%, and then passed through a 200-mesh filter material to prepare a sample solution with a sample concentration of 1g / dL. The falling time of the sample solution at a temperature of 35°C is measured using an Ostwald viscometer, and the reduced viscosity ηsp / c (dL / g) is calculated by the following formula.

[0110] ηsp / c=(t / t0-1) / c

[0111] (Wherein, t is the falling time of the sample solution (seconds), t0 is the falling time of the formic acid solution (seconds), and c is the concentration of the sample solution (g / dL).)

[0112] (C) The poly-β-alanine polymer can be produced by, for example, polymerizing acrylamide using an alkaline earth metal alkoxide as a catalyst.

[0113] (C) The polymerization reaction of the poly-β-alanine polymer may be carried out in the absence of a solvent or in the presence of a solvent. Examples of the solvent include aromatic hydrocarbons such as benzene, toluene, and xylene; and halogenated aromatic hydrocarbons such as chlorobenzene and o-dichlorobenzene.

[0114] The polymerization is carried out, for example, by adding a predetermined amount of catalyst to the dehydrated and purified acrylamide and heating it in an inert gas atmosphere. As the polymerization method, batch solution polymerization, batch bulk polymerization, continuous solution polymerization, continuous bulk polymerization, etc. can be used.

[0115] The reaction temperature of the polymerization reaction is usually preferably in the range of 70°C to 150°C, more preferably 80°C to 130°C.

[0116] In addition, as (C) poly-β-alanine polymer, a poly-β-alanine polymer having a cross-linked structure can also be used. As a poly-β-alanine polymer having a cross-linked structure, a poly-β-alanine polymer obtained by cross-linking with methylenebisacrylamide can be cited. By having a cross-linked structure, cohesion is improved and continuous productivity becomes better.

[0117] From the viewpoint of thermal stability, the content of the poly-β-alanine polymer (C) is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, relative to 100 parts by mass of the polyoxymethylene (A). In addition, from the viewpoint of the influence of foreign matter on mechanical properties, the content of the poly-β-alanine polymer (C) is preferably 3.0 parts by mass or less, more preferably 1.0 parts by mass or less, and even more preferably 0.5 parts by mass or less.

[0118] <(D) Polyamide polymer>

[0119] The polyoxymethylene composition of the present embodiment may contain (D) a polyamide polymer having a melting point of 140°C to 230°C.

[0120] The melting point of the polyamide polymer (D) is 140 to 230°C, preferably 150 to 200°C, and more preferably 150 to 180°C, from the viewpoint of productivity.

[0121] It is considered that the melting point of the polyamide polymer (D) is in the vicinity of the processing temperature range of the polyoxymethylene (A), so that the resin pressure in the extruder is reduced and the productivity is improved.

[0122] In addition, the melting point can be measured by the differential scanning calorimetry (DSC) method based on JIS K7121, and can be specifically measured by the method described in the Examples mentioned later.

[0123] As the (D) polyamide polymer, any of copolymer polyamides obtained by polycondensing lactams, diamines, dicarboxylic acids, and ω-aminocarboxylic acids alone or in a mixture of two or more thereof can be used, and at least one of them is preferably used.

[0124] (D) The polyamide polymer can be obtained by ring-opening polymerization of lactams, polycondensation of diamines and dicarboxylic acids, or self-condensation of aminocarboxylic acids, but is not limited thereto.

[0125] Specific examples of the lactams include ε-caprolactam, enantholactam, and ω-laurolactam.

[0126] The diamines can be roughly divided into aliphatic diamines, alicyclic diamines and aromatic diamines. Specific examples include tetramethylenediamine, hexamethylenediamine, undecamethylenediamine, dodecamethylenediamine, tridecamethylenediamine, 2,2,4-trimethylhexamethylenediamine, 2,4,4-trimethylhexamethylenediamine, 5-methylnonamethylenediamine, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, m-phenylenediamine, p-phenylenediamine, m-phenylenediamine, p-phenylenediamine and the like.

[0127] Dicarboxylic acids can be roughly divided into aliphatic dicarboxylic acids, alicyclic dicarboxylic acids and aromatic dicarboxylic acids. Specific examples include adipic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, 1,13-tridecanedioic acid, 1,3-cyclohexanedicarboxylic acid, terephthalic acid, isophthalic acid, naphthalene dicarboxylic acid, and dimer acid.

[0128] Specific examples of the aminocarboxylic acid include ε-aminocaproic acid, 7-aminoheptanoic acid, 8-aminooctanoic acid, 9-aminononanoic acid, 11-aminoundecanoic acid, 12-aminododecanoic acid, and 13-aminotridecanoic acid.

[0129] Examples of the polyamide polymer (D) include polyamide 6, polyamide 11, polyamide 12, polyamide 610, polyamide 612, polyamide 6 / 612, polyamide 6 / 66 / 610, etc. Among these, polyamide 6, polyamide 12, polyamide 610, and polyamide 6 / 66 / 610 are preferred, and polyamide 12 and polyamide 6 / 66 / 610 are more preferred from the viewpoint of productivity.

[0130] These polyamide polymers may be used alone or in combination of two or more.

[0131] As the (D) polyamide polymer, it is more preferable that the relative viscosity is 3.0 or less. The relative viscosity is more preferably 2.5 or less. When the relative viscosity is 3.0 or less, the productivity is excellent.

[0132] The relative viscosity was measured in accordance with JIS K6920-1: 2000. Specifically, a polyamide polymer was weighed at 1 g / 100 cm 3 The concentration of is dissolved in 98% concentrated sulfuric acid, the flow time measured by an Ostwald viscometer at 25°C is set to t1, the flow time of 98% concentrated sulfuric acid alone at 25°C is set to t0, and the relative viscosity is the value represented by "ηr=t1 / t0".

[0133] The content of the (D) polyamide polymer is preferably 0.001 to 0.1 parts by mass, more preferably 0.005 to 0.08 parts by mass, and still more preferably 0.005 to 0.05 parts by mass relative to 100 parts by mass of the (A) polyoxymethylene. When the addition amount of the (D) polyamide polymer is 0.001 parts by mass or more, productivity is improved, and when the addition amount of the (D) polyamide polymer is 0.1 parts by mass or less, the level of residual coloration can be maintained at a low level.

[0134] The mass ratio (D) / (B) of the polyamide polymer (D) relative to the boron nitride (B) is preferably in the range of 0.04 to 1.0, more preferably 0.07 to 0.7, and even more preferably 0.1 to 0.5. When the mass ratio (D) / (B) is in the above range, there is a tendency for a better balance between strength and acid resistance. Although it is hypothetical, it is believed that this is because both the boron nitride (B) and the polyamide polymer (D) have nitrogen atoms, which contribute to acid resistance as a base, and the two bases in different states, such as the boron nitride (B) present as a solid base in the polyoxymethylene (A) and the polyamide polymer (D) in a compatible state in the polyoxymethylene (A), interact with each other, and the acid can be effectively neutralized.

[0135] When the contents of (A) polyoxymethylene, (B) boron nitride, (C) poly-β-alanine polymer, and (D) polyamide polymer in the polyoxymethylene composition of the present embodiment are respectively within the above-mentioned specific ranges, a polyoxymethylene composition having particularly excellent acid resistance and thermal stability in addition to creep resistance and impact resistance can be provided, although the detailed mechanism is not yet clear.

[0136] <Other additives>

[0137] The polyoxymethylene composition of the present embodiment may further contain various additives such as pigments, dyes, various reinforcing materials, antioxidants, heat stabilizers, stabilizers such as formaldehyde and / or formic acid scavengers, weather stabilizers, release agents, lubricants, conductive agents, thermoplastic resins, thermoplastic elastomers, inorganic fillers or organic fillers, within a range that does not impair the properties of the polyoxymethylene (A).

[0138] These additives may be used alone or in combination of two or more.

[0139] The content of the additive in the polyoxymethylene composition is preferably 10 parts by mass or less relative to 100 parts by mass of (A) polyoxymethylene.

[0140] <Method for producing polyoxymethylene composition>

[0141] The polyoxymethylene composition of the present embodiment can be manufactured by mixing the above-mentioned essential components (A) and (B), optional components (C), (D), and other additive components using, for example, a Henschel mixer, a drum, a V-shaped mixer, etc., and then melt-kneading using a mixer such as a single-screw extruder or a twin-screw extruder, a heating roll, a kneader, a Banbury mixer, etc., and can be obtained in the form of products in various forms such as strands and granules. In addition, it is also possible to continuously supply each component to the extruder individually or several components at a time using a quantitative feeder without pre-mixing. In addition, it is also possible to prepare a high-concentration masterbatch containing each component in advance and dilute it with the polyoxymethylene (A) during extrusion melt kneading.

[0142] The kneading temperature may be determined according to the preferred processing temperature of the polyoxymethylene (A) used, and is usually set within the range of 180°C to 240°C, preferably within the range of 190°C to 230°C.

[0143] The granules of the polyoxymethylene composition obtained in the above manner can be dried in advance and used for the production of a molded body. There are no particular restrictions on the drying method, and examples thereof include drying methods using a box dryer (normal pressure, vacuum), a rotary and ventilated rotary dryer, a tank-type stirring dryer, a fluidized bed dryer, and the like.

[0144] The drying temperature is preferably 80° C. or higher, more preferably 100° C. or higher, in terms of the temperature of the heat medium. The drying time is preferably 0 to 10 hours, more preferably 0 to 6 hours, and even more preferably 1 to 6 hours, when the drying time is taken as the start time when the product temperature of the polyoxymethylene resin composition pellets reaches 100° C.

[0145] <Molded article of polyoxymethylene composition>

[0146] The molded article of the present embodiment includes the polyoxymethylene composition of the present embodiment. The pelletized product of the polyoxymethylene composition obtained as described above can be used to mold a desired molded article.

[0147] There is no particular restriction on the method for manufacturing the molded body, and any of the commonly used known molding methods can be applied, such as injection molding, extrusion molding, vacuum molding, blow molding, injection compression molding, decorative molding, heterogeneous material molding, gas-assisted injection molding, foam injection molding, low-pressure molding, ultra-thin-wall injection molding (ultra-high-speed injection molding), in-mold composite molding (insert molding, substrate injection molding), etc.

[0148] Example

[0149] The present invention will be described in more detail below by way of examples and comparative examples. It should be noted that the present invention is not limited to these examples.

[0150] [Various evaluation methods]

[0151] The following describes in detail various evaluation methods used in Examples and Comparative Examples.

[0152] (1) Average particle size of boron nitride

[0153] The average particle size of the boron nitride contained in the polyoxymethylene compositions of Examples and Comparative Examples was determined by obtaining an observation image of the boron nitride using a scanning microscope and performing image analysis. The measuring apparatus, conditions, and method are as follows.

[0154] Equipment: Scanning electron microscope (SEM) SU8220 manufactured by Hitachi High-Technologies Corporation

[0155] Accelerating voltage: 1.0 kV

[0156] Detector location: Top

[0157] Detection object: Secondary electron image

[0158] Image processing and analysis software: A-image-kun, manufactured by Asahi Chemical Engineering Co., Ltd.

[0159] Analytical Applications: Particle Analysis

[0160] Analysis parameters: (Brightness of particles) Bright, (Binarization method) Manual, (Range specification) No, (Edge correction) Four sides, (Hole filling) Yes, (Small pattern removal area) 10 pixels, (Correction method) Manual, (Noise removal filter) Yes, (Shadow) Yes, (Shadow size) 180, (Measurement item selection) Area

[0161] Boron nitride was sprinkled on a carbon tape attached to the SEM sample stage and fixed, osmium plasma coating was performed, and SEM observation was performed. The above-mentioned image processing and analysis software was used to edit the field of view image of 3.0μm×3.0μm range magnified to 50000 times into a binary image (manually adjusting the threshold so that the dark black part is the particle and the light black part is the grain boundary), and the longest particle size of at least 100 particles of boron nitride in the SEM image divided into particles and grain boundaries was measured, and the average value was taken as the average particle size (nm).

[0162] When measuring the average particle size of boron nitride contained in the polyoxymethylene composition, the boron nitride can be taken out by decomposing and removing the organic components in the polyoxymethylene composition by incineration or heat treatment in a nitrogen atmosphere, and then the above analysis can be performed.

[0163] (2) Boron nitride content

[0164] The content of boron nitride contained in the polyoxymethylene compositions of the examples and comparative examples was determined by quantitatively analyzing the boron element using an inductively coupled plasma mass spectrometer (ICP-MS) by the following method, and the content (parts by mass) of boron nitride based on 100 parts by mass of polyoxymethylene was determined from the boron content. The measuring device and method are as follows.

[0165] Apparatus: Inductively coupled plasma mass spectrometer (ICP-MS) manufactured by Thermo Fisher Scientific, model X series 2

[0166] First, as a pretreatment, 0.2 g of particles of the polyoxymethylene composition and 6 mL of a mixed acidic solution of nitric acid and hydrofluoric acid were added to a pressure-resistant sealed container made of polytetrafluoroethylene, and a microwave sample decomposition device (manufactured by Milestone, model: ETHOS UP) was used to perform a heating and pressurizing decomposition treatment using microwave radiation. The solution after the decomposition treatment was fixed to volume with ultrapure water to prepare a sample detection solution, and the mass analysis of the boron element was implemented by ICP-MS measurement. The content of boron nitride was calculated from the mass of the obtained boron. Regarding the calibration curve of the boron element, the boron ICP-MS standard solution (100 μg / mL aqueous solution, containing a trace amount of NH4OH) manufactured by AccuStandard was diluted with ultrapure water, and then an acidic solution of the same concentration as the sample detection solution was added to prepare a standard solution, and a calibration curve of the boron element was prepared by ICP-MS measurement.

[0167] (3) High temperature and high stress creep characteristics (rupture time)

[0168] Using an IS (100GN) injection molding machine manufactured by Toshiba Corporation, strip test pieces of 110 mm × 6.5 mm × 3 mm in size were molded from the pellets of the polyoxymethylene compositions of the examples and comparative examples under the conditions of a barrel temperature of 200°C, an injection pressure of 50 MPa, an injection speed of 30%, an injection time of 15 seconds, a cooling time of 25 seconds, and a mold temperature of 70°C, and were left standing for more than 24 hours under the conditions of an ambient temperature of 23°C ± 2°C and a humidity of 50% ± 10%. Using the left standing test piece and a creep tester (creep tester manufactured by Toyo Seiki Co., Ltd.: C200-6), a load of a tensile stress of 22 MPa was applied at a set temperature of 80°C ± 2°C, and the time until the test piece broke (break time (hours)) was measured. Three test pieces were prepared for each polyoxymethylene composition. The break time in Tables 1 and 2 represents the arithmetic mean time of n = 3.

[0169] The longer the time until fracture, the better the creep resistance to high stress load.

[0170] (4) Charpy impact strength

[0171] ISO dumbbell test pieces (with notch) for Charpy impact test were molded from the pellets of the polyoxymethylene compositions of the examples and comparative examples using a 5 ounce molding machine (manufactured by Toshiba Machine Co., Ltd., trade name "IS-100GN") with the barrel temperature set at 215°C, under the conditions of a mold temperature of 90°C, an injection time of 35 seconds, and a cooling time of 15 seconds. Six test pieces were prepared for each polyoxymethylene composition. The six test pieces were subjected to a Charpy impact test based on ISO179 / 1eA, and the Charpy impact strength (kJ / m 2). The values ​​shown in Table 1 and Table 2 are arithmetic mean values ​​of n=6.

[0172] The larger the value of the Charpy impact strength is, the better the impact resistance is.

[0173] (5) Thermal stability

[0174] The thermal stability of the pellets of the polyoxymethylene composition of the examples and comparative examples was evaluated. Using a differential thermal balance TG-DTA (manufactured by Rigaku Corporation, "Thermo plus EVO2"), the temperature was raised from 40°C to 225°C at a rate of 30°C / min at a nitrogen flow rate of 500 mL / min, and after being kept at 225°C for 60 minutes, the mass reduction rate (percentage) relative to the amount of the polyoxymethylene composition charged was calculated and used as an index of thermal stability.

[0175] (6) Acid resistance

[0176] ISO dumbbell test pieces for Charpy impact test were molded from the pellets of the polyoxymethylene compositions of the examples and comparative examples using a 5-ounce molding machine (manufactured by Toshiba Machine Co., Ltd., trade name "IS-100GN") with the barrel temperature set at 215°C, under the conditions of a mold temperature of 90°C, an injection time of 35 seconds, and a cooling time of 15 seconds. Four test pieces were prepared for each polyoxymethylene composition. 10 mL of sulfuric acid was added to a cylindrical glass container with a radius of 15 mm and a length of 200 mm, and the test piece was immersed in sulfuric acid, and was kept in a constant temperature bath at 23°C for 1 hour, and then the test piece was washed with water and the size was measured. If the dimensional change rate before and after sulfuric acid immersion is 5% or less, it is judged as "◎ (excellent)"; if the dimensional change rate before and after sulfuric acid immersion is greater than 5% and less than or equal to 8%, it is judged as "○ (good)"; if the dimensional change rate before and after sulfuric acid immersion is greater than 8% and less than or equal to 10%, it is judged as "△ (qualified)"; if the dimensional change rate before and after sulfuric acid immersion is greater than 10%, it is judged as "× (unqualified)". It should be noted that the dimensional change rate before and after sulfuric acid immersion is the arithmetic mean of n=4.

[0177] [Components used in Examples and Comparative Examples]

[0178] (A) Polyoxymethylene

[0179] An oxymethylene homopolymer stabilized by terminal acetylation (acetic acid esterification) having an MFR value (based on ISO 1133, 190° C., 2.16 kg load) of 2 g / 10 minutes was used.

[0180] (B) Boron Nitride

[0181] (B-1)

[0182] EM Japan Co., Ltd. sells Boron Nitride Nanoparticles NP-BN-2

[0183] The average particle size is 80nm.

[0184] (B-2)

[0185] ALLIANCE Biosystems sells Boron Nitride Ultrafine Powder BN-NANO5

[0186] The average particle size is 70 nm.

[0187] (B-3)

[0188] Made by Mizushima Iron & Steel Co., Ltd., product name: Boron Nitride FS-1 for special applications in BN industry

[0189] The average particle size is 250nm.

[0190] (B-4)

[0191] Denka Corporation, trade name: Denka Boron Nitride SP-2

[0192] The average particle size is 500nm.

[0193] (B-5)

[0194] Manufactured by Showa Denko K.K., trade name: Boron nitride powder UHP-S2

[0195] The average particle size is 700nm.

[0196] (B-6)

[0197] Manufactured by Mizushima Alloy Steel Co., Ltd., product name: Boron Nitride HP-P1 for special applications in BN industry

[0198] The average particle size is 1000nm.

[0199] (C) Poly-β-alanine polymer

[0200] (C-1)

[0201] In a 5L batch reactor equipped with a stirrer, 2400g of acrylamide and 1.08g of calcium propionate as a catalyst (1 / 5000 mole relative to acrylamide) were added, and the mixture was reacted at 125°C for 4 hours while stirring in a N2 gas stream. After the reaction, the solid was crushed, then washed with acetone and dried. The primary amide group content and reduced viscosity of the obtained polymer are as follows.

[0202] The content of primary amide groups was 45.0 mol%.

[0203] Reduced viscosity is 2.3 dL / g.

[0204] (C-2)

[0205] In a 5L batch reactor equipped with a stirrer, 2400g of acrylamide and 0.81g of calcium propionate as a catalyst (1 / 7500 mole relative to acrylamide) were added, and the mixture was reacted at 125°C for 4 hours while stirring in a N2 gas stream. After the reaction, the solid was crushed, then washed with acetone and dried. The primary amide group content and reduced viscosity of the obtained polymer are as follows.

[0206] The content of primary amide groups was 63.0 mol%.

[0207] Reduced viscosity: 2.31 dL / g.

[0208] (C-3)

[0209] 2400 g of acrylamide and 0.54 g of calcium propionate as a catalyst (1 / 10000 mole relative to acrylamide) were added to a 5L batch reactor equipped with a stirrer, and reacted at 125°C for 4 hours while stirring in a N2 gas stream. After the reaction, the solid was crushed, then washed with acetone and dried. The primary amide group content and reduced viscosity of the obtained polymer are as follows.

[0210] The content of primary amide groups was 75.0 mol%.

[0211] Reduced viscosity is 2.4 dL / g.

[0212] (Determination of the content of primary amide groups)

[0213] The content of the primary amide group of the above-mentioned poly-β-alanine polymer is determined as follows. First, a poly-β-alanine polymer and a 40% by mass potassium hydroxide aqueous solution are added to a flask with a stirrer, and heated at 105°C to 110°C for 20 minutes while stirring to hydrolyze the primary amide group into ammonia. Next, the contents of the flask are cooled to below 50°C, and then methanol is added to extract the ammonia together with the methanol. The extract is absorbed in a 0.1 normal aqueous sulfuric acid solution, and methyl red is used as an indicator, and a 0.1 normal aqueous sodium hydroxide solution is used for neutralization titration to determine the content of the primary amide group.

[0214] (Determination of reduced viscosity)

[0215] The reduced viscosity of the above-mentioned poly-β-alanine polymer is calculated as follows. First, 5 g of poly-β-alanine polymer is added to 100 mL of formic acid and stirred at room temperature for 2 hours to dissolve it. Then, it is filtered under reduced pressure to obtain a formic acid solution. 500 mL of methanol is added to the formic acid solution to precipitate the formic acid solution, the precipitate is filtered, and then dried under reduced pressure at 80° C. in a vacuum dryer for 10 hours. The obtained sample is dissolved in formic acid with a purity of more than 99%, and then passed through a 200-mesh filter material to prepare a sample solution with a sample concentration of 1 g / dL. The falling time of the sample solution at a temperature of 35° C. is measured using an Ostwald viscometer, and the reduced viscosity ηsp / c (dL / g) is calculated by the following formula.

[0216] ηsp / c=(t / t0-1) / c

[0217] (Wherein, t is the falling time of the sample solution (seconds), t0 is the falling time of the formic acid solution (seconds), and c is the concentration of the sample solution (g / dL).)

[0218] (D) Polyamide polymer

[0219] (D-1) Polyamide 6 / 66 / 610 copolymer

[0220] 0.45 kg of an equimolar salt of adipic acid and hexamethylenediamine, 0.32 kg of an equimolar salt of sebacic acid and hexamethylenediamine, 1.67 kg of ε-caprolactam and 2.5 kg of pure water were added to a 5L autoclave and stirred thoroughly. The atmosphere was fully replaced with N2, and then the temperature was raised from room temperature to 220°C over about 1 hour while stirring. At this time, the internal pressure of the autoclave was 18 kg / cm2 based on the natural pressure gauge generated by water vapor. 2 -G, remove water from the reaction system so that it does not reach 18kg / cm 2 -G or higher pressure, and continue heating. When the internal temperature reaches 230°C, stop heating, close the discharge valve of the autoclave, and cool to room temperature in about 8 hours. After cooling, open the autoclave, take out about 2 kg of polymer and crush it into powder. The melting point is 150°C and the relative viscosity is 2.0.

[0221] (D-2) Polyamide 12

[0222] Made by Daicel Degussa Corporation. Trade name: DAIAMID L1700

[0223] The dispersibility of the granular material was problematic, so it was crushed to powder. The melting point was 178°C and the relative viscosity was 1.7.

[0224] (D-3) Polyamide 66

[0225] 2.5 kg of an equimolar salt of adipic acid and hexamethylenediamine and 2.5 kg of pure water were added to a 5 L autoclave and stirred thoroughly. The atmosphere was fully replaced with N2 and then the temperature was raised from room temperature to 220°C over about 1 hour while stirring. At this time, the internal pressure of the autoclave reached 18 kg / cm2 using the natural pressure gauge generated by the water vapor. 2 -G, remove water from the reaction system so that it does not reach 18kg / cm 2 -G or higher pressure, and continue heating. When the internal temperature reaches 260°C, stop heating, close the discharge valve of the autoclave, and cool to room temperature in about 8 hours. After cooling, open the autoclave, take out about 2 kg of polymer and crush it into powder. The melting point is 260°C and the relative viscosity is 2.0.

[0226] (Determination of Melting Point)

[0227] The melting point of the polyamide polymer is measured according to JIS K7121 using a differential scanning calorimeter ("DSC 8000" manufactured by PerkinElmer). 8 mg of the polyamide polymer is accurately weighed and used for measurement. The measurement conditions are: in a nitrogen atmosphere, the temperature is increased from 50°C to 300°C at a heating rate of 20°C / min, maintained at 300°C for 5 minutes, then cooled to 50°C at a cooling rate of 20°C / min, and then heated from 50°C to 300°C at a heating rate of 20°C / min. The peak indicating endothermic absorption is taken as the peak indicating the melting of the polyamide polymer, and the temperature (°C) of the peak indicating endothermic absorption that appears on the highest temperature side is taken as the melting point of the polyamide polymer.

[0228] (Determination of relative viscosity)

[0229] The relative viscosity of the polyamide polymer is 1 g / 100 cm according to JIS K6920-1:2000. 3 When a polyamide polymer is dissolved in 98% concentrated sulfuric acid at a concentration of , and the flow time measured by an Ostwald viscometer at 25°C is set to t1, and the flow time of 98% concentrated sulfuric acid alone at 25°C is set to t0, the relative viscosity of the polyamide polymer is calculated by the formula "relative viscosity ηr = t1 / t0".

[0230] (E) Hindered phenolic antioxidants

[0231] Manufactured by BASF Corporation. Trade name: Irganox (registered trademark) 245

[0232] [Example 1]

[0233] A mixture was obtained by uniformly mixing (A) 100 parts by mass of polyoxymethylene, (B-1) 0.02 parts by mass of boron nitride, (C-1) 0.1 parts by mass of poly-β-alanine polymer, (D-1) 0.02 parts by mass of polyamide polymer, and (E) 0.2 parts by mass of antioxidant ((D) / (B) mass ratio = 1) using a Henschel mixer. The mixture was melt-kneaded using a 30φ single-screw extruder, extruded into strands, cooled, and granulated to obtain pellets containing a polyoxymethylene composition. The extrusion conditions were as follows: the barrel setting temperature was set to 200°C, the discharge volume was set to 5kg / hour, the screw speed was set to 50rpm, and the exhaust port pressure reduction was set to -720mmHg. The obtained pellets were dried at 80°C for 4 hours. The dried pellets were used to evaluate (2) boron nitride content, (3) high temperature high stress creep characteristics (rupture time), (4) Charpy impact strength, (5) thermal stability, and (6) acid resistance by the above-mentioned various evaluation methods. The evaluation results are shown in Table 1.

[0234] [Examples 2 to 22]

[0235] The component composition of the polyoxymethylene composition was changed as shown in Tables 1 and 2. The same operation as in Example 1 was performed to obtain dried polyoxymethylene composition pellets, which were evaluated in the same manner. The evaluation results are shown in Tables 1 and 2.

[0236] [Comparative Examples 1 to 5]

[0237] The component composition of the polyoxymethylene composition was changed as shown in Table 2. The same operation as in Example 1 was carried out except for the above to obtain dried polyoxymethylene composition pellets, which were evaluated in the same manner. The evaluation results are shown in Table 2.

[0238]

[0239]

[0240] From the results in Tables 1 and 2, it can be seen that by preparing a polyoxymethylene composition containing (A) polyoxymethylene and (B) boron nitride having a specific particle size in a specified content, a polyoxymethylene composition having high high-stress creep resistance, impact resistance, acid resistance and thermal stability is obtained.

[0241] Industrial Applicability

[0242] As described above, the polyoxymethylene composition of the present invention eliminates the contradiction between creep resistance and impact strength caused by the addition of a crystal nucleating agent, has high creep resistance and high impact strength under high stress, and is also excellent in acid resistance and thermal stability. Therefore, it can be suitably used for mechanical parts of automobiles, etc. that require reliability, or mechanical parts of equipment used under severe usage conditions, etc.

Claims

1. A polyoxymethylene composition, characterized in that: The polyoxymethylene composition comprises 100 parts by mass of (A) polyoxymethylene, 0.01 to 0.5 parts by mass of (B) boron nitride, 0.01 to 3.0 parts by mass of (C) poly-β-alanine polymer containing 30 to 70 mol % of primary amide groups, and one or more additives selected from the group consisting of a pigment, a dye, a reinforcing material, an antioxidant, a heat stabilizer, a formaldehyde and / or formic acid scavenger, a weathering stabilizer, a conductive agent, a thermoplastic resin, a thermoplastic elastomer, and an inorganic filler, or The polyoxymethylene composition comprises 100 parts by mass of (A) polyoxymethylene, 0.01 to 0.5 parts by mass of (B) boron nitride, 0.01 to 3.0 parts by mass of (C) poly-β-alanine polymer containing 30 mol % to 70 mol % of primary amide groups, and 0.001 to 0.1 parts by mass of (D) polyamide polymer having a melting point of 140° C. to 230° C., and one or more additives selected from the group consisting of pigments, dyes, reinforcing materials, antioxidants, heat stabilizers, formaldehyde and / or formic acid scavengers, weather stabilizers, conductive agents, thermoplastic resins, thermoplastic elastomers, and inorganic fillers. The boron nitride (B) has an average particle size of 100 to 800 nm of at least 100 particles in a field of view image of 3.0 μm×3.0 μm obtained by a scanning electron microscope at a magnification of 50,000 times, obtained using image processing analysis software.

2. The polyoxymethylene composition according to claim 1, wherein The average particle size of the (B) boron nitride is 80 nm to 500 nm.

3. The polyoxymethylene composition according to claim 1 or 2, wherein The average particle size of the (B) boron nitride is 100 nm to 500 nm.

4. The polyoxymethylene composition according to claim 1 or 2, wherein The content of the (B) boron nitride is 0.02 to 0.5 parts by mass.

5. The polyoxymethylene composition according to claim 1 or 2, wherein The content of the (B) boron nitride is 0.3 parts by mass or less.

6. The polyoxymethylene composition according to claim 1 or 2, wherein The content of the (B) boron nitride is 0.2 parts by mass or less.

7. The polyoxymethylene composition according to claim 1 or 2, wherein The (B) boron nitride is hexagonal boron nitride.

8. The polyoxymethylene composition according to claim 1 or 2, wherein The (A) polyoxymethylene is any one of a polyoxymethylene homopolymer, a polyoxymethylene copolymer, and a mixture of a polyoxymethylene homopolymer and a polyoxymethylene copolymer.

9. The polyoxymethylene composition according to claim 1 or 2, wherein The content of primary amide groups in the (C) poly-β-alanine polymer is 35 mol % to 65 mol %.

10. The polyoxymethylene composition according to claim 1 or 2, wherein The content of the primary amide group in the (C) poly-β-alanine polymer is 40 mol % to 60 mol %.

11. The polyoxymethylene composition according to claim 1 or 2, wherein The content of the (C) poly-β-alanine polymer is 0.05 parts by mass or more.

12. The polyoxymethylene composition according to claim 1 or 2, wherein The content of the (C) poly-β-alanine polymer is 1.0 part by mass or less.

13. The polyoxymethylene composition according to claim 1 or 2, wherein The content of the (C) poly-β-alanine polymer is 0.5 parts by mass or less.

14. The polyoxymethylene composition according to claim 1 or 2, wherein The poly-β-alanine polymer (C) comprises a structural unit (3) represented by the following formula (3) and a structural unit (4) represented by the following formula (4) in a total content of 95 mol % or more, [-CH2-CH2-CONH-] ……(3) [-CH2-CH-] | CONH2……(4).

15. The polyoxymethylene composition according to claim 1 or 2, wherein The (C) poly-β-alanine polymer has a molecular weight corresponding to a reduced viscosity (ηsp / c) of 0.5 dL / g to 15 dL / g.

16. The polyoxymethylene composition according to claim 1 or 2, wherein The (C) poly-β-alanine polymer has a molecular weight corresponding to a reduced viscosity (ηsp / c) of 1 dL / g to 10 dL / g.

17. The polyoxymethylene composition according to claim 1 or 2, wherein The (C) poly-β-alanine polymer has a molecular weight corresponding to a reduced viscosity (ηsp / c) of 2 dL / g to 5 dL / g.

18. The polyoxymethylene composition according to claim 1 or 2, wherein: The (D) polyamide polymer has a melting point of 150°C to 200°C.

19. The polyoxymethylene composition according to claim 1 or 2, wherein The (D) polyamide polymer has a melting point of 150°C to 180°C.

20. The polyoxymethylene composition according to claim 1 or 2, wherein The content of the (D) polyamide polymer is 0.005 to 0.08 parts by mass.

21. The polyoxymethylene composition according to claim 1 or 2, wherein The content of the (D) polyamide polymer is 0.005 to 0.05 parts by mass.

22. The polyoxymethylene composition according to claim 1 or 2, wherein The (D) polyamide polymer is one or more selected from the group consisting of polyamide 6, polyamide 11, polyamide 12, polyamide 610, polyamide 612, polyamide 6 / 612 and polyamide 6 / 66 / 610.

23. The polyoxymethylene composition according to claim 1 or 2, wherein The relative viscosity of the (D) polyamide polymer is 3.0 or less.

24. The polyoxymethylene composition according to claim 1 or 2, wherein: The relative viscosity of the (D) polyamide polymer is 2.5 or less.

25. The polyoxymethylene composition according to claim 1 or 2, wherein: The mass ratio (D) / (B) of the polyamide polymer (D) to the boron nitride (B) is 0.04 to 1.

0.

26. The polyoxymethylene composition according to claim 1 or 2, wherein: The mass ratio (D) / (B) of the polyamide polymer (D) to the boron nitride (B) is 0.07 to 0.

7.

27. The polyoxymethylene composition according to claim 1 or 2, wherein: The mass ratio (D) / (B) of the polyamide polymer (D) to the boron nitride (B) is 0.1 to 0.

5.

28. The polyoxymethylene composition according to claim 1 or 2, wherein: The dimensional change rate of a test piece molded using the polyoxymethylene composition before and after being immersed in sulfuric acid at 23° C. for 1 hour is 10% or less.