An arrayed molybdenum-doped cobalt diselenide composite material and its preparation method and application

Through the preparation of arrayed molybdenum-doped cobalt diselenide composite material, the problems of poor conductivity and volume changes of the negative electrode material of sodium ion battery are solved, and the battery performance with high capacity and long life is achieved, suitable for flexible electronic devices, and improved Electron and ion transfer efficiency.

CN115249797BActive Publication Date: 2024-11-26ZHEJIANG SCI-TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111623603.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-28
Publication Date
2024-11-26
Estimated Expiration
2041-12-28

AI Technical Summary

Technical Problem

The transition metal selenide, the existing sodium ion battery negative electrode material, limits its large-scale application due to poor conductivity and volume changes in electrochemical cycles.

Method used

Using arrayed molybdenum-doped cobalt diselenide composite material, the preparation process is simplified through MOF template, ion exchange and carbon coating technology, reducing electrode impedance, providing rich electron transport channels, and improving conductivity through Mo ion doping stability.

Benefits of technology

It achieves the performance of sodium ion battery with high capacity and long cycle life, is suitable for flexible electronic devices, and improves the efficiency of electron and ion transfer, alleviates the problem of volume expansion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115249797B_ABST
    Figure CN115249797B_ABST
Patent Text Reader

Abstract

The invention discloses an arrayed molybdenum-doped cobalt diselenide composite material and its preparation method and application, the method comprising: immersing a flexible conductive substrate in a mixed solution of 2-methylimidazole and cobalt nitrate to obtain a cobalt-based metal organic framework precursor with a unique structure; after cleaning and drying, placing it in a sodium molybdate solution for water bath reaction to obtain a molybdenum-cobalt double metal hydroxide array with intact structure; followed by electro-deposition coating of polypyrrole and selenization treatment to obtain an arrayed carbon-coated molybdenum-doped cobalt diselenide composite material. Molybdenum doping can improve the conductivity and electrode reaction kinetics of cobalt diselenide, and the arraying and carbon coating design can avoid the use of polymer binders, simplify the electrode preparation process, and effectively alleviate the volume expansion and contraction problems of cobalt diselenide during the process of sodium insertion and extraction. When the prepared composite electrode is used as the negative electrode material of a sodium ion battery, it exhibits excellent electrochemical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of negative electrode materials for sodium ion batteries, and in particular to an arrayed molybdenum-doped cobalt diselenide composite material and a preparation method and application thereof. Background Art

[0002] In recent years, flexible electronic devices have been increasingly used in fields such as flexible sensors, wearable devices, energy storage, and medical implants. Therefore, the development of flexible batteries as energy supply carriers has received increasing attention. Among them, sodium-ion batteries (SIBs) have attracted widespread attention from researchers due to their abundant sodium resource reserves and lower costs, highlighting their great potential as a new generation of energy storage batteries. Negative electrode materials play a vital role in improving the performance of sodium-ion batteries, among which transition metal selenides have attracted widespread attention due to their high specific capacity. However, their poor conductivity and the huge volume changes caused by the insertion and extraction of sodium during the electrochemical cycle result in rapid capacity decay at high currents, limiting their large-scale application.

[0003] In order to solve the above problems, researchers have conducted a lot of exploration and research on metal selenide materials, and found that after certain regulation of the composition and microstructure of these materials, it is beneficial to improve the storage performance of sodium ions. In terms of composition regulation, researchers usually use metal ion doping to improve the conductivity of selenides, and the defects introduced by doping are conducive to the embedding and extraction of sodium ions, thereby improving the electrochemical properties of electrode materials. In addition, in terms of microstructural design, the composite of selenide and carbon material can stabilize the microstructure of metal selenide and avoid the powdering of electrode materials due to huge volume changes and stress during the embedding and extraction of sodium. At the same time, carbon materials as conductive matrix coating metal selenides can also improve conductivity. However, the metal selenide powder materials modified by the above means still need to be made into electrodes by slurry coating, which is not suitable for flexible electronic devices. Summary of the invention

[0004] In view of the problems in the background technology, the purpose of the present invention is to provide an arrayed molybdenum-doped cobalt diselenide composite material and its preparation method and application. The present invention develops a binder-free arrayed molybdenum-doped cobalt diselenide composite electrode material, which not only simplifies the cumbersome preparation steps compared to traditional electrodes, but also reduces the impedance of the electrode and provides abundant electron transmission channels; metal ion doping selenides can accelerate the electron and ion diffusion kinetics of transition metal selenides; the stability carbon buffer layer can ensure rapid electron and ion transfer and alleviate volume expansion. When the above strategies are used for sodium ion battery negative electrode materials, they have higher capacity and longer cycle life.

[0005] Based on the above strategy, the present invention synthesizes a MOF with a unique structure as a template, and then successfully implements the incorporation of Mo ions by methods such as ion exchange, and then performs a carbon coating treatment and a one-step selenization treatment, thereby further obtaining an arrayed molybdenum-doped cobalt diselenide composite material with excellent performance.

[0006] A method for preparing an arrayed molybdenum-doped cobalt diselenide composite material comprises the following steps:

[0007] (1) stirring and mixing a cobalt salt aqueous solution and a 2-methylimidazole aqueous solution to obtain a mixed solution A;

[0008] (2) transferring the mixed solution A obtained in step (1) to a reaction kettle and adding a flexible substrate, and after standing for a period of time, taking out the flexible substrate, washing, and drying it to obtain a precursor cobalt-based metal organic framework (Co-MOF) array;

[0009] (3) dissolving sodium molybdate in water, then adding ethanol, mixing and stirring, and obtaining a mixed solution B. immersing the precursor Co-MOF array in solution B for a water bath, and after the water bath is completed, washing and drying to obtain a double metal hydroxide Mo-Co LDH array;

[0010] (4) dissolving pyrrole (Py), sodium dodecylbenzene sulfonate (SDBS), and sodium chloride in deionized water, stirring and mixing, and obtaining a mixed solution C. The Mo-Co LDH array obtained in step (3) is immersed in solution C for electro-deposition coating of polypyrrole (PPy), and after the deposition is completed, the Mo-Co LDH array is washed and dried to obtain a Mo-Co LDH@PPy array;

[0011] (5) Selenium powder and the Mo-Co LDH@PPy in the above step (4) are placed in a tube furnace, heat treated under inert gas protection, and naturally cooled to obtain a carbon-coated molybdenum-doped cobalt diselenide (Mo-Co Se2@C) array.

[0012] The following is a preferred technical solution of the present invention:

[0013] In step (1), the mixed solution A comprises the following components:

[0014] Water 60-100 mL;

[0015] Cobalt salt 1-3mmol;

[0016] 2-Methylimidazole 8-24mmol;

[0017] Wherein, the cobalt salt is one of cobalt nitrate, cobalt chloride and cobalt sulfate, the stirring time is 5-30 minutes, and solution A is a purple suspension.

[0018] In step (2), the reaction temperature is 10-60° C. and the reaction time is 3-5 hours.

[0019] In step (3), the amount of sodium molybdate is 0.1-1.0 g, and the total amount of water and ethanol is 100 mL, wherein the volume ratio of water to ethanol is 1:3-5 (preferably 1:4). The water bath temperature is 70-95°C, and the time is 10-20 minutes.

[0020] In step (4), the mixed solution B comprises the following components:

[0021]

[0022] The electrodeposition was carried out by cyclic voltammetry with the following parameters: deposition cycle number was 2-6 cycles, voltage range was 0.2-0.7V, scan rate was 0.1-2.0mVs -1 .

[0023] In step (5), the calcination atmosphere for heat treatment is nitrogen or argon, the temperature is 300-500°C, the insulation time is 1-3 hours, and the heating rate is 1-5°C / minute.

[0024] The arrayed molybdenum-doped cobalt diselenide composite material has a Mo-CoSe2@C content of 0.9-1.3 mg cm -2 .

[0025] The arrayed molybdenum-doped cobalt diselenide composite material comprises a molybdenum-doped cobalt diselenide sheet material uniformly grown on a substrate, characterized in that it exhibits a regular and orderly sheet structure before calcination, and still maintains a well-regulated morphology after carbon coating and calcination, and the length of the sheet is 1-2 μm.

[0026] The molybdenum-doped cobalt diselenide composite material array is used as the negative electrode material of the sodium ion battery. The obtained arrayed molybdenum-doped cobalt diselenide composite material is cut into 1cm*1cm square pieces and directly used as the working electrode. The sodium metal foil is used as the counter electrode and the reference electrode. At the same time, the glass fiber membrane is used as the diaphragm. The electrolyte is 1M NaClO4 dissolved in a mixed solvent of ethylene carbonate and dimethyl carbonate (EC / DMC volume ratio is 1:1), and 5% by weight of fluoroethylene carbonate (FEC) is added as an additive. When assembling the battery, the negative electrode shell, electrode material, diaphragm, electrolyte, sodium metal foil, gasket, shrapnel and positive electrode shell are assembled from bottom to top, and the operation is completed in a glove box filled with argon.

[0027] After the assembled sodium-ion battery was placed for 12 hours, a constant current charge and discharge test was performed with a charge and discharge voltage of 3V-0.01V. The specific capacity, rate performance, and charge and discharge cycle performance of the sodium-ion battery negative electrode were measured in an environment of 25±1℃.

[0028] Compared with the prior art, the present invention has the following advantages:

[0029] (1) The present invention develops a binder-free arrayed molybdenum-doped cobalt diselenide composite electrode material for use in sodium ion batteries. Compared with traditional electrodes, it not only eliminates and simplifies the cumbersome electrode preparation steps, but also reduces the impedance of the electrode, provides an orderly and rich electron transmission channel, and is suitable for flexible electronic devices.

[0030] (2) The prepared arrayed molybdenum-doped cobalt diselenide composite material successfully achieved the introduction of Mo ions, showing a specific capacity exceeding that of a single component, that is, the specific capacity of the composite electrode exceeds the theoretical specific capacity of cobalt diselenide. Mo ion doping is beneficial to increase the lattice size of metal selenides, improve their electrical conductivity and electrochemical activity, and accelerate the diffusion kinetics of electrons and ions in transition metal selenides, thereby obtaining sodium storage performance that exceeds that of single-component transition metal selenides.

[0031] (3) The prepared arrayed molybdenum-doped cobalt diselenide composite material was successfully carbon-coated. The stable carbon buffer layer can ensure rapid electron and ion transfer during charging and discharging, and alleviate the volume expansion and contraction caused by sodium insertion and extraction. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The X-ray diffraction (XRD) pattern of the arrayed molybdenum-doped cobalt diselenide composite material prepared in Example 1;

[0033] Figure 2 The following are scanning electron microscope (SEM) images of the precursor Co-MOF prepared in Example 1 at different magnifications;

[0034] Figure 3 The SEM images of Mo-Co LDH prepared in Example 1 at different magnifications;

[0035] Figure 4 The SEM images of Mo-Co LDH@PPy prepared in Example 1 at different magnifications;

[0036] Figure 5 The SEM images of the arrayed molybdenum-doped cobalt diselenide Mo-CoSe2@C composite electrode material prepared in Example 1 at different magnifications;

[0037] Figure 6 The battery cycle performance of the arrayed molybdenum-doped cobalt diselenide composite electrode material prepared in Example 1;

[0038] Figure 7 This is the battery rate performance of the arrayed molybdenum-doped cobalt diselenide composite electrode material prepared in Example 1. DETAILED DESCRIPTION

[0039] The present invention is further described in detail below by way of examples, but the present invention is not limited to the following examples.

[0040] Example 1

[0041] (1) 40 mL of an aqueous solution containing 0.5821 g of cobalt nitrate hexahydrate and 40 mL of an aqueous solution containing 1.3137 g of 2-methylimidazole (molar ratio 1:8) were mixed and stirred for 10 minutes to obtain a mixed solution A;

[0042] (2) transferring the mixed solution A obtained in step (1) to a reactor and adding carbon cloth, standing at 25° C. for 4 hours, taking out the sample, washing it alternately with water and anhydrous ethanol three times, and drying it to obtain a precursor Co-MOF array;

[0043] (3) 0.2 g of sodium molybdate dihydrate was first dissolved in 20 mL of water, and then 80 mL of ethanol was added, and the mixture was stirred for 5 minutes to obtain a mixed solution B. Then, the precursor Co-MOF array was immersed in the mixed solution B and placed in a water bath at 85°C for 12 minutes. After the water bath ended, the sample was washed alternately with water and anhydrous ethanol three times, and dried to obtain a double metal hydroxide Mo-Co LDH array;

[0044] (4) 70 μL of pyrrole, 0.384 g of sodium dodecylbenzene sulfonate (SDBS), and 0.0583 g of sodium chloride were dissolved in 100 mL of deionized water, and the mixture was stirred for 30 minutes to obtain a mixed solution C. The Mo-Co LDH array obtained in step (3) was immersed in solution C for electrodeposition by cyclic voltammetry with a voltage range of 0.2-0.7 V, a deposition cycle of 4 cycles, and a scan rate of 1.0 mVs -1 After the deposition, the Mo-Co LDH@PPy array was obtained by washing with water and anhydrous ethanol three times alternately and drying.

[0045] (5) Take 3.0 mg of selenium powder and the Mo-Co LDH@PPy in the above step (4) in a tube furnace, and under nitrogen protection, heat the temperature to 400°C at a heating rate of 2°C / min and keep it at this temperature for 2 hours for selenization treatment. After natural cooling, a Mo-CoSe2@C array is obtained.

[0046] Figure 1 This is the XRD pattern of the arrayed molybdenum-doped cobalt diselenide composite material prepared in Example 1. Figure 1 It can be seen that the molybdenum-doped cobalt diselenide composite material prepared in Example 1 shows characteristic peaks of cobalt diselenide with a makassite structure (JCPDS No. 53-0449) and cobalt diselenide with a pyrite structure (JCPDS No. 09-0234). Figure 2These are SEM images of the precursor Co-MOF prepared in Example 1 at different magnifications. The surface of the precursor Co-MOF array is smooth, and the length of the sheet is 1-2 μm. Figure 3 These are SEM images of the Mo-Co LDH prepared in Example 1 at different magnifications, and the surface is relatively rough. Figure 4 These are SEM images of Mo-Co LDH@PPy prepared in Example 1 at different magnifications. The flakes are obviously thickened, and the structure does not collapse and remains intact. Figure 5 The SEM images of the arrayed Mo-CoSe2@C composite material prepared in Example 1 at different magnifications have a complete flake array structure and a flake size of 1-2 μm.

[0047] Example 2

[0048] (1) 40 mL of an aqueous solution containing 1.1246 g of cobalt sulfate hexahydrate and 40 mL of an aqueous solution containing 1.3137 g of 2-methylimidazole (molar ratio 1:4) were mixed and stirred for 10 minutes to obtain a mixed solution A;

[0049] (2) transferring the mixed solution A obtained in step (1) to a reactor and adding carbon cloth, standing at 25° C. for 4 hours, taking out the sample, washing it alternately with water and anhydrous ethanol three times, and drying it to obtain a precursor Co-MOF array;

[0050] (3) 0.2 g of sodium molybdate dihydrate was first dissolved in 20 mL of water, and then 80 mL of ethanol was added, and the mixture was stirred for 5 minutes to obtain a mixed solution B. Then, the precursor Co-MOF array was immersed in the mixed solution B and placed in a water bath at 85°C for 12 minutes. After the water bath ended, the sample was washed alternately with water and anhydrous ethanol three times, and dried to obtain a double metal hydroxide Mo-Co LDH array;

[0051] (4) 70 μL of pyrrole, 0.384 g of sodium dodecylbenzene sulfonate (SDBS), and 0.0583 g of sodium chloride were dissolved in 100 mL of deionized water, and the mixture was stirred for 30 minutes to obtain a mixed solution C. The Mo-Co LDH array obtained in step (3) was immersed in solution C for electrodeposition by cyclic voltammetry with a voltage range of 0.2-0.7 V, a deposition cycle of 4 cycles, and a scan rate of 1.0 mVs -1 After the deposition, the Mo-Co LDH@PPy array was obtained by washing with water and anhydrous ethanol three times alternately and drying.

[0052] (5) Take 3.0 mg of selenium powder and the Mo-Co LDH@PPy in the above step (4) in a tube furnace, and under nitrogen protection, heat the temperature to 400°C at a heating rate of 2°C / min and keep it at this temperature for 2 hours for selenization treatment. After natural cooling, a Mo-CoSe2@C array is obtained.

[0053] Example 3

[0054] (1) 40 mL of an aqueous solution containing 0.2379 g of cobalt chloride hexahydrate and 40 mL of an aqueous solution containing 1.3137 g of 2-methylimidazole (molar ratio 1:16) were mixed and stirred for 10 minutes to obtain a mixed solution A;

[0055] (2) transferring the mixed solution A obtained in step (1) to a reactor and adding carbon cloth, standing at 25° C. for 4 hours, taking out the sample, washing it alternately with water and anhydrous ethanol three times, and drying it to obtain a precursor Co-MOF array;

[0056] (3) 0.2 g of sodium molybdate dihydrate was first dissolved in 20 mL of water, and then 80 mL of ethanol was added, and the mixture was stirred for 5 minutes to obtain a mixed solution B. Then, the precursor Co-MOF array was immersed in the mixed solution B and placed in a water bath at 85°C for 12 minutes. After the water bath ended, the sample was washed alternately with water and anhydrous ethanol three times, and dried to obtain a double metal hydroxide Mo-Co LDH array;

[0057] (4) 70 μL of pyrrole, 0.384 g of sodium dodecylbenzene sulfonate (SDBS), and 0.0583 g of sodium chloride were dissolved in 100 mL of deionized water, and the mixture was stirred for 30 minutes to obtain a mixed solution C. The Mo-Co LDH array obtained in step (3) was immersed in solution C for electrodeposition by cyclic voltammetry with a voltage range of 0.2-0.7 V, a deposition cycle of 4 cycles, and a scan rate of 1.0 mVs -1 After the deposition, the Mo-Co LDH@PPy array was obtained by washing with water and anhydrous ethanol three times alternately and drying.

[0058] (5) Take 3.0 mg of selenium powder and the Mo-Co LDH@PPy in the above step (4) in a tube furnace, and under nitrogen protection, heat the temperature to 400°C at a heating rate of 2°C / min and keep it at this temperature for 2 hours for selenization treatment. After natural cooling, a Mo-CoSe2@C array is obtained.

[0059] Example 4

[0060] (1) 40 mL of an aqueous solution containing 0.5821 g of cobalt nitrate hexahydrate and 40 mL of an aqueous solution containing 1.3137 g of 2-methylimidazole were mixed and stirred for 10 minutes to obtain a mixed solution A;

[0061] (2) transferring the mixed solution A obtained in step (1) to a reactor and adding carbon cloth, standing at 25° C. for 4 hours, taking out the sample, washing it alternately with water and anhydrous ethanol three times, and drying it to obtain a precursor Co-MOF array;

[0062] (3) 0.2 g of sodium molybdate dihydrate was first dissolved in 20 mL of water, and then 80 mL of ethanol was added, and the mixture was stirred for 5 minutes to obtain a mixed solution B. Then, the precursor Co-MOF array was immersed in the mixed solution B and placed in a water bath at 70°C for 12 minutes. After the water bath ended, the sample was washed alternately with water and anhydrous ethanol three times, and dried to obtain a double metal hydroxide Mo-Co LDH array;

[0063] (4) 100 μL of pyrrole, 0.384 g of sodium dodecylbenzene sulfonate (SDBS), and 0.0583 g of sodium chloride were dissolved in 100 mL of deionized water, and the mixture was stirred for 30 minutes to obtain a mixed solution C. The Mo-Co LDH array obtained in step (3) was immersed in solution C for electrodeposition by cyclic voltammetry with a voltage range of 0.2-0.7 V, a deposition cycle of 4 cycles, and a scan rate of 1.0 mVs -1 After the deposition, the Mo-Co LDH@PPy array was obtained by washing with water and anhydrous ethanol three times alternately and drying.

[0064] (5) 3.0 mg of selenium powder and the Mo-Co LDH@PPy prepared in step (4) were placed in a tube furnace, heated to 300 °C at a heating rate of 2 °C / min under nitrogen protection, and kept at this temperature for 2 h for selenization treatment. After natural cooling, a Mo-CoSe2@C array was obtained.

[0065] Example 5

[0066] (1) 40 mL of an aqueous solution containing 0.5821 g of cobalt nitrate hexahydrate and 40 mL of an aqueous solution containing 1.3137 g of 2-methylimidazole were mixed and stirred for 10 minutes to obtain a mixed solution A;

[0067] (2) transferring the mixed solution A obtained in step (1) to a reactor and adding carbon cloth, standing at 25° C. for 4 hours, taking out the sample, washing it alternately with water and anhydrous ethanol three times, and drying it to obtain a precursor Co-MOF array;

[0068] (3) 0.2 g of sodium molybdate dihydrate was first dissolved in 20 mL of water, and then 80 mL of ethanol was added, and the mixture was stirred for 5 minutes to obtain a mixed solution B. Then, the precursor Co-MOF array was immersed in the mixed solution B and placed in a water bath at 95° C. for 12 minutes. After the water bath ended, the sample was washed alternately with water and anhydrous ethanol three times, and dried to obtain a double metal hydroxide Mo-Co LDH array;

[0069] (4) 40 μL of pyrrole, 0.384 g of sodium dodecylbenzene sulfonate (SDBS), and 0.0583 g of sodium chloride were dissolved in 100 mL of deionized water, and the mixture was stirred for 30 minutes to obtain a mixed solution C. The Mo-Co LDH array obtained in step (3) was immersed in solution C for electrodeposition by cyclic voltammetry with a voltage range of 0.2-0.7 V, a deposition cycle of 4 cycles, and a scan rate of 1.0 mVs -1 After the deposition, the Mo-Co LDH@PPy array was obtained by washing with water and anhydrous ethanol three times alternately and drying.

[0070] (5) Take 3.0 mg of selenium powder and the Mo-Co LDH@PPy in the above step (4) in a tube furnace, and under nitrogen protection, heat the temperature to 500°C at a heating rate of 2°C / min and keep it at this temperature for 2 hours for selenization treatment. After natural cooling, a Mo-CoSe2@C array is obtained.

[0071] Example 6

[0072] (1) 40 mL of an aqueous solution containing 0.5821 g of cobalt nitrate hexahydrate and 40 mL of an aqueous solution containing 1.3137 g of 2-methylimidazole were mixed and stirred for 10 minutes to obtain a mixed solution A;

[0073] (2) transferring the mixed solution A obtained in step (1) to a reactor and adding carbon cloth, standing at 25° C. for 4 hours, taking out the sample, washing it alternately with water and anhydrous ethanol three times, and drying it to obtain a precursor Co-MOF array;

[0074] (3) 0.2 g of sodium molybdate dihydrate was first dissolved in 20 mL of water, and then 80 mL of ethanol was added, and the mixture was stirred for 5 minutes to obtain a mixed solution B. Then, the precursor Co-MOF array was immersed in the mixed solution B and placed in a water bath at 85°C for 12 minutes. After the water bath ended, the sample was washed alternately with water and anhydrous ethanol three times, and dried to obtain a double metal hydroxide Mo-Co LDH array;

[0075] (4) 40 μL of pyrrole, 0.384 g of sodium dodecylbenzene sulfonate SDBS, and 0.0583 g of sodium chloride were dissolved in 100 mL of deionized water, and the mixture was stirred for 30 minutes to obtain a mixed solution C. The Mo-CoLDH array obtained in step (3) was immersed in solution C for electrodeposition by cyclic voltammetry with a voltage range of 0.2-0.7 V, a deposition cycle of 2 cycles, and a scan rate of 0.5 mVs -1 After the deposition, the Mo-CoLDH@PPy array was obtained by washing with water and anhydrous ethanol three times alternately and drying.

[0076] (5) Take 3.0 mg of selenium powder and the Mo-CoLDH@PPy in the above step (4) in a tube furnace, and under nitrogen protection, heat the temperature to 400°C at a heating rate of 2°C / min and keep it at this temperature for 2 hours for selenization treatment. After natural cooling, a Mo-CoSe2@C array is obtained.

[0077] Example 7

[0078] (1) 40 mL of an aqueous solution containing 0.5821 g of cobalt nitrate hexahydrate and 40 mL of an aqueous solution containing 1.3137 g of 2-methylimidazole were mixed and stirred for 10 minutes to obtain a mixed solution A;

[0079] (2) transferring the mixed solution A obtained in step (1) to a reactor and adding carbon cloth, standing at 25° C. for 4 hours, taking out the sample, washing it alternately with water and anhydrous ethanol three times, and drying it to obtain a precursor Co-MOF array;

[0080] (3) 0.2 g of sodium molybdate dihydrate was first dissolved in 20 mL of water, and then 80 mL of ethanol was added, and the mixture was stirred for 5 minutes to obtain a mixed solution B. Then, the precursor Co-MOF array was immersed in the mixed solution B and placed in a water bath at 85°C for 12 minutes. After the water bath ended, the sample was washed alternately with water and anhydrous ethanol three times, and dried to obtain a double metal hydroxide Mo-Co LDH array;

[0081] (4) 100 μL of pyrrole, 0.384 g of sodium dodecylbenzene sulfonate (SDBS), and 0.0583 g of sodium chloride were dissolved in 100 mL of deionized water, and the mixture was stirred for 30 minutes to obtain a mixed solution C. The Mo-Co LDH array obtained in step (3) was immersed in solution C for electrodeposition by cyclic voltammetry with a voltage range of 0.2-0.7 V, a deposition cycle of 6 cycles, and a scan rate of 2.0 mVs -1 After the deposition, the Mo-Co LDH@PPy array was obtained by washing with water and anhydrous ethanol three times alternately and drying.

[0082] (5) Take 3.0 mg of selenium powder and the Mo-Co LDH@PPy in the above step (4) in a tube furnace, and under nitrogen protection, heat the temperature to 400°C at a heating rate of 2°C / min and keep it at this temperature for 2 hours for selenization treatment. After natural cooling, a Mo-CoSe2@C array is obtained.

[0083] The molybdenum-doped cobalt diselenide composite material obtained in step (5) of the above embodiment is used as the negative electrode material of the sodium ion battery, the arrayed molybdenum-doped cobalt diselenide composite material is cut into 1cm*1cm square pieces and directly used as the working electrode, the sodium metal foil is used as the counter electrode and the reference electrode, and the glass fiber membrane is used as the diaphragm, and the electrolyte is 1M NaClO4 dissolved in a mixed solvent of ethylene carbonate and dimethyl carbonate (EC / DMC volume ratio is 1:1), and 5% by weight of fluoroethylene carbonate (FEC) is added as an additive. When assembling the battery, the negative electrode shell, electrode material, diaphragm, electrolyte, sodium foil, gasket, shrapnel and positive electrode shell are assembled from bottom to top, and the operation is completed in a glove box filled with argon.

[0084] After the assembled sodium-ion battery was placed for 12 hours, a constant current charge and discharge test was performed with a charge and discharge voltage of 3V-0.01V. The specific capacity, rate performance, and charge and discharge cycle performance of the sodium-ion battery negative electrode were measured in an environment of 25±1℃.

[0085] As the selenization temperature and the number of electrodeposition cycles change, the sodium ion battery exhibits different electrochemical properties. The maximum discharge capacity of the Mo-doped cobalt diselenide composite array material in Examples 1-7 at different current densities after being assembled into a sodium ion battery as a sodium ion electrode material is shown in Table 1:

[0086] Table 1

[0087]

[0088] As can be seen from the table, the water bath temperature, the heat treatment selenization temperature and the carbon coating process all have an impact on the performance of the Mo-doped cobalt diselenide composite material. When the water bath temperature and the selenization temperature are reduced (Examples 1 and 4), the material performance decreases accordingly, indicating that at a lower water bath temperature, the exchange rate of Mo ions decreases, resulting in insufficient exchange of Mo ions; at the same time, the diffusion is insufficient at a lower temperature, and the crystallinity of the composite material is low, thereby reducing the rate performance; however, too high a selenization temperature (Examples 1 and 5) will make the material flake thinner and brittle, resulting in severe pulverization of the electrode material during the cycle, reducing the overall performance of the electrode. Then, when studying the effect of carbon coating thickness on the battery, it was found that moderate carbon coating (Examples 1, 6, and 7) has an important influence on the improvement of performance. Because the carbon coating layer is too thin, the mitigation effect on the volume expansion of the material during the cycle is insufficient; the carbon coating layer is too thick, which will hinder the migration of sodium ions and reduce the rate performance.

[0089] Figure 6 The cycle performance diagram of the sodium ion battery in Example 1. It can be seen from the figure that the sodium ion battery has a current density of 0.5Ag -1The electrochemical performance was excellent, and after 200 cycles, it still maintained 672.5 mAh g -1 capacity. Figure 7 This is the rate diagram of sodium ion battery. Sodium ion battery at 0.2Ag -1 , 0.5Ag -1 , 1Ag -1 , 2Ag -1 , 5Ag -1 and returns 0.2A g -1 The capacities at current densities of 1203.8 mAh g -1 、754.1mAh g -1 , 522.5mAh g -1 、398.4mAhg -1 , 313.9mAh g -1 、1109.1mAh g -1 , showing excellent rate performance.

Claims

1. A method for preparing an arrayed molybdenum-doped cobalt diselenide composite material, characterized in that: The following steps are involved: (1) stirring and mixing a cobalt salt aqueous solution and a 2-methylimidazole aqueous solution to obtain a mixed solution A; The mixed solution A comprises the following components: Water 60-100 mL; Cobalt salt 1-3mmol; 2-Methylimidazole 8-24mmol; The cobalt salt is one of cobalt nitrate, cobalt chloride and cobalt sulfate; (2) transferring the mixed solution A obtained in step (1) to a reactor and adding a flexible substrate, allowing the flexible substrate to react, removing, washing, and drying the flexible substrate to obtain a precursor Co-MOF array; (3) dissolving sodium molybdate in water, then adding ethanol, mixing and stirring, and obtaining a mixed solution B, immersing the precursor Co-MOF array in the mixed solution B for a water bath, and after the water bath is completed, washing and drying to obtain a double metal hydroxide Mo-Co LDH array; (4) dissolving pyrrole, sodium dodecylbenzene sulfonate, and sodium chloride in deionized water successively, stirring and mixing, to obtain a mixed solution C, immersing the Mo-Co LDH array obtained in step (3) in the mixed solution C for electroplating and coating polypyrrole, and after the deposition, washing and drying the Mo-Co LDH array to obtain a Mo-Co LDH@PPy array; (5) taking the selenium powder and the Mo-Co LDH@PPy array obtained in step (4) into a tube furnace, heat-treating them under a protective gas, and cooling them to obtain an arrayed molybdenum-doped cobalt diselenide composite material.

2. The preparation method according to claim 1, characterized in that: In step (2), the temperature for the standing reaction is 10-60° C., and the standing reaction time is 3-5 hours.

3. The preparation method according to claim 1, characterized in that: In step (3), the ratio of water and ethanol to sodium molybdate is 100mL:0.1-1.0g, wherein the volume ratio of water to ethanol in water and ethanol is 1:3-5.

4. The preparation method according to claim 1, characterized in that: In step (3), the water bath temperature is 70-95°C and the time is 10-20 minutes.

5. The preparation method according to claim 1, characterized in that: In step (4), the mixed solution C comprises the following components:

6. The preparation method according to claim 1, characterized in that: In step (5), the protective gas is nitrogen or argon, the heat treatment temperature is 300-500° C., and the heat treatment holding time is 1-3 hours.

7. The arrayed molybdenum-doped cobalt diselenide composite material prepared by the preparation method according to any one of claims 1 to 6, characterized in that: It is a flake structure.

8. Use of the arrayed molybdenum-doped cobalt diselenide composite material according to claim 7 as a negative electrode material for sodium ion batteries.