Integral reinforcement method of masonry structure based on Fe-SMA self-prestressing
Through Fe-SMA self-prestressed overall reinforcement method of masonry structure, Fe-SMA material is used to generate recovery stress under complex stress states, which solves the shortcomings of the existing caulking reinforcement method in the old mortar restraint and overall reinforcement effect, and achieves It provides efficient masonry structure reinforcement and is suitable for the protection of historical buildings.
Patent Information
- Application Number
- CN202210873662.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-21
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-07-21
AI Technical Summary
The existing caulking reinforcement method has limited ability to constrain old mortar and cannot give full play to the performance of new materials under complex stress conditions. It is only applicable to a single building component, making it difficult to improve the overall performance of the house. It is especially deficient in the protection of historical and cultural relics. .
The Fe-SMA self-prestressed overall reinforcement method of the masonry structure is adopted. By determining the area to be reinforced, the original mortar joints are removed and filled with high-performance mortar, the pre-stretched Fe-SMA material is embedded, and the Fe-SMA is energized to excite the equipment. The SMA material generates recovery stress to achieve overall reinforcement.
It achieves a better low-intervention reinforcement effect, improves the pressure-bearing capacity and out-of-plane collapse resistance of the masonry structure, simplifies the construction process, reduces the disturbance to the masonry structure, and is suitable for the protection of historical and cultural relics buildings.
Smart Images

Figure CN115199076B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of masonry structure reinforcement, in particular to an integral reinforcement method of a masonry structure based on Fe-SMA self-prestressing. Background Art
[0002] During the thousands of years of development in my country, masonry structures have been widely used as a cost-effective, simple and practical building form, becoming one of the most important forms of building structures in my country. However, due to the poor mechanical properties of masonry structures, the lack of structural protection measures, the change of the use function of many houses and the disrepair over the years, many masonry structures are in urgent need of repair and reinforcement.
[0003] However, many existing reinforcement methods have interfered too much with the original masonry structure, resulting in a reduction in the user-usable area and damage to the exterior architectural style, making it difficult to meet the minimum intervention principle and various aesthetic and practical requirements for the reinforcement of masonry structures, especially historical and cultural relics. In recent years, the caulking reinforcement method has been widely used as an increasingly popular low-intervention reinforcement method. This method replaces part of the low-strength mortar of the original masonry structure in a certain way and replaces it with high-performance mortar, thereby achieving the purpose of improving the seismic performance of the masonry structure. This method is particularly suitable for masonry structures with weak mortar performance, and can have a certain reinforcement effect on the masonry structure without reducing the usable area of the house and affecting the appearance of the building.
[0004] The current caulking reinforcement method usually adopts two methods: directly embedding high-performance mortar after removing the joints, or embedding reinforcing bars and high-performance mortar after removing the joints. However, these two methods have limited ability to restrain the old mortar, especially when the building is in use, and cannot work well with the building. It is impossible to fully exert the performance of the new caulking material under the complex stress state of tension, compression, bending and shearing of the mortar joints, and the reinforcement effect is limited. At the same time, the current caulking reinforcement method is only applicable to one component of the building, such as only for the reinforcement of a wall, which is of little significance to the improvement of the overall performance of the house.
[0005] Therefore, the prior art requires a reinforcement method that can make good use of the performance of caulking materials, work better with buildings, and systematically complete the reinforcement and repair of buildings from the perspective of the entire building. This method should improve the effect of the caulking reinforcement method and be widely used in a series of masonry structures that need to be reinforced, such as historical and cultural relics protection buildings. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a method for overall reinforcement of masonry structures based on Fe-SMA self-prestressing in view of the deficiencies of the above-mentioned prior art. The method for overall reinforcement of masonry structures based on Fe-SMA self-prestressing determines the area to be reinforced of the structure, uses corresponding tools to remove the original mortar joints in the area to be reinforced to a specified depth, cleans the mortar joints, and uses different reinforcement methods in the mortar joints at different positions and fills them with high-performance mortar, embeds pre-stretched Fe-SMA materials in the mortar joints filled with high-performance mortar, and reserves energized positions, and after the mortar curing is completed, uses energized excitation equipment to connect the pre-stretched Fe-SMA materials through the reserved energized positions to perform energized heating operations, so that the Fe-SMA materials generate restoring stress, thereby realizing overall reinforcement of masonry structures based on Fe-SMA energized excitation self-prestressing technology.
[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0008] A method for integrally reinforcing a masonry structure based on Fe-SMA self-prestressing comprises the following steps.
[0009] Step 1: Determine the area to be reinforced: Determine the area to be reinforced based on the structural characteristics of the masonry structure to be reinforced and the damaged location to be reinforced.
[0010] Step 2: Remove the mortar joints, which specifically includes the following steps.
[0011] Step 2A, select the frequency of removing seams: For each area to be reinforced determined in step 1, select the original seams as the seams to be removed in a top-to-bottom or bottom-to-top order and at a set interval frequency.
[0012] Step 2B, removing gray seams: remove each gray seam selected in step 2A.
[0013] Step 3: Fill the joints: Fill each joint with high-performance mortar.
[0014] Step 4: Embedding Fe-SMA material: embed pre-stretched Fe-SMA material in the chisel filled with high-performance mortar, and reserve a position for power supply.
[0015] Step 5, strengthening the masonry structure: after the high-performance mortar is cured to the specified strength, an energized excitation device is used to connect the pre-stretched Fe-SMA material through the reserved energized position for energized excitation, so that the Fe-SMA material generates restoring stress to complete the overall reinforcement of the masonry structure.
[0016] In step 1, the specific method for determining the area to be reinforced is:
[0017] A. When the masonry structure to be reinforced has a ring beam, only the entire wall to be reinforced needs to be regarded as the area to be reinforced.
[0018] B. When the masonry structure to be reinforced has no ring beam, the top annular wall area close to each floor slab and the entire wall to be reinforced shall be the area to be reinforced; among them, the joints corresponding to the top annular wall area located at each floor slab are called annular joints.
[0019] In step 3, before filling in the high-performance mortar, when the masonry structure to be reinforced has no ring beam, an L-shaped steel sheet is installed at each corner of the top annular wall area of each floor slab, and the L-shaped steel sheet has an embedded portion corresponding to the annular joint, and the embedded portion can be embedded in the corresponding annular joint.
[0020] In step 4, when the masonry structure to be reinforced has no ring beam, the Fe-SMA material is embedded in the annular joint in a closed loop.
[0021] In step 1, when the masonry structure to be reinforced has no ring beam, the height of the top annular wall area is 4-8 bricks; and there are at least two annular joints.
[0022] In step 2A, the interval frequency of selecting the joints to be removed is set to remove once every 1-4 original joints; in step 2B, the depth of the joints is 10%-30% of the wall thickness, and the height of the joints is consistent with the original joint height.
[0023] The height and depth of the embedded part of the L-shaped steel sheet should correspond to the height and depth of the annular chiseling, and the deviation should be controlled within 10% of the corresponding height or corresponding depth. The length is generally not less than the length of one building block; the embedded part is formed by mold making or mechanical extrusion.
[0024] In step 4, the embedding depth of the Fe-SMA material in the high-performance mortar is not less than 10% of the corresponding chiseling depth.
[0025] In step 5, the power-on excitation device refers to a low-voltage, high-current, high-power electrical device with an output voltage lower than 36V and an output current greater than 100A, which can electrically heat the Fe-SMA material.
[0026] In step 5, when the power is turned on for excitation, the heating temperature is 200°C.
[0027] The present invention has the following beneficial effects:
[0028] 1. The present invention can reduce disturbance to the masonry structure to the greatest extent.
[0029] 2. In the present invention, the component to be reinforced does not need to be provided with a support system, which simplifies the construction process and reduces the investment in manpower and material resources.
[0030] 3. Achieve the best low-intervention reinforcement effect, improve the bearing capacity, overall performance and anti-out-of-plane collapse ability of the masonry structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The present invention is a flow chart of a method for integrally reinforcing a masonry structure based on Fe-SMA self-prestressing.
[0032] Figure 2 The figure is a schematic diagram of the structure of an L-shaped steel sheet installed in the top annular wall area of the present invention.
[0033] Figure 3 It is a cross-sectional view of the unreinforced structural wall after the seams are removed in the embodiment.
[0034] Figure 4 It is a cross-sectional view of a wall after caulking is completed in an embodiment.
[0035] Figure 5 This is a schematic diagram of the completed house reinforcement in the embodiment.
[0036] The accompanying drawings are denoted as follows:
[0037] 1-Block, 2-Original mortar, 3-L-shaped steel sheet, 4-High-performance mortar, 5-Fe-SMA material, 6-Floor slab. DETAILED DESCRIPTION
[0038] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific preferred embodiments.
[0039] In the description of the present invention, it should be understood that the terms "left side", "right side", "upper part", "lower part" and the like indicate the orientation or positional relationship based on the orientation or positional relationship shown in the drawings, which is only for the convenience of describing the present invention and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation. "First", "second" and the like do not indicate the importance of the components, and therefore cannot be understood as limiting the present invention. The specific dimensions used in this embodiment are only for illustrating the technical solution, and do not limit the scope of protection of the present invention.
[0040] like Figure 1 As shown, a method for overall reinforcement of masonry structure based on Fe-SMA self-prestressing comprises the following steps.
[0041] Step 1: Determine the area to be reinforced: Determine the area to be reinforced of the masonry structure based on the structural characteristics of the masonry structure to be reinforced and the damaged location to be reinforced.
[0042] In step 1, the specific method for determining the area to be reinforced is as follows.
[0043] A. When the masonry structure to be reinforced has a ring beam, only the entire wall to be reinforced needs to be regarded as the area to be reinforced.
[0044] B. When the masonry structure to be reinforced has no ring beam, the top annular wall area close to each floor slab and the entire wall to be reinforced are required to be the area to be reinforced; wherein, the joints corresponding to the top annular wall area located on each floor slab are called annular joints. The height of the top annular wall area is preferably 4-8 bricks; there are at least two annular joints. For example, the area of 6 bricks on the top of the 4 walls of each floor of a house with a rectangular cross section is selected to form a closed loop.
[0045] Step 2: Remove the gray seams, which specifically includes the following steps:
[0046] Step 2A, select the frequency of removing seams: For each area to be reinforced determined in step 1, select the original seams as the seams to be removed in a top-to-bottom or bottom-to-top order and at a set interval frequency.
[0047] The set interval frequency when selecting the gray seams to be removed is preferably once for every 1-4 original gray seams.
[0048] Step 2B, removing mortar joints: use a blower to clean the mortar joints, and remove each mortar joint selected in step 2A; the depth of the joint removal is preferably 10%-30% of the wall thickness, and the height of the joint removal is preferably consistent with the original mortar joint height. The preferred joint removal tool for joint removal refers to a tool that can remove the original mortar joint to a specified depth, including but not limited to electric drills, circular saws, high-pressure water jet joint removal machines and other joint removal tools.
[0049] In this embodiment, the tops of the four walls at the bottom of the structural floor without a ring beam and two of the walls are selected as the seam-cutting areas. An original mortar seam is selected every two blocks.
[0050] Use an electric drill to remove the seams of the original mortar 2 from top to bottom. The depth of the seams is 20% of the thickness of the masonry to be reinforced. The length is slightly less than the length of the wall. The amplitude is controlled at 20mm. The height should be consistent with the mortar joint. Try not to damage the original masonry block 1 during the process. Figure 3 As shown. Select the first brick under the floor slab as the starting point to remove the joints. Among them, the first two joints to be removed, that is, the two joints to be removed closest to the floor slab, should be removed from four walls to form a circumferential joint. For the rest, only the joints of the selected walls should be removed.
[0051] For the positions near each floor slab of the masonry structure without ring beam, after the ring joint is removed, the ring reinforcement is adopted. Specifically, first, at the corner of the ring area removed under the masonry structure floor slab without ring beam, usually the corner of the wall of the area sandwiched between the removed ring joint and the area included by the upper and lower bricks of the removed ring joint, that is, the corner of the wall of the ring joint area, L-shaped steel sheets that can be embedded in the removed joint are installed, so as to avoid uneven force on the end blocks at the corner when prestress is applied, which affects the reinforcement effect.
[0052] That is, when the masonry structure to be reinforced has no ring beam, L-shaped steel sheets are installed at the four corners of the top annular wall area of each floor slab. The installation diagram of the L-shaped steel sheet and the top annular wall area is as follows: Figure 2 and Figure 5 shown.
[0053] The L-shaped steel sheet has an embedding portion corresponding to the annular chisel, and the embedding portion can be embedded in the corresponding annular chisel.
[0054] In this embodiment, the L-shaped steel sheet refers to a steel sheet made of ordinary steel, with a top and bottom height of about 200mm, a left and right single-side limb width of about 250mm, and a thickness of 2-20mm. The steel sheet can be formed into at least one groove that can be embedded in the removed seam through a mold or mechanical extrusion. The groove needs to be chamfered at the turning point and can be bent 90° along the center line of the steel sheet. The height and depth of the extruded groove-shaped embedded part should be slightly smaller than the corresponding size of the removed seam, and the amplitude is generally controlled within 2mm. The total length of the embedded part is consistent with the total length of the steel sheet. The steel sheet is inserted into the removed seam through the embedded part, and the unextruded left and right flat surfaces are fitted with the walls on both sides of the structural corner, thereby achieving installation, so that when prestress is applied, the blocks at the corners of the wall can better cooperate with the mortar to bear force.
[0055] Step 3, filling mortar joints: high-performance mortar is filled into each chink. The high-performance mortar in this embodiment refers to a mortar that can be used in masonry structure construction and whose mechanical properties are substantially unaffected at a high temperature of at least 200°C.
[0056] Step 4, embedding Fe-SMA material: embed pre-stretched Fe-SMA material in the chisel filled with high-performance mortar, and reserve a power-on position. Reserving a power-on position means reserving a position capable of connecting the Fe-SMA material so that the Fe-SMA material can form a closed loop with the power-on excitation device after being connected to the power-on excitation device, including but not limited to connecting a power-on wire with a length exceeding the chisel depth at the end of the Fe-SMA material and leading the wire out of the mortar, reserving a position of a certain width at the end of the Fe-SMA material without embedding the mortar so that the power-on device can be connected later, and other measures.
[0057] Fe-SMA materials refer to industrial products of various shapes that are bendable or can be bent, made of iron-based shape memory alloys, including but not limited to Fe-SMA ribs, Fe-SMA strips, Fe-SMA wire ropes, etc. The diameter or height should be smaller than the thickness of the plastered seam and the height of the angle steel groove.
[0058] The principle of embedding Fe-SMA materials is: for masonry structures without ring beams, near each floor slab, usually at least two circumferential mortar joints cut near the floor slab, pre-stretched Fe-SMA materials are embedded in the mortar joints filled with high-performance mortar, so that the Fe-SMA materials are buried in the mortar for at least 10% of the corresponding depth of the joints. The Fe-SMA materials embedded in this area should form a closed loop, pressing the steel sheet in the mortar joints of the joints cut at the corners of the structure, so that a hoop force can be formed when prestress is applied, producing a similar effect to the ring beam, and forming an overall reinforcement for the structure. The measures for the Fe-SMA materials in this area to form a closed loop can be to bolt or weld the ends of the Fe-SMA materials embedded in the two walls at the same steel sheet position and embed them in the high-performance mortar; or to use a bendable Fe-SMA material to hoop the entire structure, and after the two ends are embedded in the mortar to form a closed loop, they are connected by screws or welded, and then the connection parts are buried in the high-performance mortar. For other locations of the masonry structure, usually various walls, Fe-SMA materials with a length slightly smaller than the length of the removed mortar joints are embedded in the mortar joints.
[0059] That is, when the masonry structure to be reinforced has no ring beam, the Fe-SMA material is embedded in the annular joint in a closed loop.
[0060] Furthermore, the embedding depth of the Fe-SMA material in the high-performance mortar is not less than 10% of the corresponding chiseling depth.
[0061] Step 5, strengthening the masonry structure: after the high-performance mortar is cured to the specified strength, such as after 28 days of curing, an energized excitation device is used to connect the pre-stretched Fe-SMA material through the reserved energized position for energized excitation, so that the Fe-SMA material generates restoring stress to complete the overall reinforcement of the masonry structure.
[0062] The above-mentioned power-on excitation device refers to a low-voltage, high-current, high-power electrical device with an output voltage lower than 36V and an output current greater than 100A, which can heat the Fe-SMA material by power-on. When power-on excitation is performed, the power-on heating temperature is preferably 200°C.
[0063] The preferred embodiments of the present invention are described in detail above; however, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, various equivalent transformations can be made to the technical solutions of the present invention, and these equivalent transformations all belong to the protection scope of the present invention.
Claims
1. A method for integral reinforcement of masonry structures based on Fe-SMA self-prestressing, characterized in that: The steps include: Step 1: Determine the area to be reinforced: Determine the area to be reinforced according to the structural characteristics of the masonry structure to be reinforced and the damaged location to be reinforced; the specific method for determining the area to be reinforced is as follows: A. When the masonry structure to be reinforced has a ring beam, only the entire wall to be reinforced is used as the area to be reinforced; B. When the masonry structure to be reinforced has no ring beam, the top annular wall area close to each floor slab and the entire wall to be reinforced shall be the area to be reinforced; wherein, the height of the top annular wall area is 4-8 bricks; the joints corresponding to the top annular wall area located at each floor slab are called annular joints; there are at least two annular joints; Step 2: Remove the gray seams, which specifically includes the following steps: Step 2A, selecting the frequency of seam removal: for each area to be reinforced determined in step 1, the original mortar seams are selected as the mortar seams to be removed in a top-to-bottom or bottom-to-top order and at a set interval frequency; Step 2B, removing gray seams: removing each gray seam to be removed selected in step 2A; Step 3, filling the mortar joints: high-performance mortar is filled in each joint; before the high-performance mortar is filled, when the masonry structure to be reinforced has no ring beam, an L-shaped steel sheet is installed at each corner of the annular wall area at the top of each floor slab, and the L-shaped steel sheet has an embedded portion corresponding to the annular joint, and the embedded portion can be embedded in the corresponding annular joint, and the embedded portion is formed by a mold or mechanical extrusion to form at least one groove that can be embedded in the joint to be mortared, and the groove needs to be chamfered at the turning point, and can be bent 90° along the center line of the steel sheet; Step 4, embedding Fe-SMA material: embed pre-stretched Fe-SMA material in the joints filled with high-performance mortar, and reserve the position for power supply; when the masonry structure to be reinforced has no ring beam, the Fe-SMA material is embedded in the annular joint in a closed loop; press the L-shaped steel sheet in the mortar joint of the joint area at the corner of the structure, so that hoop force can be formed when prestressing is applied, so as to form an overall reinforcement for the structure; Step 5, strengthening the masonry structure: after the high-performance mortar is cured to the specified strength, an energized excitation device is used to connect the pre-stretched Fe-SMA material through the reserved energized position for energized excitation, so that the Fe-SMA material generates restoring stress to complete the overall reinforcement of the masonry structure.
2. The method for integral reinforcement of masonry structure based on Fe-SMA self-prestressing according to claim 1 is characterized in that: In step 2A, the interval frequency of selecting the joints to be removed is set to remove once every 1-4 original joints; in step 2B, the depth of the joints is 10%-30% of the wall thickness, and the height of the joints is consistent with the original joint height.
3. The method for integral reinforcement of masonry structure based on Fe-SMA self-prestressing according to claim 2 is characterized in that: The height and depth of the embedded part of the L-shaped steel sheet should correspond to the height and depth of the annular chiseling, with the deviation controlled within 10% of the corresponding height or corresponding depth, and the length should be not less than the length of one building block; the embedded part is formed by mold making or mechanical extrusion.
4. The method for integral reinforcement of masonry structure based on Fe-SMA self-prestressing according to claim 1 is characterized in that: In step 4, the embedding depth of the Fe-SMA material in the high-performance mortar is not less than 10% of the corresponding chiseling depth.
5. The method for integral reinforcement of masonry structure based on Fe-SMA self-prestressing according to claim 1 is characterized in that: In step 5, the power-on excitation device refers to a low-voltage, high-current, high-power electrical device with an output voltage lower than 36V and an output current greater than 100A, which can electrically heat the Fe-SMA material.
6. The method for integral reinforcement of masonry structure based on Fe-SMA self-prestressing according to claim 1 is characterized in that: In step 5, when the power is turned on for excitation, the heating temperature is 200°C.
Citation Information
Patent Citations
Traditional earthen kiln folk house overall structure reinforcement system and construction technology
CN109281487A
Ancient building masonry wall reinforced by carbon fiber rib caulked joint and reinforcing construction process thereof
CN112096111A
Method for intelligently controlling crack threshold value of concrete beam through SMA wire or rib strain
CN114263126A