Polyimide varnish
By using specific block copolymers and non-cyclic aliphatic tetracarboxylic acid dianhydride in polyimide varnish, the problem of dianiline skeleton polyimide results in reduced membrane transmittance is solved, and high transmittance is achieved and polyimide film with good performance.
Patent Information
- Application Number
- CN202180020418.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-03-13
- Filing Date
- 2021-03-04
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-03-04
AI Technical Summary
Polyimides with dianiline skeletons tend to reduce the transmittance of the film during polymerization, affecting their application in liquid crystal alignment films.
Using polyimide varnish containing specific block copolymers, the diamine component with dianiline backbone with acyclic aliphatic tetracarboxylic acid dianhydride or specific alicyclic tetracarboxylic acid dianhydride at lower temperatures The anhydride reaction inhibits the oxidation reaction and increases the transmittance of the film.
It is realized that a polyimide film with a high transmittance can be obtained even with polyimide having a diphenylline skeleton, and performs well in voltage retention, residual DC voltage, residual image characteristics and brush wear resistance.
Smart Images

Figure CN115244105B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a polyimide varnish having a diphenylamine skeleton and capable of obtaining a polyimide film having high film transmittance. Background Art
[0002] Polyimide is widely used as a protective material in the electrical / electronic field due to its high mechanical strength, heat resistance, and solvent resistance. Specifically, when used as a liquid crystal alignment film for a liquid crystal display, a polyimide coating film of 0.05 to 0.2 μm is usually formed on a transparent supporting substrate with a transparent electrode, and a thin polyimide coating film is formed on various supporting substrates for use.
[0003] To form a polyimide coating film, a polyimide varnish prepared by dissolving a polyimide (precursor) in an appropriate organic solvent is usually applied onto a supporting substrate by spin coating, offset printing, gravure printing, flexographic printing, inkjet printing or the like, followed by heat treatment.
[0004] In recent years, from the viewpoint of providing various characteristics to a liquid crystal aligning film, polyimide having a diphenylamine skeleton has been proposed in Patent Document 1 and Patent Document 2.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: WO2004 / 021076
[0008] Patent Document 2: WO2013 / 008822 Summary of the invention
[0009] Problems to be solved by the invention
[0010] For polyimide with diphenylamine skeleton, it is clear that there is a tendency that the transmittance of the obtained film is reduced, which easily affects the raw material monomer used in the polymerization reaction. The present inventors have conducted research, and as a result, for the polyimide obtained using a specific alicyclic tetracarboxylic dianhydride, the transmittance of the obtained film is significantly reduced. Various reasons have been investigated, and the results show that when the polyimide (precursor) takes a specific molecular arrangement, the film transmittance is reduced. In addition, it is also clear that the structure of the imide precursor during heat treatment becomes one of the main factors that induce coloration.
[0011] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a polyimide varnish capable of obtaining a polyimide film having a high transmittance even when a polyimide having a diphenylamine skeleton is used.
[0012] Solutions for solving problems
[0013] The present inventors have conducted intensive studies to achieve the above-mentioned problems and, as a result, have found that a polyimide varnish containing a specific block copolymer is effective for achieving the above-mentioned purpose, thereby completing the present invention.
[0014] The present invention is based on this finding and has the following contents as its main points.
[0015] A polyimide varnish comprising at least one block copolymer selected from the group consisting of a polyimide precursor having a block (b1) comprising a repeating unit represented by the following formula (1) and a block (b2) comprising a repeating unit represented by the following formula (2) and a polyimide obtained by imidating the polyimide precursor.
[0016]
[0017] (X1 represents a tetravalent organic group. X2 represents a tetravalent organic group derived from acyclic aliphatic tetracarboxylic dianhydride or a tetravalent organic group represented by the following formula (X2). Y1 represents a divalent organic group having 3 to 50 carbon atoms and not having a diphenylamine skeleton. Y2 represents a divalent organic group having a diphenylamine skeleton. The two R1s and R2s each independently represent a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and the two Z1s and Z2s each independently represent a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may have a substituent, an alkenyl group having 2 to 10 carbon atoms which may have a substituent, an alkynyl group having 2 to 10 carbon atoms which may have a substituent, a tert-butoxycarbonyl group, or a 9-fluorenylmethoxycarbonyl group.)
[0018]
[0019] (R 21 ~R 24 Each independently represents a hydrogen atom, a methyl group, an ethyl group, a propyl group, a chlorine atom or a phenyl group.)
[0020] It should be noted that, in this specification, * represents a bond in any case. Boc represents a tert-butoxycarbonyl group. In addition, in this specification, examples of halogen atoms include fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms.
[0021] Effects of the Invention
[0022] According to the polyimide varnish of the present invention, even if a polyimide having a diphenylamine skeleton is used, a polyimide film with high film transmittance can be obtained. In addition, the polyimide varnish of the present invention can obtain a polyimide film with high film transmittance while also obtaining good polyimide film properties from other viewpoints (e.g., voltage holding ratio, residual DC voltage, afterimage characteristics, brush abrasion resistance). Furthermore, according to the present invention, a method for manufacturing the above-mentioned polyimide varnish is provided.
[0023] The mechanism by which the present invention obtains the above-mentioned effects is not necessarily clear, but the following is considered to be one of the causes.
[0024] That is, the reaction of the diamine component having a diphenylamine skeleton and the non-cyclic aliphatic tetracarboxylic dianhydride or the specific alicyclic tetracarboxylic dianhydride component proceeds at a relatively low temperature, and thus, compared with the reaction at a high temperature, the coloration caused by the oxidation of the diamine component in the reaction system can be suppressed. In addition, the film using the following polyimide precursor is easily thermally imidized during heat treatment, so the electron donating property of the amine can be reduced, and a polyimide film with high transmittance of the film can be obtained. The polyimide precursor is obtained using the diamine having a diphenylamine skeleton and the non-cyclic aliphatic tetracarboxylic dianhydride or the specific alicyclic tetracarboxylic dianhydride. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a graph which shows the transmittance|permeability obtained using the liquid crystal aligning agent (A-1) of Example 1 and the liquid crystal aligning agent (B-1) of Comparative Example 1. DETAILED DESCRIPTION
[0026] <Block copolymer>
[0027] The polyimide varnish of the present invention contains at least one block copolymer selected from the group consisting of a polyimide precursor and a polyimide obtained by imidizing the polyimide precursor, wherein the polyimide precursor has a block (b1) containing a repeating unit represented by the following formula (1) and a block (b2) containing a repeating unit represented by the following formula (2). That is, the polyimide varnish of the present invention contains at least one block copolymer selected from the group consisting of a polyimide precursor and a polyimide obtained by imidizing the polyimide precursor, wherein the polyimide precursor has the above block (b1) and the block (b2) and does not have an imide ring structure, and the polyimide has any repeating unit of the repeating unit obtained by imidizing the above formula (1), the repeating unit obtained by imidizing the above formula (2), or other repeating units obtained by imidizing.
[0028]
[0029] (X1 represents a tetravalent organic group. X2 represents a tetravalent organic group derived from acyclic aliphatic tetracarboxylic dianhydride or a tetravalent organic group represented by the following formula (X2). Y1 represents a divalent organic group having 3 to 50 carbon atoms and not having a diphenylamine skeleton. Y2 represents a divalent organic group having a diphenylamine skeleton. The two R1s and R2s each independently represent a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and the two Z1s and Z2s each independently represent a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may have a substituent, an alkenyl group having 2 to 10 carbon atoms which may have a substituent, an alkynyl group having 2 to 10 carbon atoms which may have a substituent, a tert-butoxycarbonyl group, or a 9-fluorenylmethoxycarbonyl group.)
[0030]
[0031] (R 21 ~R 24 Each independently represents a hydrogen atom, a methyl group, an ethyl group, a propyl group, a chlorine atom or a benzene ring.)
[0032] In formula (1), X1 preferably represents a tetravalent organic group derived from tetracarboxylic dianhydride, and more preferably represents at least one selected from the group consisting of structures represented by the following formulae (X1-1) to (X1-12).
[0033]
[0034] In formula (1), Y1 preferably represents a divalent organic group having 3 to 50 carbon atoms and having a structure represented by the following formulas (S1) to (S3) or a divalent organic group having 3 to 50 carbon atoms and not having the structure represented by the formulas (S1) to (S3). It should be noted that the divalent organic group having 3 to 50 carbon atoms and not having the structure represented by the formulas (S1) to (S3) do not have a diphenylamine skeleton as described above. Specific examples of the divalent organic group having 3 to 50 carbon atoms and not having the structure represented by the formulae (S1) to (S3) include divalent organic groups having a nitrogen-containing heterocycle in the molecule such as the following formulae (2a-1) to (2a-14), divalent organic groups having a radical initiating function such as the following formulae (2b-1) to (2b-5), divalent organic groups having a carboxyl group such as the following formulae (2c-1) to (2c-2), groups having a group "-N(D)-" (D represents a tert-butoxycarbonyl group) such as the following formulae (2d-1) to (2d-7), groups having a photo-alignment property such as the following formulae (2e-1) to (2e-11), divalent organic groups having an oxygen-containing heterocycle such as (2f-1) to (2f-3), or divalent organic groups derived from aromatic diamines having no side chain group having 3 or more carbon atoms such as the following formulae (2-1) to (2-35).
[0035]
[0036] (X 1 and X 2 Each independently represents a single bond, -(CH2) a -(a is an integer of 1 to 15), -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -COO-, -OCO- or -((CH2) a1 -A1) m1 -. wherein a1 is an integer of 1 to 15, A1 is an oxygen atom or -COO-, and m1 is 1 to 2. 1 and G 2 Each independently represents a divalent cyclic group selected from a divalent aromatic group having 6 to 12 carbon atoms and a divalent alicyclic group having 3 to 8 carbon atoms. Any hydrogen atom on the cyclic group may be substituted. m and n are each independently an integer of 0 to 3, and m+n is 1 to 4. R 1 represents an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or an alkoxyalkyl group having 2 to 20 carbon atoms, forming R 1 Any hydrogen atom of may be substituted by a fluorine atom. When m, n and ml are 2 or more, there are a plurality of X 1 , X 2 , G 1 , G 2 , a1, ml and A1 each independently have the above-mentioned definitions. As substituents that may optionally replace any hydrogen atom on the cyclic group, for example, there can be cited substituents selected from the group consisting of halogen atoms, alkyl groups containing halogen atoms, alkoxy groups containing halogen atoms, alkyl groups having 1 to 10 carbon atoms, alkoxy groups having 1 to 10 carbon atoms, alkenyl groups having 2 to 10 carbon atoms, and substituents in the group consisting of heteroatom-containing groups in which any carbon-carbon bond of the above-mentioned alkyl groups containing halogen atoms, alkoxy groups containing halogen atoms, alkyl groups, alkoxy groups, and alkenyl groups is interrupted by oxygen atoms. )
[0037] -X 3 -R 2 (S2)
[0038] (X 3 R represents a single bond, -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -CH2O-, -COO- or -OCO-. 2 represents an alkyl group having 1 to 20 carbon atoms or an alkoxyalkyl group having 2 to 20 carbon atoms, forming R 2 Any hydrogen atom of is optionally substituted by a fluorine atom. )
[0039] -X4 -R 3 (S3)
[0040] (X 4 R represents -CONH-, -NHCO-, -O-, -CH2O-, -COO- or -OCO-. 3 Indicates a structure with a steroidal skeleton.)
[0041]
[0042]
[0043]
[0044]
[0045] From the viewpoint of improving the transmittance of the obtained polyimide film, in formula (1), at least one of Y1 is preferably a divalent organic group having a structure represented by the above formulas (S1) to (S3), a divalent organic group having a nitrogen-containing heterocyclic ring in the molecule, or a divalent organic group represented by the above formulas (2-1) to (2-35). Specific examples of the divalent organic group having a structure represented by the above formulas (S1) to (S3) include groups formed by removing two amino groups from a diamine represented by the following formulas (Ys-1) to (Ys-13).
[0046]
[0047] (Where, in the formula, X v1 ~X v4 , X p1 ~X p8 Each independently represents -(CH2) a -(a is an integer of 1 to 15), -CONH-, -NHCO-, -CO-N(CH3)-, -NH-, -O-, -CH2O-, -CH2-OCO-, -COO- or -OCO-, X v5 represents -O-, -CH2O-, -CH2-OCO-, -COO- or -OCO-, X V6 ~X V7 , X s1 ~X s4 Each independently represents -O-, -CH2O-, -COO- or -OCO-. a ~X f Represents a single bond, -O-, -NH-, or -O-(CH2) m -O-, R v1 ~R v4 , R 1a ~R 1hRepresented independently -C n H 2n+1 (n is an integer from 1 to 20) or -O-C n H 2n+1 (n is an integer from 2 to 20. m is an integer from 1 to 8.)
[0048] In formula (1), two R1s each independently represent preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. Two Z1s each independently represent preferably a hydrogen atom or a methyl group.
[0049] In formula (1), X1, Y1, R1, and Z1 may each be one type or two or more types.
[0050] The block (b1) having the repeating unit represented by the formula (1) may have any repeating unit other than the repeating unit represented by the formula (1).
[0051] The content of the repeating unit represented by formula (1) is preferably 5 to 90 mol %, more preferably 10 to 80 mol %, and particularly preferably 20 to 70 mol % based on the total of the repeating units in blocks (b1) and (b2).
[0052] In formula (2), "non-cyclic aliphatic tetracarboxylic dianhydride" of X2 refers to an acid dianhydride obtained by intramolecular dehydration of four carboxyl groups bonded to a chain hydrocarbon structure. It need not be composed of only a chain hydrocarbon structure, and a part thereof may have an alicyclic structure or an aromatic ring structure.
[0053] Specific examples of the "non-cyclic aliphatic tetracarboxylic dianhydride" include the following compounds: 2a ).
[0054]
[0055] (X 2a It is selected from the following formula (X 2a -1)~(X 2a -5) at least one of the group consisting of the structures shown in )
[0056]
[0057] In formula (2), X2 preferably represents at least one selected from the group consisting of structures represented by the following formulae (X2-1) to (X2-4).
[0058]
[0059] In formula (2), Y2 preferably represents a structure represented by the following formula (d2).
[0060]
[0061] (A1 represents a single bond, -NR- (R represents a hydrogen atom or a monovalent organic group), -O-, -C(=O)-, -C(=O)NR- (R represents a hydrogen atom or a monovalent organic group), -C(=O)O- or a divalent organic group. R1 and R2 each independently represent a hydrogen atom or a monovalent organic group. When n is 2, a plurality of A1 and R2 each independently have the above definition.)
[0062] Examples of the divalent organic group in A1 include -CH2-, -C(CH3)2-, an alkylene group having 2 to 20 carbon atoms, or a divalent organic group in which a part of the methylene group of the alkylene group is substituted by -NR- (R represents a hydrogen atom or a monovalent organic group), -O-, -C(=O)-, -C(=O)NR- (R represents a hydrogen atom or a monovalent organic group), or -C(=O)O-.
[0063] As the monovalent organic group in formula (d2), there can be listed: alkyl groups having 1 to 10 carbon atoms such as methyl and ethyl groups; alkyl groups having 1 to 10 carbon atoms having halogen atoms such as trifluoroalkyl groups; alkoxyalkyl groups having 1 to 10 carbon atoms; groups containing a thermally detachable group; or groups in which a part of the methylene groups of the alkyl groups is substituted with -O-, -C(=O)-, or -C(=O)NR- (R represents a hydrogen atom or a methyl group) (except for the above-mentioned groups containing a thermally detachable group). As the group containing a thermally detachable group, there can be listed: carbamate-based protecting groups such as tert-butyloxycarbonyl (Boc group), benzyloxycarbonyl, 9-fluorenylmethoxycarbonyl, or allyloxycarbonyl groups; or groups in which a part of the hydrogen atoms of the alkyl groups is substituted with the group "*-O-E" (E represents a hydrogen atom or a carbamate-based protecting group).
[0064] As more preferable structures of Y2, the following formulae (d2-1) to (d2-13) are mentioned.
[0065]
[0066] In formula (2), two R2's each independently represent preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. Two Z2's each independently represent preferably a hydrogen atom or a methyl group.
[0067] In formula (2), X2, Y2, R2, and Z2 may each be one type or two or more types.
[0068] The block (b2) having the repeating unit represented by the formula (2) may have any repeating unit other than the repeating unit represented by the formula (2).
[0069] The content of the repeating unit represented by formula (2) is preferably 5 to 90 mol %, more preferably 10 to 80 mol %, and particularly preferably 20 to 70 mol % based on the total of the repeating units in blocks (b1) and (b2).
[0070] The ratio of the total molar number of the repeating units represented by formula (1) to the total molar number of the repeating units represented by formula (2) per molecule of the block copolymer of the present invention is preferably 9:1 to 1:9, more preferably 8:2 to 2:8, particularly preferably 7:3 to 3:7.
[0071] When the ratio of the total molar number of the repeating units is within this range, it is excellent in that a high transmittance of the film can be obtained.
[0072] The block copolymer of the present invention may have any repeating units other than the block (b1) comprising the repeating unit represented by the formula (1) and the block (b2) comprising the repeating unit represented by the formula (2).
[0073] <Production of polyimide precursor (polyamic acid)>
[0074] As the polyimide precursor used in the present invention, polyamic acid, polyamic acid ester, etc. can be mentioned.
[0075] The polyamic acid used as the polyimide precursor in the present invention can be produced, for example, by a production method comprising the following steps (I) to (II). Step (I) is to react a tetracarboxylic acid component comprising a tetracarboxylic dianhydride or a derivative thereof represented by the following formula (1-T) with a diamine component comprising a diamine represented by the following formula (1-D) to obtain a block (b1); and step (II) is to add a tetracarboxylic acid component comprising a tetracarboxylic dianhydride or a derivative thereof represented by the following formula (2-T) and a diamine component comprising a diamine represented by the following formula (2-D) to the block (b1) and react them to obtain a polyimide precursor comprising a block (b1) and a block (b2).
[0076]
[0077] (X1, X2, Y1, and Y2 are the same as X1, X2, Y1, and Y2 defined in formula (1) and formula (2).)
[0078] In addition, in the above, as a derivative of tetracarboxylic dianhydride, a tetracarboxylic acid, a tetracarboxylic acid dihalide, a tetracarboxylic acid diester dichloride, a tetracarboxylic acid diester, etc. are mentioned.
[0079] The reaction temperature in the step (II) is preferably a temperature lower than the reaction temperature in the step (I), more preferably a temperature at least 10° C. lower than the reaction temperature in the step (I), and particularly preferably a temperature at least 20° C. lower than the reaction temperature in the step (I). The polyimide varnish containing the block copolymer obtained by reacting within the above range does not require a high temperature during heating, and thus oxidation during the reaction can be suppressed. For this reason, a polyimide film with high film transmittance can be obtained.
[0080] Preferably, the reaction temperature in step (I) is 0 to 150° C., and the reaction temperature in step (II) is −20 to 130° C. More preferably, the reaction temperature in step (I) is 5 to 100° C., and the reaction temperature in step (II) is −5 to 80° C.
[0081] The tetracarboxylic acid component in step (I) may contain any tetracarboxylic dianhydride or its derivative other than the tetracarboxylic dianhydride or its derivative represented by the above formula (1-T), but preferably consists of the tetracarboxylic dianhydride or its derivative represented by the above formula (1-T).
[0082] The diamine component in step (I) may contain any diamine other than the diamine represented by the above formula (1-D), but is preferably composed of the diamine represented by the above formula (1-D).
[0083] The tetracarboxylic acid component in step (II) may contain any tetracarboxylic dianhydride or its derivative other than the tetracarboxylic dianhydride or its derivative represented by the above formula (2-T), but preferably consists of the tetracarboxylic dianhydride or its derivative represented by the above formula (2-T).
[0084] The diamine component in step (II) may contain any diamine other than the diamine represented by the above formula (2-D), but is preferably composed of the diamine represented by the above formula (2-D).
[0085] The polyamic acid which is a polyimide precursor used in the present invention can also be produced by, for example, a production method including the following steps (III) to (V).
[0086] Step (III), reacting a tetracarboxylic acid component comprising tetracarboxylic dianhydride or a derivative thereof represented by the following formula (1-T) with a diamine component comprising a diamine represented by the following formula (1-D) to obtain a block (b1); step (IV), reacting a tetracarboxylic acid component comprising tetracarboxylic dianhydride or a derivative thereof represented by the following formula (2-T) with a diamine component comprising a diamine represented by the following formula (2-D) to obtain a block (b2); and step (V), coupling the block (b1) obtained in the step (III) with the block (b2) obtained in the step (IV) to obtain a polyimide precursor comprising the block (b1) and the block (b2).
[0087]
[0088] (X1, X2, Y1, and Y2 are the same as X1, X2, Y1, and Y2 defined in formula (1) and formula (2).)
[0089] The reaction temperature in the step (IV) is preferably a temperature lower than the reaction temperature in the step (III), more preferably a temperature at least 10° C. lower than the reaction temperature in the step (III), and particularly preferably a temperature at least 20° C. lower than the reaction temperature in the step (III). The polyimide varnish containing the block copolymer obtained by reacting within the above range does not require a high temperature during heating, and thus oxidation during the reaction can be suppressed. For this reason, a polyimide film having a high transmittance can be obtained.
[0090] Preferably, the reaction temperature in the step (III) is 0 to 150° C., and the reaction temperature in the step (IV) is −20 to 130° C. More preferably, the reaction temperature in the step (III) is 5 to 100° C., and the reaction temperature in the step (IV) is −5 to 80° C.
[0091] The tetracarboxylic acid component in step (III) may contain any tetracarboxylic dianhydride or its derivative other than the tetracarboxylic dianhydride or its derivative represented by the above formula (1-T), but preferably consists of the tetracarboxylic dianhydride or its derivative represented by the above formula (1-T).
[0092] The diamine component in step (III) may contain any diamine other than the diamine represented by the above formula (1-D), but is preferably composed of the diamine represented by the above formula (1-D).
[0093] The tetracarboxylic acid component in step (IV) may contain any tetracarboxylic dianhydride or its derivative other than the tetracarboxylic dianhydride or its derivative represented by the above formula (2-T), but preferably consists of the tetracarboxylic dianhydride or its derivative represented by the above formula (2-T).
[0094] The diamine component in step (IV) may contain any diamine other than the diamine represented by the above formula (2-D), but is preferably composed of the diamine represented by the above formula (2-D).
[0095] The method for coupling the block (b1) and the block (b2) in the step (V) is not particularly limited, and examples thereof include: (1) when the ends of the blocks (b1) and (b2) are anhydride groups or derivatives thereof, a method of adding a diamine for further reaction; (2) when the ends of the blocks (b1) and (b2) are amine ends, a method of adding tetracarboxylic dianhydride or a derivative thereof for further reaction; and (3) when the blocks (b1) and (b2) have both an acid anhydride group or a derivative thereof and an amine end, a method of reacting the blocks (b1) and (b2).
[0096] The reaction of the diamine component and the tetracarboxylic acid component is usually carried out in an organic solvent. The organic solvent used at this time is not particularly limited as long as it dissolves the generated polyimide precursor. The following lists specific examples of organic solvents used in the reaction, but are not limited to these examples. For example, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone or γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide or 1,3-dimethyl-2-imidazolidinone can be listed.
[0097] When the polyimide precursor has high solubility, methyl ethyl ketone, cyclohexanone, cyclopentanone, 4-hydroxy-4-methyl-2-pentanone, or an organic solvent represented by the following formula [D-1] to [D-3] can be used.
[0098]
[0099] In formula [D-1], D 1 represents an alkyl group having 1 to 3 carbon atoms, wherein D 2 represents an alkyl group having 1 to 3 carbon atoms, wherein D 3 It represents an alkyl group having 1 to 4 carbon atoms.
[0100] These organic solvents may be used alone or in combination. Furthermore, even if the solvent does not dissolve the polyimide precursor, it may be used in combination with the above-mentioned solvent within a range in which the generated polyimide precursor does not precipitate.
[0101] The concentration of the polyamic acid in the reaction system is preferably 1 to 30% by mass, more preferably 5 to 20% by mass, from the viewpoint of preventing precipitation of the polymer and easily obtaining a high molecular weight product.
[0102] The polyamic acid obtained as described above can be recovered by injecting the reaction solution into a poor solvent while fully stirring the reaction solution. In addition, the polymer is precipitated and recovered. In addition, the precipitation is carried out several times, and after washing with a poor solvent, the powder of the purified polyamic acid can be obtained at room temperature or by heating and drying. The poor solvent is not particularly limited, and examples thereof include water, methanol, ethanol, hexane, butyl cellosolve, acetone, toluene, etc.
[0103] <Production of polyimide precursor (polyamic acid ester)>
[0104] The polyamic acid ester as the polyimide precursor used in the present invention can be produced, for example, by the following reactions: (1) esterification reaction of polyamic acid using an esterifying agent; (2) reaction of tetracarboxylic acid diester dichloride with diamine; or (3) polycondensation reaction of tetracarboxylic acid diester with diamine. The production method of (2) or (3) can be carried out according to the production of polyamic acid described above.
[0105] Among the above three production methods, the production method of (1) or (2) is particularly preferred in order to obtain high molecular weight polyamic acid ester.
[0106] The solution of polyamic acid ester obtained as described above can be injected into a poor solvent while being fully stirred to precipitate the polymer. After precipitation is performed several times, it is washed with a poor solvent and dried at room temperature or by heating to obtain a powder of the purified polyamic acid ester. The poor solvent is not particularly limited, and examples thereof include water, methanol, ethanol, hexane, butyl cellosolve, acetone, toluene, and the like.
[0107] <Manufacturing of polyimide>
[0108] The polyimide used in the present invention can be produced by imidizing the above-mentioned polyimide precursor.
[0109] In the polyimide used in the present invention, the ring closure ratio (also referred to as imidization ratio) of the amic acid group does not necessarily need to be 100%, and can be arbitrarily adjusted according to the application and purpose.
[0110] For example, from the viewpoint of improving the solubility of the polyimide varnish, the imidization ratio of the polyimide may be 20% to 100%, 50% to 99%, or 70% to 99%.
[0111] Imidization can be carried out by stirring the polyamic acid to be imidized in an organic solvent in the presence of a basic catalyst and an acid anhydride. As an organic solvent, the above-mentioned organic solvent used during the polymerization reaction can be used. As a basic catalyst, pyridine, triethylamine, trimethylamine, tributylamine, trioctylamine, etc. can be listed. Among them, pyridine has a moderate alkalinity that allows the reaction to proceed, so it is preferred. In addition, as an acid anhydride, acetic anhydride, trimellitic anhydride, pyromellitic anhydride, etc. can be listed, wherein, if acetic anhydride is used, purification after the reaction is completed becomes easy, so it is preferred.
[0112] The temperature during the imidization reaction is -20 to 140°C, preferably 0 to 100°C, and the reaction time can be 0.5 to 100 hours, preferably 1 to 80 hours. The amount of the basic catalyst is 0.5 to 30 times by mole of the amic acid, preferably 2 to 20 times by mole, and the amount of the acid anhydride is 1 to 50 times by mole of the amic acid, preferably 3 to 30 times by mole. The imidization rate of the obtained polymer can be controlled by adjusting the amount of catalyst, temperature, and reaction time.
[0113] Since the added catalyst and the like remain in the solution after the imidization reaction of the polyimide precursor, it is preferred to recover the obtained imidized polymer by the method described below, redissolve it in an organic solvent, and use it as a component of the liquid crystal aligning agent of the present invention.
[0114] The polymer can be precipitated by injecting the polyimide solution obtained as described above into a poor solvent while stirring it thoroughly. The precipitation is performed several times, and after washing with a poor solvent, it is dried at room temperature or by heating to obtain a purified polyimide powder.
[0115] The poor solvent is not particularly limited, and examples thereof include methanol, acetone, hexane, butyl cellosolve, heptane, methyl ethyl ketone, methyl isobutyl ketone, ethanol, toluene, and benzene.
[0116] <Polyimide varnish>
[0117] The polyimide varnish of the present invention contains the block copolymer. The content of the block copolymer in the polyimide varnish can be appropriately changed according to the thickness of the polyimide film to be formed. From the perspective of forming a uniform and defect-free coating film, it is preferably 1 to 10% by mass of the entire liquid crystal aligning agent, more preferably 2 to 9% by mass, and particularly preferably 2 to 7% by mass.
[0118] The polyimide varnish of the present invention preferably further contains at least one polymer (P) selected from the group consisting of a polyimide precursor having a repeating unit represented by the following formula (3) and a polyimide obtained by imidating the polyimide precursor.
[0119]
[0120] (X3 represents a tetravalent organic group, preferably a tetravalent organic group derived from tetracarboxylic dianhydride. Y3 represents a divalent organic group derived from a diamine, preferably a divalent organic group having 3 to 50 carbon atoms and not having a diphenylamine skeleton. R3 and Z3 have the same meanings as R1 and Z1 in formula (1). Two R3 and Z3 each independently have the above definitions.)
[0121] The polymer (P) preferably does not have a diphenylamine skeleton. By further containing the polymer (P), the properties of the polyimide varnish of the present invention (for example, the voltage holding ratio and brush abrasion resistance of a liquid crystal alignment film obtained from the polyimide varnish) can be improved.
[0122] When the polyimide varnish of the present invention contains a polymer (P), the content ratio of at least one block copolymer selected from the group consisting of a polyimide precursor having the above-mentioned block (b1) and the above-mentioned block (b2) and a polyimide obtained by imidizing the polyimide precursor to the polymer (P) can be 10 / 90 to 90 / 10, 20 / 80 to 90 / 10, or 20 / 80 to 80 / 20 in terms of the mass ratio of [block copolymer (b)] / [polymer (P)].
[0123] In formula (3), X3 preferably represents a compound selected from the following formulas (X3-1) to (X3-18), the above formula (X3- 2a -1)~(X 2a -2), (X 2a -5) is at least one of the group consisting of structures represented by Formula (X3-13). Preferred specific examples of the following formula (X3-13) include structures represented by Formulas (X2-1) to (X2-4) described above.
[0124]
[0125] (R 31 ~R 34 Each of them independently represents a hydrogen atom, a methyl group, an ethyl group, a propyl group, a chlorine atom or a benzene ring. j and k represent 0 or 1, and A1 and A2 independently represent a single bond, -O-, -CO-, -COO-, a phenylene group, a sulfonyl group or an amide group. Two A2s each independently have the above definition.)
[0126] Preferred specific examples of (X3-17) and (X3-18) include the following formulas (X3-19) to (X3-34).
[0127]
[0128] In formula (3), Y3 preferably represents at least one selected from the group consisting of the structures represented by Y1 above.
[0129] In formula (3), two R3's each independently represent preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. Two Z3's each independently represent preferably a hydrogen atom or an alkyl group having 1 carbon atom.
[0130] In formula (3), X3, Y3, R3, and Z3 may each be one type or two or more types.
[0131] The polyimide precursor is preferably composed of a repeating unit represented by the formula (3).
[0132] In the polymer (P), the total amount of the repeating unit (3) and the imidized structural unit of the repeating unit (3) is more preferably 10 to 100 mol %, and further preferably 15 to 100 mol % of all the repeating units.
[0133] In the above formula (3), X3 is (X3-1) to (X3-11), (X3-13) (more preferably (X2-1) to (X2-4)), or (X3-14). 2a -1)~(X 2a The total amount of the repeating unit (3) of -2) and the imidized structural unit of the repeating unit (3) is more preferably 10 to 100 mol %, and further preferably 15 to 100 mol % of all the repeating units.
[0134] The polyimide varnish of the present invention further contains the polymer (P), thereby achieving the effects of obtaining a high voltage holding ratio and good orientation.
[0135] The polyimide varnish of the present invention can be prepared, for example, by dispersing or dissolving the block copolymer of the present invention and, if necessary, the polymer (P) and other components in an organic solvent.
[0136] Examples of other components include antioxidants (phenolic, phosphite, thioether, etc.), ultraviolet absorbers, hindered amine light stabilizers, nucleating agents, resin additives (fillers, talc, glass fibers, etc.), flame retardants, and processability improvers / lubricants.
[0137] Examples of the organic solvent include lactone solvents such as γ-valerolactone and γ-butyrolactone; lactam solvents such as γ-butyrolactam; amide solvents such as N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide; 4-hydroxy-4-methyl-2-pentanone, 2,6-dimethyl-4-heptanone (diisobutyl ketone), methyl lactate, ethyl lactate, n-propyl lactate, n-butyl lactate, isopentyl lactate, n-butyl acetate, propylene glycol monoethyl acetate, methyl pyruvate, ethyl pyruvate, methyl methoxypropionate, ethyl ethoxypropionate, ethylene glycol monomethyl ether, ethylene glycol ethyl ether, ethylene glycol monobutyl ether, ethylene glycol n-propyl ether, ethylene glycol isopropyl ether, ethylene glycol n-butyl acetate. Butyl ether (butyl cellosolve), ethylene glycol dimethyl ether, ethylene glycol monoethyl ether acetate, ethylene glycol butyl ether acetate, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, propylene glycol monobutyl ether, propylene glycol diacetate, dipropylene glycol, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol dimethyl ether, tripropylene glycol monomethyl ether, isoamyl propionate, isoamyl isobutyrate, diisopropyl ether, diisoamyl ether; carbonate solvents such as ethylene carbonate and propylene carbonate; 1-hexanol, cyclohexanol, 1,2-ethylene glycol, diisobutylcarbinol (2,6-dimethyl-4-heptanol), etc. These may be used alone or in combination of two or more.
[0138] Preferred combinations of solvents include: N-methyl-2-pyrrolidone and ethylene glycol monobutyl ether; N-methyl-2-pyrrolidone, γ-butyrolactone and ethylene glycol monobutyl ether; N-methyl-2-pyrrolidone, γ-butyrolactone and propylene glycol monobutyl ether; N-ethyl-2-pyrrolidone and propylene glycol monobutyl ether; N-methyl-2-pyrrolidone, γ-butyrolactone, 4-hydroxy-4-methyl-2-pentanone and diethylene glycol diethyl ether; N-ethyl-2-pyrrolidone, N-methyl-2-pyrrolidone and 4-hydroxy-4-methyl-2-pentanone; N-methyl-2-pyrrolidone, 4-hydroxy-4-methyl-2-pentanone and diisobutyl ketone; N-methyl-2-pyrrolidone, 4-hydroxy-4-methyl-2-pentanone and dipropylene glycol monomethyl ether; N-methyl-2-pyrrolidone, 4-Hydroxy-4-methyl-2-pentanone and propylene glycol monobutyl ether; N-methyl-2-pyrrolidone, 4-hydroxy-4-methyl-2-pentanone and propylene glycol diacetate; γ-butyrolactone, 4-hydroxy-4-methyl-2-pentanone and diisobutyl ketone; γ-butyrolactone, 4-hydroxy-4-methyl-2-pentanone and propylene glycol diacetate; N-methyl-2-pyrrolidone, γ-butyrolactone, propylene glycol diacetate alcohol monobutyl ether and diisobutyl ketone; N-methyl-2-pyrrolidone, γ-butyrolactone, propylene glycol monobutyl ether and diisopropyl ether; N-methyl-2-pyrrolidone, γ-butyrolactone, propylene glycol monobutyl ether and diisobutyl carbinol; N-methyl-2-pyrrolidone, γ-butyrolactone and dipropylene glycol dimethyl ether; N-methyl-2-pyrrolidone, propylene glycol monobutyl ether and dipropylene glycol dimethyl ether, etc. The type and content of such solvents can be appropriately selected according to the coating device, coating conditions, coating environment, etc. of the liquid crystal alignment agent.
[0139] <Liquid crystal alignment agent>
[0140] The liquid crystal aligning agent of the present invention is preferably prepared as a coating liquid so as to be suitable for forming a liquid crystal aligning film. The liquid crystal aligning agent of the present invention can be prepared by, for example, dispersing or dissolving the polyimide varnish of the present invention and other components as needed in an organic solvent.
[0141] Examples of other components include a crosslinking compound, a functional silane compound, a surfactant, a compound having a photopolymerizable group, and an organic solvent.
[0142] The crosslinking compound can be used for the purpose of improving the strength of the liquid crystal alignment film. Examples of the crosslinking compound include compounds having an isocyanate group or a cyclocarbonate group as described in paragraphs
[0109] to
[0113] of International Publication WO2016 / 047771, or compounds having at least one group selected from the group consisting of lower alkoxyalkyl groups, and compounds having a blocked isocyanate group.
[0143] Blocked isocyanate compounds are commercially available, and for example, CORONATE APSTABLE M, CORONATE 2503, 2515, 2507, 2513, 2555, MILLIONATE MS-50 (all manufactured by Nippon Polyurethane Industries, Ltd.), TAKENATE B-830, B-815N, B-820NSU, B-842N, B-846N, B-870N, B-874N, B-882N (all manufactured by Mitsui Chemicals, Inc.) and the like can be preferably used.
[0144] Specific examples of preferred crosslinking compounds include compounds represented by the following formulae (CL-1) to (CL-11).
[0145]
[0146] The above is an example of the crosslinking compound, but the invention is not limited thereto. Moreover, the crosslinking compound used for the liquid crystal aligning agent of the present invention may be one kind or a combination of two or more kinds.
[0147] Content of other crosslinking|crosslinked compound in the liquid crystal aligning agent of this invention is 0.1-150 mass parts, or 0.1-100 mass parts, or 1-50 mass parts with respect to 100 mass parts of all polymer components.
[0148] The functional silane compound can be used for the purpose of improving the adhesion between the liquid crystal alignment film and the base substrate. As a specific example, the silane compound described in paragraph
[0019] of International Publication Gazette 2014 / 119682 can be cited. The content of the functional silane compound is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 20 parts by mass relative to 100 parts by mass of the total polymer components.
[0149] Surfactants can be used for the purpose of improving the uniformity of the film thickness and surface smoothness of the liquid crystal alignment film. As compounds, fluorine-based surfactants, silicone-based surfactants, nonionic surfactants, etc. can be listed. Their specific examples can list the surfactants described in paragraph
[0117] of the International Publication WO2016 / 047771. The amount of the surfactant used is preferably 0.01 to 2 parts by mass, more preferably 0.01 to 1 part by mass, relative to 100 parts by mass of all polymer components contained in the liquid crystal alignment agent.
[0150] Examples of the compound having a photopolymerizable group include compounds having one or more polymerizable unsaturated groups such as an acrylate group and a methacrylate group in the molecule, for example, compounds represented by the following formulae (M-1) to (M-7).
[0151]
[0152] Moreover, in the liquid crystal aligning agent of the present invention, as a compound that promotes the charge transfer in the liquid crystal aligning film and promotes the charge escape of the element, a nitrogen-containing heterocyclic amine compound represented by formula [M1] to formula [M156] described in paragraphs
[0194] to
[0200] of International Publication WO2011 / 132751 (published on October 27, 2011) can be added, and 3-aminomethylpyridine and 4-aminomethylpyridine are more preferably added. The amine compound can be directly added to the liquid crystal aligning agent, but it is preferably added after making a solution with a concentration of 0.1 to 10% by mass, preferably 1 to 7% by mass. The solvent is not particularly limited as long as it dissolves the polyimide varnish.
[0153] When the liquid crystal aligning agent of this invention contains a polyamic acid, a polyamic acid ester, or a polyamic acid-polyamic acid ester copolymer, you may add an imidization accelerator etc. for the purpose of efficiently performing imidization by heating when baking a coating film.
[0154] Examples of the organic solvent contained in the liquid crystal alignment agent of the present invention include lactone solvents such as γ-valerolactone and γ-butyrolactone; lactam solvents such as γ-butyrolactam, N-methyl-2-pyrrolidone, and N-ethyl-2-pyrrolidone; amide solvents such as N,N-dimethylformamide and N,N-dimethylacetamide; 4-hydroxy-4-methyl-2-pentanone, 2,6-dimethyl-4-heptanone, methyl lactate, ethyl lactate, n-propyl lactate, n-butyl lactate, isopentyl lactate, n-butyl acetate, propylene glycol monoethyl acetate, methyl pyruvate, ethyl pyruvate, methyl methoxypropionate, ethyl ethoxypropionate, ethylene glycol monomethyl ether, ethylene glycol ethyl ether, ethylene glycol monobutyl ether, and ethylene glycol n-propyl ether. , ethylene glycol isopropyl ether, ethylene glycol n-butyl ether (butyl cellosolve), ethylene glycol dimethyl ether, ethylene glycol ethyl ether acetate, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, propylene glycol monobutyl ether, propylene glycol diacetate, dipropylene glycol, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol dimethyl ether, tripropylene glycol monomethyl ether, isopentyl propionate, isopentyl isobutyrate, diisopropyl ether, diisoamyl ether; carbonate solvents such as ethylene carbonate and propylene carbonate; 1-hexanol, cyclohexanol, 1,2-ethylene glycol, 2,6-dimethyl-4-heptanol, etc. These can be used alone or in combination of two or more.
[0155] Preferred combinations of solvents include: N-methyl-2-pyrrolidone and ethylene glycol monobutyl ether; N-methyl-2-pyrrolidone, γ-butyrolactone and ethylene glycol monobutyl ether; N-methyl-2-pyrrolidone, γ-butyrolactone and propylene glycol monobutyl ether; N-ethyl-2-pyrrolidone and propylene glycol monobutyl ether; N-methyl-2-pyrrolidone, γ-butyrolactone, 4-hydroxy-4-methyl-2-pentanone and diisopropyl ether. Ethylene glycol diethyl ether; N-ethyl-2-pyrrolidone, N-methyl-2-pyrrolidone and 4-hydroxy-4-methyl-2-pentanone; N-methyl-2-pyrrolidone, 4-hydroxy-4-methyl-2-pentanone and 2,6-dimethyl-4-heptanone; N-methyl-2-pyrrolidone, 4-hydroxy-4-methyl-2-pentanone and dipropylene glycol monomethyl ether; N-methyl-2-pyrrolidone, 4-hydroxy-4-methyl-2-pentanone Methyl-2-pentanone and propylene glycol monobutyl ether; N-methyl-2-pyrrolidone, 4-hydroxy-4-methyl-2-pentanone and propylene glycol diacetate; γ-butyrolactone, 4-hydroxy-4-methyl-2-pentanone and 2,6-dimethyl-4-heptanone; γ-butyrolactone, 4-hydroxy-4-methyl-2-pentanone and propylene glycol diacetate; N-methyl-2-pyrrolidone, γ-butyrolactone, propylene glycol monobutyl ether and 2,6-dimethyl-4-heptanone; N-methyl-2-pyrrolidone, γ-butyrolactone, propylene glycol monobutyl ether and diisopropyl ether; N-methyl-2-pyrrolidone, γ-butyrolactone, propylene glycol monobutyl ether and 2,6-dimethyl-4-heptanol; N-methyl-2-pyrrolidone, γ-butyrolactone and dipropylene glycol dimethyl ether; N-methyl-2-pyrrolidone, propylene glycol monobutyl ether and dipropylene glycol dimethyl ether, etc. The type and content of such solvents are appropriately selected according to the coating device, coating conditions, coating environment, etc. of the liquid crystal alignment agent.
[0156] The solid content concentration in the liquid crystal aligning agent (the ratio of the total mass of the components other than the organic solvent of the liquid crystal aligning agent to the total mass of the liquid crystal aligning agent) is appropriately selected in consideration of viscosity, volatility, etc., and is preferably in the range of 1 to 10 mass %.
[0157] The range of particularly preferred solid content concentration varies depending on the method used when applying the liquid crystal alignment agent to the substrate. For example, in the case of spin coating, the solid content concentration is particularly preferably in the range of 1.5 to 4.5% by mass. In the case of printing, it is particularly preferred to set the solid content concentration in the range of 3 to 9% by mass, thereby setting the solution viscosity in the range of 12 to 50 mPa·s. In the case of inkjet method, it is particularly preferred to set the solid content concentration in the range of 1 to 5% by mass, thereby setting the solution viscosity in the range of 3 to 15 mPa·s.
[0158] <Liquid crystal alignment film / liquid crystal display element>
[0159] The liquid crystal alignment film of the present invention is obtained from the above-mentioned liquid crystal alignment agent. The liquid crystal alignment film of the present invention can be used for a horizontally oriented or vertically oriented liquid crystal alignment film. The vertically oriented liquid crystal alignment film is a liquid crystal alignment film suitable for a vertically oriented liquid crystal display element such as a VA (Vertical Alignment) mode or a PSA (Polymer Sustained Alignment) mode. More preferably, the vertically oriented liquid crystal alignment film can be preferably used for a liquid crystal display element obtained by the following method for manufacturing a liquid crystal display element, that is, a coating film is formed by coating on a pair of substrates having a conductive film, and the coating film is arranged oppositely with a layer of liquid crystal molecules separated to form a liquid crystal box, and the liquid crystal box is irradiated with light in a state where a voltage is applied between the conductive films of the pair of substrates. More specifically, it is a PSA-type liquid crystal display element described later, and a liquid crystal display element for a SC-PVA (Patterned Vertical Alignment: Image Vertical Orientation) mode. The liquid crystal display element of the present invention has the above-mentioned liquid crystal alignment film. The liquid crystal display element of the present invention can be produced, for example, by a method including the following steps (1) to (3) or steps (1) to (4).
[0160] (1) Process of applying a liquid crystal alignment agent on a substrate
[0161] The liquid crystal alignment agent of the present invention is applied to one side of a substrate provided with a patterned transparent conductive film by a suitable coating method such as a roller coater method, a spin coating method, a printing method, an inkjet method, etc. Here, as a substrate, there is no particular limitation as long as it is a substrate with high transparency, and a plastic substrate such as an acrylic substrate, a polycarbonate substrate, etc. may also be used together with a glass substrate, a silicon nitride substrate, etc. In addition, in a reflective liquid crystal display element, if it is only a single-sided substrate, an opaque object such as a silicon wafer may also be used, and the electrode in this case may also use a light-reflecting material such as aluminum.
[0162] (2) Process of firing the coating film
[0163] After the liquid crystal alignment agent is applied, it is preferred to first perform preliminary heating (pre-baking) for the purpose of preventing the applied alignment agent from dripping. The pre-baking temperature is preferably 30 to 200°C, more preferably 40 to 150°C, and particularly preferably 40 to 100°C. The pre-baking time is preferably 0.25 to 10 minutes, more preferably 0.5 to 5 minutes. It is also preferred to perform a heating (post-baking) process.
[0164] The post-baking temperature is preferably 80 to 300° C., more preferably 120 to 250° C. The post-baking time is preferably 5 to 200 minutes, more preferably 10 to 100 minutes. The film thickness of the film formed in this way is preferably 5 to 300 nm, more preferably 10 to 200 nm.
[0165] The coating film formed in the above step (1) can be used as a liquid crystal alignment film as it is, or the coating film can be subjected to a treatment to impart an alignment ability. Examples of the treatment to impart an alignment ability include: a brushing treatment in which a roll of cloth made of fibers such as nylon, rayon, and cotton is wound around the coating film and rubbed in a certain direction; and a photo-alignment treatment in which the coating film is irradiated with polarized or non-polarized radiation.
[0166] In the photo-alignment treatment, as the radiation irradiated to the coating film, for example, ultraviolet rays and visible light containing light with a wavelength of 150 to 800 nm can be used. In the case of polarized radiation, it can be linearly polarized or partially polarized. In addition, when the radiation used is linearly polarized or partially polarized, the irradiation can be performed from a direction perpendicular to the substrate surface, from an oblique direction, or a combination thereof. In the case of irradiating non-polarized radiation, the irradiation direction is set to an oblique direction.
[0167] (3) Step of forming a liquid crystal layer
[0168] (3-1) Case of VA-type liquid crystal display element
[0169] As described above, two substrates formed with liquid crystal alignment films are prepared, and liquid crystal is arranged between the two opposing substrates. Specifically, the following two methods can be cited. The first method is a previously known method. First, two substrates are arranged opposite to each other with a gap (cell gap) between the respective liquid crystal alignment films. Then, the peripheral portions of the two substrates are bonded together using a sealant, and a liquid crystal composition is injected into the cell gap divided by the substrate surface and the sealant, and after contacting the film surface, the injection hole is encapsulated.
[0170] In addition, the second method is a method called ODF (One Drop Fill: liquid crystal dripping) method. At a predetermined location on one of the two substrates with a liquid crystal alignment film, for example, a UV-curable sealant is applied, and a liquid crystal composition is further dripped into several predetermined locations on the surface of the liquid crystal alignment film. Then, the substrate of the other side is bonded in a manner that the liquid crystal alignment film is opposite, and the liquid crystal composition is extended to the entire surface of the substrate and contacts the film surface. Then, ultraviolet light is irradiated on the entire surface of the substrate to cure the sealant. In the case of using any of the methods, it is ideal that the liquid crystal composition used is further heated to a temperature at which it becomes isotropic, and then slowly cooled to room temperature, thereby removing the flow orientation during liquid crystal filling.
[0171] (3-2) Manufacturing of PSA Type Liquid Crystal Display Element
[0172] The same procedure as in (3-1) is performed except that a liquid crystal composition containing a polymerizable compound is injected or dropped. Examples of the polymerizable compound include polymerizable compounds represented by the above formulae (M-1) to (M-7).
[0173] (3-3) When a coating film is formed on a substrate using a liquid crystal aligning agent containing a compound having a polymerizable group
[0174] After the same process as (3-1) above, a method for manufacturing a liquid crystal display element by irradiating ultraviolet rays described later can also be used. According to this method, as in the case of manufacturing the PSA type liquid crystal display element, a liquid crystal display element with excellent response speed can be obtained with a small amount of light irradiation. The compound having a polymerizable group can be a compound having one or more polymerizable unsaturated groups such as acrylate groups and methacrylate groups in the molecule as shown in the formula (M-1) to (M-7), and its content is preferably 0.1 to 30 parts by mass, more preferably 1 to 20 parts by mass relative to 100 parts by mass of all polymer components. In addition, the polymerizable group may also have a polymer for a liquid crystal aligning agent, and as such a polymer, for example, a polymer obtained by using the following diamine component for reaction can be listed, and the diamine component contains a diamine having the photopolymerizable group at the end.
[0175] (4) Ultraviolet irradiation process
[0176] The liquid crystal box is irradiated with light while a voltage is applied between the conductive films of a pair of substrates obtained in (3-2) or (3-3) above. Here, the applied voltage can be set to, for example, a direct current or alternating current of 5 to 50 V. In addition, as the irradiated light, for example, ultraviolet light and visible light with a wavelength of 150 to 800 nm can be used, preferably ultraviolet light with a wavelength of 300 to 400 nm. As the light source of the irradiated light, for example, a low-pressure mercury lamp, a high-pressure mercury lamp, a deuterium lamp, a metal halide lamp, an argon resonance lamp, a xenon lamp, an excimer laser, etc. can be used. The irradiation amount of light is preferably 1000 to 200,000 J / m 2 , more preferably 1000 to 100000 J / m 2 .
[0177] Furthermore, a liquid crystal display element can be obtained by bonding a polarizing plate to the outer surface of the liquid crystal cell. Examples of the polarizing plate bonded to the outer surface of the liquid crystal cell include a polarizing plate formed by sandwiching a polarizing film called "H film" that stretches and orients polyvinyl alcohol and absorbs iodine between cellulose acetate protective films, or a polarizing plate composed of the H film itself.
[0178] The liquid crystal display element of the present invention can be effectively used in various devices, for example, it can be used in various display devices such as clocks, portable game consoles, word processors, notebook computers, car navigation systems, portable cameras, PDAs (Personal Digital Assistants), digital cameras, mobile phones, smart phones, various monitors, liquid crystal televisions, information displays, etc.
[0179] Example
[0180] Hereinafter, the present invention will be described in further detail based on Examples, but the present invention is not limited to the Examples at all.
[0181] <Synthesis of Liquid Crystal Alignment Agent>
[0182] The abbreviations used in preparation of the following liquid crystal aligning agent are as follows.
[0183] (Tetracarboxylic dianhydride)
[0184] BODA: bicyclo[3,3,0]octane-2,4,6,8-tetracarboxylic dianhydride.
[0185] CBDA: 1,2,3,4-cyclobutanetetracarboxylic dianhydride.
[0186] BDA: meso-butane-1,2,3,4-tetracarboxylic dianhydride.
[0187] (Diamine)
[0188]
[0189] (additive)
[0190]
[0191] (Solvent)
[0192] NMP: N-methyl-2-pyrrolidone, BCS: butyl cellosolve.
[0193] <Molecular weight measurement>
[0194] Measuring apparatus: room temperature gel permeation chromatography (GPC) (SSC-7200) manufactured by SENSHU Scientific Co., Ltd.; chromatographic column: chromatographic column manufactured by Shodex Co., Ltd. (KD-803 and KD-805 connected in series); chromatographic column temperature: 50°C; eluent: N,N-dimethylformamide (as additives, lithium bromide monohydrate (LiBr·H2O) is 30 mmol / L, phosphoric acid / anhydrous crystals (o-phosphoric acid) is 30 mmol / L, and tetrahydrofuran (THF) is 10 ml / L); flow rate: 1.0 mL / min; standard samples for preparing calibration curve: TSK standard polyethylene oxide manufactured by Tosoh Co., Ltd. (molecular weight of about 900,000, 150,000, 100,000, and 30,000), and polyethylene glycol manufactured by Polymer Laboratory Co., Ltd. (molecular weight of about 12,000, 4,000, and 1,000).
[0195] <Measurement of Imidization Ratio>
[0196] 20 mg of polyimide powder was added to an NMR sample tube (NMR standard sample tube φ5 manufactured by Kusano Scientific Co., Ltd.), 1.0 mL of deuterated dimethyl sulfoxide (DMSO-d6, 0.05% TMS mixture) was added, and ultrasonic waves were applied to completely dissolve the mixture. The solution was measured by 500 MHz proton NMR using an NMR measuring instrument (JNW-ECA500) manufactured by DATUM Co., Ltd. of Japan Electronics Co., Ltd.
[0197] The chemical imidization rate is calculated as follows: a proton derived from a structure that does not change before and after imidization is determined as a reference proton, and the peak integral value of the proton and the peak integral value of the proton derived from the NH group of the amic acid appearing near 9.5 to 10.0 ppm are used to calculate the chemical imidization rate using the following formula. It should be noted that, in the formula, x is the peak integral value of the proton derived from the NH group of the amic acid, y is the peak integral value of the reference proton, and α is the ratio of the number of reference protons to one NH proton of the amic acid in the case of polyamic acid (imidization rate of 0%).
[0198] Imidization rate (%) = (1-α·x / y) × 100
[0199] <Synthesis example 1>
[0200] BODA (1.75 g, 7.0 mmol) and DA-5 (1.66 g, 8.4 mmol) were dissolved in NMP (13.7 g), reacted at 60°C for 3 hours, DA-1 (1.12 g, 5.6 mmol) and NMP (4.5 g) were added to dissolve, CBDA (1.31 g, 6.7 mmol) and NMP (5.3 g) were added, and reacted at 40°C for 4 hours to obtain a polyamic acid solution (1). The number average molecular weight Mn of the polyamic acid was 10200, and the weight average molecular weight Mw was 38400.
[0201] <Synthesis example 2>
[0202] BODA (1.88 g, 7.5 mmol), DA-3 (0.65 g, 6.0 mmol) and DA-4 (1.18 g, 3.0 mmol) were dissolved in NMP (14.8 g) and reacted at 60°C for 3 hours, DA-1 (1.20 g, 6.0 mmol) and NMP (4.8 g) were added and dissolved, CBDA (1.41 g, 7.2 mmol) and NMP (5.6 g) were added, and reacted at 40°C for 4 hours to obtain a polyamic acid solution (2). The polyamic acid had an Mn of 11200 and an Mw of 25800.
[0203] <Synthesis Example 3>
[0204] BODA (0.75 g, 3.0 mmol) and DA-5 (2.08 g, 10.5 mmol) were dissolved in NMP (11.3 g) and reacted at 60°C for 3 hours, DA-2 (0.96 g, 4.5 mmol) and NMP (3.8 g) were added to dissolve, CBDA (2.18 g, 11.1 mmol) and NMP (8.7 g) were added, and reacted at 40°C for 4 hours to obtain a polyamic acid solution (3). The polyamic acid had an Mn of 10,600 and an Mw of 28,700.
[0205] <Synthesis example 4>
[0206] BODA (2.50 g, 10.0 mmol), DA-5 (0.99 g, 5.0 mmol), DA-6 (0.66 g, 2.0 mmol), DA-7 (1.42 g, 6.0 mmol) and DA-4 (2.76 g, 7.0 mmol) were dissolved in NMP (33.4 g), reacted at 60°C for 3 hours, and then CBDA (1.92 g, 9.8 mmol) and NMP (7.7 g) were added, and reacted at 40°C for 4 hours to obtain a polyamic acid solution. NMP was added to the polyamic acid solution (25 g) to dilute it to 6.5% by mass, and then acetic anhydride (4.96 g) and pyridine (1.53 g) as imidization catalysts were added, and reacted at 50°C for 3 hours. The reaction solution was put into methanol (334 g), and the resulting precipitate was filtered out. The precipitate was washed with methanol and dried under reduced pressure at 60°C to obtain a polyimide powder. The imidization ratio of the polyimide was 59%, Mn was 12500, and Mw was 42300. NMP (28.0 g) was added to the obtained polyimide powder (2.0 g) and stirred at 70° C. for 15 hours to dissolve the mixture. BCS (20.0 g) was added to the solution to obtain a polyimide solution (1).
[0207] <Synthesis Example 5>
[0208] BDA (2.58 g, 13.0 mmol), DA-8 (3.42 g, 14.0 mmol) and DA-9 (3.34 g, 6.0 mmol) were dissolved in NMP (52.9 g), reacted at 50 ° C for 2 hours, and then CBDA (1.33 g, 6.8 mmol) and NMP (7.6 g) were added, and reacted at 40 ° C for 4 hours to obtain a polyamic acid solution. After adding NMP to the polyamic acid solution (25 g) to dilute it to 6.5% by mass, acetic anhydride (3.59 g) and pyridine (1.11 g) as imidization catalysts were added, and reacted at 40 ° C for 2.5 hours. The reaction solution was put into methanol (250 g) and the resulting precipitate was filtered out. The precipitate was washed with methanol and dried under reduced pressure at 60 ° C to obtain a polyimide powder. The imidization ratio of the polyimide was 65%, Mn was 11200, and Mw was 38100. NMP (28.0 g) was added to the obtained polyimide powder (2.0 g), and the mixture was stirred at 70° C. for 15 hours to dissolve the mixture. BCS (20.0 g) was added to the solution to obtain a polyimide solution (2).
[0209] <Comparative Synthesis Example 1>
[0210] BODA (1.75 g, 7.0 mmol), DA-5 (1.66 g, 8.4 mmol) and DA-1 (1.12 g, 5.6 mmol) were dissolved in NMP (18.1 g) and reacted at 60°C for 3 hours, then CBDA (1.31 g, 6.7 mmol) and NMP (5.2 g) were added and reacted at 40°C for 4 hours to obtain a polyamic acid solution (4). The polyamic acid had an Mn of 11100 and an Mw of 31900.
[0211] <Comparative Synthesis Example 2>
[0212] BODA (1.88 g, 7.5 mmol), DA-3 (0.65 g, 6.0 mmol), DA-4 (1.18 g, 3.0 mmol) and DA-1 (1.20 g, 6.0 mmol) were dissolved in NMP (19.6 g) and reacted at 60°C for 3 hours, then CBDA (1.41 g, 7.2 mmol) and NMP (5.5 g) were added and reacted at 40°C for 4 hours to obtain a polyamic acid solution (5). The polyamic acid had an Mn of 10,000 and an Mw of 20,200.
[0213] <Comparative Synthesis Example 3>
[0214] BODA (0.75 g, 3.0 mmol), DA-5 (2.08 g, 10.5 mmol) and DA-2 (0.96 g, 4.5 mmol) were dissolved in NMP (15.2 g) and reacted at 60°C for 3 hours, then CBDA (2.18 g, 11.1 mmol) and NMP (8.7 g) were added and reacted at 40°C for 4 hours to obtain a polyamic acid solution (6). The polyamic acid had an Mn of 9400 and an Mw of 34200.
[0215] The specifications of the polymers obtained in the above-mentioned synthesis examples and comparative synthesis examples are shown in Table 1 below.
[0216] [Table 1]
[0217]
[0218] <Preparation of Liquid Crystal Alignment Agent>
[0219] The examples of preparing the liquid crystal aligning agent are described in the examples and comparative examples. Using the liquid crystal aligning agents obtained in the examples and comparative examples, liquid crystal display elements were prepared and various evaluations were performed.
[0220] [Example 1]
[0221] NMP (16.0 g) and BCS (16.0 g) were added to the polyamic acid solution (1) (8.0 g) obtained in Synthesis Example 1, and the mixture was stirred at room temperature for 2 hours, thereby obtaining a liquid crystal aligning agent (A-1).
[0222] [Examples 2, 3, Comparative Examples 1 to 3]
[0223] Liquid crystal aligning agents (A-2), (A-3), (B-1) to (B-3) of Examples 2 and 3 and Comparative Examples 1 to 3 were obtained in the same manner as in Example 1 except that the polyamic acid solutions (2) to (6) were used instead of the polyamic acid solution (1).
[0224] [Example 4]
[0225] The polyimide solution (1) (3.0 g) obtained in Synthesis Example 4, the liquid crystal aligning agent (A-1) (7.0 g) obtained in Example 1, and AD-1 (0.04 g) were mixed to obtain a liquid crystal aligning agent (C-1).
[0226] [Examples 5, 6, Comparative Examples 4 to 6]
[0227] Liquid crystal aligning agents (C-2), (C-3), (D-1) to (D-3) of Examples 5 and 6 and Comparative Examples 4 to 6 were obtained in the same manner as in Example 4 except that the liquid crystal aligning agents (A-2), (A-3), and (B-1) to (B-3) were used instead of the liquid crystal aligning agent (A-1).
[0228] [Example 7]
[0229] The polyimide solution (2) (3.0 g) obtained in Synthesis Example 5 and the liquid crystal aligning agent (A-1) (7.0 g) obtained in Example 1 were mixed to obtain a liquid crystal aligning agent (C-4).
[0230] [Example 8, Comparative Examples 7 and 8]
[0231] Liquid crystal aligning agents (C-5), (D-4), and (D-5) of Example 8 and Comparative Examples 7 and 8 were obtained in the same manner as in Example 7 except that the liquid crystal aligning agents (A-3), (B-1), and (B-3) were used instead of the liquid crystal aligning agent (A-1).
[0232] In the liquid crystal aligning agents (A-1) to (A-3), (B-1) to (B-3), (C-1) to (C-5), and (D-1) to (D-5) obtained as described above, no abnormalities such as turbidity and precipitation were observed, and it was confirmed that they were uniform solutions. Using the obtained liquid crystal aligning agents, transmittance evaluation, liquid crystal cell preparation, voltage holding ratio evaluation, and residual DC voltage evaluation were performed.
[0233] [Evaluation of transmittance]
[0234] The liquid crystal alignment agents (A-1) to (A-3), (C-1) to (C-5), (B-1) to (B-3), and (D-1) to (D-5) obtained in the examples and comparative examples were spin-coated on a quartz substrate and dried on a hot plate at 70°C for 90 seconds. Then, they were calcined in an IR (infrared) oven at 230°C for 20 minutes to form a coating with a film thickness of 100 nm, thereby obtaining a substrate with a liquid crystal alignment film. The substrate with the liquid crystal alignment film was set to the inner side, and another quartz substrate was used to sandwich a refractive liquid (contact liquid manufactured by Shimadzu Equipment Manufacturing Co., Ltd.) for the purpose of preventing interference of light. In the evaluation of the transmittance, the measuring device used was UV-3600 (manufactured by Shimadzu Corporation), and the measurement was carried out at a temperature of 25°C and a scanning wavelength of 380 to 800 nm. At this time, a reference was used in which two uncoated quartz substrates were used to sandwich a refractive liquid. The transmittance at a wavelength of 580 nm was used as a reference, and its value is shown in Table 2 below. An example of the relationship between wavelength and transmittance is shown in Figure 1 .
[0235] [Preparation of Liquid Crystal Display Element for Evaluation of Voltage Holding Ratio and Residual DC Characteristics]
[0236] Liquid crystal aligning agents (A-1) to (A-3), (C-1) to (C-3), (B-1) to (B-3), and (D-1) to (D-3) obtained in the examples and comparative examples were used to produce a liquid crystal box in the order described below. The liquid crystal aligning agent was spin-coated on a glass substrate with an ITO electrode, dried on a hot plate at 70°C for 90 seconds, and then fired in an IR oven at 230°C for 20 minutes to form a liquid crystal aligning film with a thickness of 100 nm. Two substrates with the liquid crystal aligning film were prepared, and a bead-shaped spacer with a diameter of 4 μm (made by JGC Catalysts & Chemicals, silk balls, SW-D1) was coated on the liquid crystal aligning film of one of the substrates, and a thermosetting sealant (made by Mitsui Chemicals, XN-1500T) was printed. Next, the surface of the other substrate on which the liquid crystal aligning film was formed was set to the inner side, and after being bonded to the previous substrate, the sealant was cured to produce an empty box. Liquid crystal MLC-3023 (Merck) was injected into the empty cell by the reduced pressure injection method to produce a liquid crystal cell. Then, a DC voltage of 15 V was applied to the liquid crystal cell and 10 J / cm 2UV that passed through a cutoff filter below 325 nm. It should be noted that the UV illuminance was measured using UV-MO3A manufactured by ORC. Then, in order to deactivate the unreacted polymerizable compound remaining in the liquid crystal box, UV (UV lamp: FLR40SUV32 / A-1) was irradiated for 30 minutes using a UV-FL irradiation device manufactured by Toshiba Lighting & Technology without applying voltage.
[0237] [Preparation of Liquid Crystal Display Element for Evaluation of Afterimage Characteristics]
[0238] Liquid crystal cells were prepared in the following order using the liquid crystal aligning agents (A-2), (C-1) to (C-3), (B-2), (D-1) to (D-3) obtained in the examples and comparative examples. The liquid crystal aligning agents were spin-coated on an ITO electrode substrate (length: 35 mm, width: 30 mm, thickness: 0.7 mm) on which an ITO electrode pattern with a pixel size of 200 μm×600 μm and a line width / line spacing of 3 μm was formed and on an ITO surface of a glass substrate (length: 35 mm, width: 30 mm, thickness: 0.7 mm) on which an optical spacer (photo spacer) with a height of 3.2 μm was patterned, dried on a hot plate at 70°C for 90 seconds, and then fired in an IR oven at 230°C for 20 minutes to form a liquid crystal aligning film with a film thickness of 100 nm. The ITO electrode substrate on which the ITO electrode pattern is formed is divided into four crosschecker (grid) patterns, and can be driven separately for each of the four regions.
[0239] Next, a sealant (XN-1500T manufactured by Mitsui Chemicals) was printed. Next, the surface of the other substrate on which the liquid crystal alignment film was formed was set to the inner side, and after being bonded to the previous substrate, the sealant was cured to produce an empty box. Liquid crystal MLC-3023 (manufactured by MERCK) was injected into the empty box by the reduced pressure injection method to produce a liquid crystal box. While applying a DC voltage of 15V to the liquid crystal box, 10J / cm 2 UV that passed through a cutoff filter below 325 nm. It should be noted that the UV illuminance was measured using UV-MO3A manufactured by ORC. Then, in order to deactivate the unreacted polymerizable compound remaining in the liquid crystal box, UV was irradiated for 30 minutes using a UV-FL irradiation device manufactured by Toshiba Lighting & Technology without applying voltage (UV lamp: FLR40SUV32 / A-1).
[0240] [Evaluation of voltage holding ratio]
[0241] The voltage holding rate was measured using a liquid crystal box for evaluating the voltage holding rate after UV irradiation. A voltage of 1V was applied for 60μs in a hot air circulation oven at 60°C, and then the voltage was measured after 16.67msec. The voltage holding rate was calculated as the voltage holding rate. VHR-1 manufactured by TOYO Corporation was used in the determination of the voltage holding rate. The values are shown in Table 2 below.
[0242] [Evaluation of residual DC voltage]
[0243] A 30 Hz, 7.8 Vpp rectangular wave with a DC voltage of 2 V was applied to the liquid crystal box prepared above for voltage retention evaluation at 25° C. for 100 hours, and the voltage (residual DC voltage) remaining in the liquid crystal box 1 hour after the DC voltage was cut off was obtained by the flicker elimination method. The values are shown in Table 2 below.
[0244] [Afterimage characteristics]
[0245] Using the liquid crystal box for afterimage characteristic evaluation prepared above, an AC voltage of 60 Hz and 20 Vp-p was applied to two diagonal areas of four pixel areas, and the drive was performed at a temperature of 25°C for 168 hours. Then, all four pixel areas were driven with an AC voltage of 5 Vp-p, and the brightness difference of the pixels was visually observed. The state in which almost no brightness difference was confirmed was considered good, and the evaluation results are shown in Table 2.
[0246] [Brush resistance]
[0247] The liquid crystal alignment agents (C-4), (C-5), (B-1), (B-3), (D-4), and (D-5) obtained in the examples and comparative examples were spin-coated on the ITO surface of a glass substrate with an ITO electrode on the entire surface, and temporarily dried on a hot plate at 70°C for 90 seconds. Then, they were sintered in an IR oven at 230°C for 20 minutes to form a coating film with a film thickness of 100 nm, thereby obtaining a substrate with a liquid crystal alignment film. The liquid crystal alignment film was brushed with rayon cloth (roller diameter: 120 mm, roller rotation speed: 1000 rpm, moving speed: 20 mm / sec, pressing length: 0.6 mm). The substrate was observed under a microscope, and the case where no stripes were observed on the film surface due to brushing was evaluated as "good", and the case where stripes were observed was evaluated as "poor", and the results are shown in Table 2.
[0248] [Table 2]
[0249]
[0250] As shown in Table 2 and Figure 1As shown, it can be seen that for the evaluation results of the transmittance of the liquid crystal alignment agents (A-1) to (A-3) and (C-1) to (C-5) obtained in Examples 1 to 8, compared with the corresponding evaluation results of the transmittance of the liquid crystal alignment agents (B-1) to (B-3) and (D-1) to (D-5) obtained in Comparative Examples 1 to 8, a liquid crystal alignment film with high transmittance can be obtained. It should be noted that a difference of 1% in transmittance is a significant difference in the technical field of this invention. On the other hand, it can be seen that in the evaluation of voltage holding ratio, residual DC voltage, afterimage characteristics, and brush abrasion resistance, liquid crystal alignment films having the same degree of characteristics can be obtained.
[0251] In addition, the liquid crystal display element using the liquid crystal aligning agents (C-1) to (C-3) shows a high voltage holding characteristic compared to the liquid crystal display element using the liquid crystal aligning agents (A-1) to (A-3). That is, by mixing the polyimide solution (1) without a diphenylamine skeleton, a liquid crystal aligning film with a high transmittance can be obtained, and a liquid crystal display element with a high voltage holding ratio can be obtained.
[0252] Furthermore, the liquid crystal display element using the liquid crystal aligning agents (C-4) and (C-5) exhibits good brush abrasion resistance. That is, by mixing the polyimide solution (2) without a diphenylamine skeleton, a liquid crystal aligning film having a high transmittance can be obtained, and a liquid crystal display element exhibiting good brush abrasion resistance can be obtained.
[0253] It should be noted that the entire contents of the specification, claims, drawings, and abstract of Japanese Patent Application No. 2020-044505 filed on Mar. 13, 2020 are incorporated herein by reference in their entirety and are incorporated as a disclosure of the specification of the present invention.
Claims
1. A polyimide varnish comprising at least one block copolymer selected from the group consisting of a polyimide precursor and a polyimide obtained by imidizing the polyimide precursor, wherein the polyimide precursor has a block (b1) comprising a repeating unit represented by the following formula (1) and a block (b2) comprising a repeating unit represented by the following formula (2), In the formula, X1 represents a tetravalent organic group; X2 represents a tetravalent organic group derived from acyclic aliphatic tetracarboxylic dianhydride or a tetravalent organic group represented by the following formula (X2); Y1 represents a divalent organic group having 3 to 50 carbon atoms and not having a diphenylamine skeleton; Y2 represents a divalent organic group having a diphenylamine skeleton and having a structure represented by the following formula (d2); two R1 and R2 each independently represent a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and two Z1 and Z2 each independently represent a hydrogen atom, an alkyl group having 1 to 10 carbon atoms optionally having a substituent, an alkenyl group having 2 to 10 carbon atoms optionally having a substituent, an alkynyl group having 2 to 10 carbon atoms optionally having a substituent, a tert-butoxycarbonyl group, or a 9-fluorenylmethoxycarbonyl group, In formula (X2), R 21 ~R 24 each independently represents a hydrogen atom, a methyl group, an ethyl group, a propyl group, a chlorine atom or a phenyl group, In formula (d2), A1 represents a single bond, -NR-, -O-, -C(=O)-, -C(=O)NR-, -C(=O)O-, or a divalent organic group, in the -NR-, R represents a hydrogen atom or a monovalent organic group, in the -C(=O)NR-, R represents a hydrogen atom or a monovalent organic group; R1 and R2 each independently represent a hydrogen atom or a monovalent organic group; when n is 2, there are multiple A1 and R2 each independently having the above definition.
2. The polyimide varnish according to claim 1, wherein In formula (1), X1 represents at least one selected from the group consisting of structures represented by the following formulae (X1-1) to (X1-12), 3. The polyimide varnish according to claim 1 or 2, wherein In formula (1), Y1 represents at least one selected from the group consisting of a divalent organic group having 3 to 50 carbon atoms and having a structure represented by the following formulae (S1) to (S3) and a divalent organic group having 3 to 50 carbon atoms and not having a structure represented by the above formulae (S1) to (S3), The divalent organic group having 3 to 50 carbon atoms and the divalent organic group having no structure represented by the formulae (S1) to (S3) and the divalent organic group having 3 to 50 carbon atoms and not having the structure represented by the formulae (S1) to (S3) do not have a diphenylamine skeleton. In formula (S1), X 1 and X 2 Each independently represents a single bond, -(CH2) a -, -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -COO-, -OCO- or -((CH2) a1 -A1) m1 -, said -(CH2) a -, a is an integer of 1 to 15; wherein a1 is an integer of 1 to 15, A1 is an oxygen atom or -COO-, and m1 is 1 to 2; G 1 and G 2 Each independently represents a divalent cyclic group selected from a divalent aromatic group having 6 to 12 carbon atoms and a divalent alicyclic group having 3 to 8 carbon atoms; any hydrogen atom on the cyclic group is optionally substituted; m and n are each independently an integer of 0 to 3, and m+n is 1 to 4; R 1 represents an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or an alkoxyalkyl group having 2 to 20 carbon atoms, forming R 1 Any hydrogen atom of is optionally substituted by a fluorine atom; when m, n and m1 are 2 or more, there are multiple X 1 , X 2 , G 1 , G 2 , a1, m1 and A1 are independently defined above, —X 3 -R 2 (S2) In formula (S2), X 3 represents a single bond, -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -CH2O-, -COO- or -OCO-; R 2 represents an alkyl group having 1 to 20 carbon atoms or an alkoxyalkyl group having 2 to 20 carbon atoms, forming R 2 Any hydrogen atom of is optionally substituted by a fluorine atom, -X 4 -R 3 (S3) In formula (S3), X 4 Indicates -CONH-, -NHCO-, -O-, -CH2O-, -COO- or -OCO-; R 3 It indicates a structure having a steroidal skeleton.
4. The polyimide varnish according to claim 3, wherein In formula (1), at least one of Y1 represents a divalent organic group having 3 to 50 carbon atoms and having a structure represented by formulas (S1) to (S3).
5. The polyimide varnish according to claim 3, wherein In formula (1), at least one of Y1 represents a divalent organic group having 3 to 50 carbon atoms and not having the structure represented by formulas (S1) to (S3).
6. The polyimide varnish according to claim 3 or 5, wherein The divalent organic group having 3 to 50 carbon atoms and not having the structure represented by the formulae (S1) to (S3) is a divalent organic group having a nitrogen-containing heterocycle in the molecule, a divalent organic group having a free radical initiating function, a divalent organic group having a carboxyl group, a group having a group "-N(D)-", a group having a photo-alignment property, a divalent organic group having an oxygen-containing heterocycle, or a divalent organic group derived from an aromatic diamine having no side chain group having 3 or more carbon atoms, wherein -N(D)-, D is a tert-butoxycarbonyl group.
7. The polyimide varnish according to claim 1 or 2, wherein: In formula (2), X2 represents at least one selected from the group consisting of structures represented by the following formulae (X2-1) to (X2-4), 8. The polyimide varnish according to claim 1 or 2, wherein The ratio of the total molar number of the repeating units represented by the formula (1) to the total molar number of the repeating units represented by the formula (2) per molecule of the block copolymer is 1:9 to 9:
1.
9. The polyimide varnish according to claim 1 or 2, wherein: The polyimide varnish further contains at least one polymer (P) selected from the group consisting of a polyimide precursor and a polyimide obtained by imidizing the polyimide precursor, wherein the polyimide precursor has a repeating unit represented by the following formula (3): In formula (3), X3 represents a tetravalent organic group; Y3 represents a divalent organic group having 3 to 50 carbon atoms and not having a diphenylamine skeleton; R3 and Z3 are synonymous with R1 and Z1 in formula (1); two R3 and Z3 each independently have the above definitions.
10. The polyimide varnish according to claim 9, wherein The polymer (P) does not have a diphenylamine skeleton.
11. A method for producing a polyimide varnish, which is a method for producing the polyimide varnish according to any one of claims 1 to 10, the method comprising: Step (I), reacting a tetracarboxylic acid component including tetracarboxylic dianhydride represented by the following formula (1-T) or a derivative thereof with a diamine component including a diamine represented by the following formula (1-D) to obtain a block (b1); and Step (II) of adding a tetracarboxylic acid component including tetracarboxylic dianhydride represented by the following formula (2-T) or a derivative thereof and a diamine component including a diamine represented by the following formula (2-D) to the block (b1) and reacting them to obtain a polyimide precursor having the block (b1) and the block (b2); In the formula, X1, X2, Y1, and Y2 are the same as X1, X2, Y1, and Y2 defined in formula (1) and formula (2).
12. The method for producing a polyimide varnish according to claim 11, wherein: The reaction temperature in the step (II) is lower than the reaction temperature in the step (I).
13. A method for producing a polyimide varnish, which is a method for producing the polyimide varnish according to any one of claims 1 to 10, the method comprising: Step (III), reacting a tetracarboxylic acid component including tetracarboxylic dianhydride represented by the following formula (1-T) or a derivative thereof with a diamine component including a diamine represented by the following formula (1-D) to obtain a block (b1); Step (IV), reacting a tetracarboxylic acid component including tetracarboxylic dianhydride represented by the following formula (2-T) or a derivative thereof with a diamine component including a diamine represented by the following formula (2-D) to obtain a block (b2); and Step (V), coupling the block (b1) obtained in the step (III) with the block (b2) obtained in the step (IV) to obtain a polyimide precursor having the block (b1) and the block (b2), In the formula, X1, X2, Y1, and Y2 are the same as X1, X2, Y1, and Y2 defined in formula (1) and formula (2).
14. The method for producing a polyimide varnish according to claim 13, wherein: The reaction temperature in the step (IV) is lower than the reaction temperature in the step (III). 15 . A liquid crystal aligning agent obtained from the polyimide varnish according to claim 1 . 16 . A liquid crystal alignment film, formed using the liquid crystal alignment agent according to claim 15 . 17 . A liquid crystal display element comprising the liquid crystal alignment film according to claim 16 .
18. A method for manufacturing a liquid crystal display element, which is the following method: The liquid crystal alignment agent as described in claim 15 is applied on a pair of substrates having a conductive film to form a coating film, and the coating films are arranged opposite to each other with a layer of liquid crystal molecules therebetween to form a liquid crystal box, and the liquid crystal box is irradiated with light while a voltage is applied between the conductive films of the pair of substrates.
Citation Information
Patent Citations
Material for liquid crystal alignment and liquid crystal displays made by using the same
WO2004021076A1
Liquid-crystal alignment agent, liquid-crystal alignment film, and liquid-crystal display element
WO2011132751A1
Liquid crystal aligning agent, liquid crystal alignment film, and liquid crystal display element
WO2013008822A1
Liquid crystal aligning agent, liquid crystal alignment film, and liquid crystal display element
WO2014119682A1
LCD element
WO2016047771A1