A method and device for improving the curvature of the extruded tire sidewall

By setting the opening ratio and chamfering of the lip profile plate, the sidewall rubber material is discharged at a consistent speed, and the online roller pressing device is used to press the sidewall wear-resistant rubber, which solves the sidewall bending problem and improves production efficiency and Finished product quality.

CN115257028BActive Publication Date: 2024-10-15SAILUN GRP CO LTD +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202210918280.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-01
Publication Date
2024-10-15
Estimated Expiration
2042-08-01

AI Technical Summary

Technical Problem

In the tire rubber industry, the combination of sidewall rubber and wear-resistant rubber causes the sidewall to easily bend during the production process, affecting production efficiency and finished product quality.

Method used

By setting the opening ratio of the mouth plate and developing chamfers, the rubber dispensing speeds of the two rubber materials on the sidewall are differentiated, and the sidewall wear-resistant rubber is pressed together with an online roller pressing device to improve the sidewall bending problem.

Benefits of technology

It effectively reduces the amount of sidewall bending, improves production efficiency, reduces production costs, and improves the average dynamic performance of the finished tire.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115257028B_ABST
    Figure CN115257028B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of tire rubber component production and manufacturing, and relates to a method and device for improving the bending of the extruded sidewall, and the method specifically includes the following steps: (1) measuring the bending of the wear-resistant rubber of each specification of the sidewall; (2) correlating the wear-resistant rubber bending value of each specification of the sidewall with the die plate opening rate, and setting the die plate opening rate; (3) setting a chamfer at the wear-resistant rubber part of the die plate, the width of the chamfer corresponds to the width of the die plate, the height of the chamfer is set according to the opening height of the wear-resistant rubber part, and the depth of the chamfer is three quarters of the thickness of the die plate; (4) extruding two sidewalls through the die plate, and conveying them to an online rolling device for rolling. The method improves the bending of the wear-resistant rubber of the sidewall by setting the die plate opening rate and developing the chamfer of the die plate, and at the same time combines the online rolling device of the wear-resistant rubber part of the sidewall, solves the problem of bending and deformation of the sidewall after winding and parking, improves the production efficiency and molding production efficiency of the sidewall, and reduces the production cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of tire rubber component production and manufacturing, and in particular relates to a method and a device for improving the bending of an extruded tire sidewall. Background Art

[0002] At present, in the tire rubber industry, the sidewall structure of semi-steel tires is mostly composed of two parts: sidewall rubber and wear-resistant rubber. The sidewall rubber and wear-resistant rubber are two rubber materials with different formulas. The two rubber materials have great differences in physical properties such as elongation, hardness, and Mooney. During the production and processing of the sidewall, the combination of the sidewall rubber and the wear-resistant rubber is affected by factors such as the opening rate of the extrusion outlet mold plate, the difference in rubber performance, and the shape of the sidewall structure. The sidewall will bend after being extruded, coiled and parked by the extrusion equipment, and it is mostly bent in the direction of the wear-resistant rubber.

[0003] The production of defective sidewall bending not only affects production efficiency and increases production costs, but also causes problems such as skewed sidewall fitting and misaligned joints when the bent sidewall is used in the molding process. The use of bent sidewalls can easily cause the finished tire to have lower movement and taper performance, seriously affecting production efficiency and tire quality. Summary of the invention

[0004] The purpose of the present invention is to solve the problem of sidewall bending in the prior art, and a method and device for improving the bending of the extruded sidewall is proposed. The method sets the opening rate of the die plate and develops the chamfer of the die plate, so that the discharging speed of the two rubbers of the sidewall and the wear-resistant rubber is different, and the bending amount of the sidewall is reduced. At the same time, the wear-resistant rubber part of the sidewall is pressed by an online roller pressing device, thereby improving or solving the bending of the wear-resistant rubber of the sidewall and the bending deformation of the sidewall after winding and parking. Solving the problem of sidewall bending can greatly improve the production efficiency and molding production efficiency of the sidewall, reduce production costs, and improve the performance of the finished tire.

[0005] The technical solution of the present invention is:

[0006] A method for improving the curvature of a tire sidewall, the method comprising: setting the opening ratio of a die plate and developing a chamfer, and performing rolling in combination with an online rolling device; the method specifically comprises the following steps:

[0007] (1) Measure the curvature of the sidewall wear-resistant rubber of each specification and record the measurement data; measure and record the width of the sidewall rubber and the wear-resistant rubber;

[0008] (2) Correlate the die plate opening ratio with the wear-resistant rubber bending value of each specification of the tire sidewall measured, and set the die plate opening ratio;

[0009] (3) A chamfer is set at the wear-resistant rubber part of the die plate, the width of the chamfer corresponds to the width of the die plate, the height of the chamfer is set according to the opening height of the wear-resistant rubber part, and the depth of the chamfer is three quarters of the thickness of the die plate;

[0010] (4) The double sidewalls are extruded through the die plate and transported to the online rolling device for rolling.

[0011] Furthermore, in the step (1), after the sidewall is extruded normally, the left and right sidewalls are cut and sampled, and the sampling length is greater than 1m; the cut sidewall samples are shaken to shrink them as quickly as possible to reach a curved state, and when the curvature no longer changes, the curvature value of the highest point of the sidewall curvature is measured and recorded; the wear-resistant rubber bending value of the sidewalls of various specifications is measured according to the above operation, and they are classified according to the bending value and the ratio of the wear-resistant rubber to the sidewall rubber width to form a preliminary corresponding relationship, so as to prepare for the next step of setting the opening rate of the die plate.

[0012] Furthermore, in the step (2), the sidewall is classified according to the sidewall rubber and the wear-resistant rubber width according to the bending value of the sidewall wear-resistant rubber, a preliminary corresponding relationship is formed, and the ratio of the sidewall rubber width to the wear-resistant rubber width is calculated; the linear relationship between the bending value of the sidewall wear-resistant rubber of each specification and the opening rate of the die plate is y=-0.114x+1.0504, wherein y is the opening rate of the die plate at the wear-resistant rubber part, and x is the ratio of the sidewall rubber width to the wear-resistant rubber width.

[0013] Furthermore, in the step (3), the spacing between different thickness measurement points of the wear-resistant rubber portion of the die plate is set as the sub-width according to the differences in width and thickness of the sidewall wear-resistant rubber of each specification; chamfers are set at corresponding sub-width positions on the upper or lower plate of the die plate whose opening rate has been set, and the width of each chamfer is consistent with the sub-width.

[0014] Furthermore, three sub-widths are set at the wear-resistant rubber part of the die plate, including the first sub-width, the second sub-width and the third sub-width. The height value of the first chamfer set at the first sub-width position is 2 to 3 times the maximum opening height of the die plate at that position; the height values ​​of the second chamfer and the third chamfer set at the second sub-width and the third sub-width positions are both 1 times the corresponding opening height of the die plate.

[0015] Furthermore, the depth of the chamfer at each width position is three quarters of the thickness of the die plate.

[0016] The present invention also protects an online rolling device for improving the bending of the extruded tire side, comprising a device frame and a fixed rod installed above the device frame, a left cylinder and a right cylinder are symmetrically installed at both ends of the fixed rod, the left cylinder is connected to the left pressure roller angle adjustment bolt and the left pressure roller in sequence, and the right cylinder is connected to the right pressure roller angle adjustment bolt and the right pressure roller in sequence; a left screw and a right screw are arranged between the device frames, and a left screw rotating handle for adjusting the rotation of the left screw and a right screw rotating handle for adjusting the rotation of the right screw are installed on one side of the device frame; a digital air pressure valve for setting and displaying the air pressure value is also installed on the device frame.

[0017] Furthermore, the online rolling device is installed on a linkage line conveying roller, and the linkage line conveying roller is composed of a plurality of rollers, and the distance between every two rollers is 45 mm.

[0018] Furthermore, the steps of rolling the tire sidewalls by the online rolling device to improve the sidewall curvature are as follows:

[0019] S1. The tapers of the left and right pressure rollers are adjusted respectively by the left and right pressure roller angle adjustment bolts. After the double sidewalls are extruded through the die plate, they are conveyed to the bottom of the online roller pressing device. The left and right screw rotating handles are rotated to adjust the left and right screws, so that the left and right pressure rollers with a certain taper on the left and right sides are located above the wear-resistant rubber part of the sidewalls.

[0020] S2. Open the air pressure valve switch, the left cylinder and the right cylinder extend, push the left pressure roller and the right pressure roller down to the middle of the two rollers, press the pressure rollers onto the left and right tire sides being transported, support the tire sides being transported with the two rollers, and roll the wear-resistant rubber parts of the left and right tire sides with the left pressure roller and the right pressure roller respectively, so that the wear-resistant rubber parts after rolling appear in an extended state;

[0021] S3. According to the rolling conditions of the left and right pressure rollers on the wear-resistant rubber part, the air pressure value of the digital air pressure valve is adjusted to control the rolling effect of the pressure rollers on the sidewall wear-resistant rubber;

[0022] S4. When the tire sidewall production is finished, the air pressure valve is closed, the left and right cylinders are raised, and the rolling of the wear-resistant rubber part is finished.

[0023] Beneficial effects of the present invention:

[0024] (1) The method for improving the curvature of the extruded tire sidewall provided by the present invention relates to the die plate opening rate by associating the curvature of the tire sidewall, and develops a suitable die plate opening rate and die plate chamfer, so that the two rubber materials on the tire sidewall can achieve basically the same stretching and shrinkage after extrusion, so as to reduce the curvature of the tire sidewall. At the same time, the tire sidewall is rolled by an online rolling device, which can effectively improve the curvature of the extruded tire sidewall, reduce the return rate of defective products, effectively improve the production efficiency and the quality of the finished tire, and reduce the production cost.

[0025] (2) The online rolling device provided by the present invention is simple and convenient to operate, and the rolling pressure can be adjusted and set according to different specifications of sidewalls. The wear-resistant rubber part of the sidewall is rolled by the pressure roller of the rolling device, so that the wear-resistant rubber of the sidewall reaches an extended state (wave shape); after the wear-resistant rubber in the extended state and the sidewall rubber are transported, wound and parked through the linkage line, the contraction of the sidewall rubber and the wear-resistant rubber can be consistent, thereby solving the problem of the sidewall bending toward the wear-resistant rubber side and the bending and deformation of the sidewall after winding and parking. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 A schematic diagram of measuring the sidewall and the curvature of the sidewall provided by the present invention;

[0027] Figure 2 A schematic diagram of the structure of the sidewall mouth plate provided by the present invention;

[0028] Figure 3 The linear relationship between the bending value of the wear-resistant rubber of the sidewall of each specification provided by the present invention and the opening ratio of the wear-resistant rubber of the die plate;

[0029] Figure 4 A front view schematic diagram of the wear-resistant rubber portion of the sidewall of the die plate provided by the present invention;

[0030] Figure 5 A schematic diagram of the chamfering of the wear-resistant rubber portion of the sidewall of the die plate provided by the present invention;

[0031] Figure 6 A schematic diagram of the chamfer dimensions of the wear-resistant rubber portion of the die plate provided by the present invention;

[0032] Figure 7 A front schematic diagram of an online rolling device provided by the present invention;

[0033] Figure 8 A side schematic diagram of the online roller pressing device (installed on the conveying roller table of the linkage line) provided by the present invention;

[0034] In the above figures, 1. device frame; 2. digital display air pressure valve; 3. left screw rotation handle; 4. right screw rotation handle; 5. left screw; 6. right screw; 7. fixing rod; 8. left cylinder; 9. right cylinder; 10. left pressure roller; 11. right pressure roller; 12. left pressure roller angle adjustment bolt; 13. right pressure roller angle adjustment bolt; 14. linkage line conveyor roller; 15. roller. DETAILED DESCRIPTION

[0035] In order to further understand the present invention, the technical solution of the present invention is clearly and completely described below in conjunction with the accompanying drawings and embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] This embodiment provides a method for improving the curvature of the pressed tire sidewall, which is implemented by the following steps:

[0037] (1) Measure the curvature of the sidewall wear-resistant rubber of each specification and record the data;

[0038] (ii) Correlate the die plate opening ratio with the curvature of the sidewall wear-resistant rubber to determine the appropriate die plate opening ratio;

[0039] (iii) Chamfering is performed according to the sidewall pre-die shape, die plate shape and size so that the two rubber materials on the sidewall shrink in the same manner after extrusion or parking;

[0040] (iv) Rolling the sidewall wear-resistant rubber by an online rolling device.

[0041] The above method develops the die plate opening rate and die plate chamfer, which makes the glue output speed of the two rubbers on the sidewall different, so that the two rubbers on the sidewall can achieve basically the same stretching and shrinkage after extrusion, so as to reduce the sidewall bending. At the same time, the sidewall wear-resistant rubber is rolled by an online rolling device, which can greatly improve the sidewall wear-resistant rubber bending and even completely solve the sidewall bending problem.

[0042] Specifically, the implementation process of the four steps in the above method is:

[0043] (I) Measurement of the curvature of the sidewall wear-resistant rubber of various specifications:

[0044] 1. After the tire sidewall is extruded normally, it is transported from the linkage line to the winding station, and the left and right tire sidewalls are cut and sampled respectively, and the sampling length is greater than 1m;

[0045] 2. Place the two cut sidewalls flat on the platform and shake them manually to shrink them as quickly as possible to reach a curved state;

[0046] 3. When the curvature of the tire sidewall no longer changes, use a tape measure or ruler to measure the highest point of the curvature of the tire sidewall at a length of 1m. Figure 1 As shown, record the bending height value;

[0047] 4. Measure and record the bending value of the sidewall wear-resistant rubber of each specification, classify them according to the bending value and the width ratio of the wear-resistant rubber to the sidewall rubber, and form a preliminary corresponding relationship to set the opening rate of the die plate.

[0048] (II) Method and steps for correlating the sidewall wear-resistant rubber bending value with the die plate opening rate:

[0049] During the die plate opening process, it is very important to define the opening width of the die plate. The suitability of the die plate opening rate needs to take into account the structure of the component and the physical properties of the rubber. The size of the die plate opening rate directly affects the shrinkage and dimensional stability of the component.

[0050] Due to the large differences in the physical properties of the sidewall rubber and the wear-resistant rubber (the sidewall rubber is soft and shrinks more at the same length; the wear-resistant rubber is hard and shrinks less at the same length) and structure, if you want the two rubbers to shrink the same amount on the linkage line (after winding and parking), you need to make the glue output speed of the two rubbers different within a certain period of time, that is, the glue output speed of the wear-resistant rubber should be greater than that of the sidewall rubber, and the wear-resistant rubber is slightly extended (wavy) after being extruded from the die plate. To achieve the extended state of the extruded wear-resistant rubber, the opening of the die plate wear-resistant rubber needs to be reduced, so the die plate opening rate needs to be set in combination with the structural width of the two rubbers and the curvature of the wear-resistant rubber.

[0051] The structure of the sidewall plate is as follows: Figure 2 shown.

[0052] The bending value of the sidewall wear-resistant rubber is closely related to the sidewall structure, and the width of the wear-resistant rubber directly affects the bending value. Therefore, it is classified according to the bending value of the sidewall wear-resistant rubber and the ratio of the wear-resistant rubber to the sidewall rubber width, see Table 1 below; the ratio of the sidewall rubber to the wear-resistant rubber width is calculated, see Table 1 below.

[0053] Table 1 Corresponding relationship between the width ratio of sidewall rubber to wear-resistant rubber and the opening ratio of the die plate at the wear-resistant rubber part

[0054]

[0055] According to the physical properties of the wear-resistant rubber, the opening rate of the die plate at the wear-resistant rubber part should be controlled within the range of 65% to 105%. If the opening rate is set beyond this range, it is difficult to obtain a qualified size. Therefore, according to the ratio of the wear-resistant rubber width to the sidewall rubber width, a suitable opening rate is found within a certain range for trial production; the opening rate of the die plate at the sidewall part is opened at 100%; the sidewalls with different wear-resistant rubber widths and sidewall rubber widths in the above table are respectively set according to the proportion of the opening rate to open and debug the die plate. After the die plate is adjusted, the wear-resistant rubber part of the sidewall can appear slightly wavy, which is the appropriate die plate opening rate.

[0056] The linear relationship between the bending value of the sidewall wear-resistant rubber of each specification and the opening rate of the die plate wear-resistant rubber is as follows: Figure 3 As shown, the Y axis is the opening rate of the die plate at the wear-resistant rubber part, and the X axis is the ratio of the sidewall rubber to the wear-resistant rubber width. For each specification of sidewall, the linear relationship formula obtained by the above method can be substituted into the calculation to obtain the appropriate opening rate of the die plate at the wear-resistant rubber part.

[0057] (III) Development of chamfering of die plate:

[0058] After associating the bending value of the wear-resistant rubber with the opening rate of the die plate according to the above step (ii), the actual opening width and thickness of the die plate at the wear-resistant rubber part are much smaller than the standard value. Therefore, if the wear-resistant rubber extrusion size is to reach the standard value, the die plate needs to be chamfered.

[0059] The chamfer is located at the sidewall wear-resistant rubber part. By developing and adjusting the chamfer of the die plate, the width and thickness of the wear-resistant rubber after extrusion meet the standard requirements. Depending on the machine model, the chamfer is developed at the wear-resistant rubber part on the upper or lower die plate.

[0060] The width is set at the wear-resistant rubber position of the die plate. The width and thickness of the wear-resistant rubber of each specification of the sidewall are different, so the distance between different thickness measurement points is called the width. Figure 4 and Figure 5 As shown, three widths are provided at the wear-resistant rubber portion of the die plate, including width 1, width 2 and width 3, and the chamfer width of the wear-resistant rubber of the die plate corresponds to the width of the die plate (there are differences in the width of the wear-resistant rubber of the sidewalls of different specifications).

[0061] like Figure 6 As shown, the height value of chamfer h1 can be 2 to 3 times the maximum opening height of the die plate at the wear-resistant rubber part, and the height of chamfer h2 and h3 of each width section can be 1 times the opening height of the corresponding die plate; the chamfer depth of each width section can be three-quarters of the die plate thickness k. The chamfer height and depth of each width section can be adjusted according to different specifications.

[0062] (IV) Online roller pressing device improves the bending of the sidewall wear-resistant rubber:

[0063] like Figure 7 and Figure 8 As shown, the online rolling device is a rolling device added to the existing linkage line conveying roller 14. The online rolling device is simple and convenient to operate and can adjust and set the rolling pressure for different specifications of the sidewall. The rolling device rolls the sidewall (wear-resistant rubber side) during transportation with a cylinder lifting and lowering roller to make the wear-resistant rubber part of the sidewall reach an extended state. The wear-resistant rubber in the extended state and the sidewall rubber can shrink in the same way after being conveyed by the linkage line and rolled up and parked, solving the problem of the sidewall bending toward the wear-resistant rubber side.

[0064] 1. Online sidewall rolling device:

[0065] The online rolling device is installed on the linkage line conveying roller 14, which is an extrusion linkage production line for conveying the tire side; the linkage line conveying roller 14 is composed of multiple rollers 15, which form a conveying track driven by a chain, and the distance between every two rollers 15 is 45mm.

[0066] The online rolling device includes a device frame 1 and a fixed rod 7 installed above the device frame 1. The device frame 1 is fixed on the linkage line conveyor roller 14. The fixed rod 7 is used to fix the cylinder and the pressure roller. The left cylinder 8 and the right cylinder 9 are symmetrically installed at both ends of the fixed rod 7.

[0067] The left cylinder 8 is used to raise and lower the left pressure roller 10. The left cylinder 8 is connected to the left pressure roller angle adjustment bolt 12 and the left pressure roller 10 in sequence. The left pressure roller angle adjustment bolt 12 is used to adjust the angle of the left pressure roller 10. Two left pressure rollers 10 are arranged on one side to roll the wear-resistant rubber part of the tire side. The number of pressure rollers can be increased according to actual conditions to perform multi-roller rolling.

[0068] The right cylinder 9 is used to raise and lower the right pressure roller 11. The right cylinder 9 is connected to the right pressure roller angle adjustment bolt 13 and the right pressure roller 11 in sequence. The right pressure roller angle adjustment bolt 13 is used to adjust the angle of the right pressure roller 11. Similarly, two right pressure rollers 11 are arranged on one side to roll the wear-resistant rubber part of the tire side. The number of pressure rollers can be increased according to actual conditions to perform multi-roller rolling.

[0069] A left screw 5 and a right screw 6 are provided between the device frame 1. The left screw 5 is used to adjust the position of the left pressure roller 10, and the right screw 6 is used to adjust the position of the right pressure roller 11. A left screw rotating handle 3 for adjusting the rotation of the left screw 5 and a right screw rotating handle 4 for adjusting the rotation of the right screw 6 are installed on one side of the device frame 1. The left and right screw rotating handles move the pressure rollers by adjusting the left and right screws. A digital air pressure valve 2 for setting and displaying the air pressure value is also installed on the device frame 1. The appropriate air pressure value can be formulated according to the tire side specifications to form parameter solidification.

[0070] 2. The specific steps of improving the sidewall curvature by online roller pressing device are as follows:

[0071] S1. The tapers of the left pressure roller 10 and the right pressure roller 11 are adjusted respectively by the left pressure roller angle adjustment bolt 12 and the right pressure roller angle adjustment bolt 13 (wherein, the taper of the pressure rollers of the left and right pressure rollers can be 10°-15°, the taper length is set according to the width of the sidewall wear-resistant rubber, which can be 40-70 mm, preferably 60 mm, and the major diameter is set according to the roller spacing size, which can be 20-40 mm, preferably 32 mm); after the double sidewalls are extruded through the die plate, they are transported to the online rolling device by the linkage line conveying roller 14, and the left screw rotating handle 3 and the right screw rotating handle 4 are rotated to make the left pressure roller 10 and the right pressure roller 11 with a certain taper on the left and right sides be located above the sidewall wear-resistant rubber part;

[0072] S2, open the air pressure valve switch, the left cylinder 8 and the right cylinder 9 extend, push the left pressure roller 10 and the right pressure roller 11 to fall; the left pressure roller 10 and the right pressure roller 11 fall to the middle position of the two rollers 15, and the pressure rollers press on the left and right sidewalls being transported, and the two rollers 15 support the sidewalls being transported, and the left pressure roller 10 and the right pressure roller 11 respectively roll the wear-resistant rubber parts of the left and right sidewalls, so that the wear-resistant rubber parts after rolling appear in an extended state (wavy shape);

[0073] S3, according to the rolling conditions of the left pressure roller 10 and the right pressure roller 11 on the wear-resistant rubber part, the air pressure value of the digital air pressure valve 2 can be adjusted to control the rolling effect of the pressure roller on the sidewall wear-resistant rubber;

[0074] S4, the tire sidewall production is finished, the air pressure valve is closed, the left cylinder 8 and the right cylinder 9 are raised, and the rolling of the wear-resistant rubber part is finished.

[0075] The above-mentioned sidewall online rolling device is a device with two lifting and lowering rollers (two rollers on each side and the number of rollers can be increased according to the situation). The roller of the device falls to the wear-resistant rubber part of the sidewall between the two rollers of the conveying roller, and the wear-resistant rubber is rolled by the roller, so that the wear-resistant rubber appears in an extended state (wave shape). After the sidewall is rolled by the roller, it is conveyed on the auxiliary line, rolled up and parked, and the sidewall rubber and the wear-resistant rubber shrink in unison, solving the problem of bending deformation of the sidewall after rolling up and parking.

[0076] Through the above-mentioned die plate opening rate setting, die plate chamfer development and the coordinated use of the online rolling device, the problem of the sidewall bending toward the wear-resistant rubber has been completely solved, as shown in Table 2 below, which is the data of some specifications of the sidewall corresponding to the improved front and rear bending values.

[0077] Table 2 Improved front and rear camber values ​​corresponding to some specifications of sidewall data

[0078] Sidewall specifications Improved front sidewall curvature (mm) Improved bending value (mm) BZ3290 10±2 0 BZ7871 15±2 2 BZ6360 20±2 0 BZ0092 25±2 0 BZ6720 30±2 2 BZ7981 35±2 3 BZ3256 40±2 0 BZ1807 45±2 0 BZ7751 50±2 0

[0079] The above description is only a preferred embodiment of the present invention, and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art can still modify the technical solutions described in the above embodiments, or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, modification, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for improving the curvature of a pressed tire sidewall, characterized in that: The method includes setting the opening ratio of the die plate and developing the chamfer, and simultaneously performing rolling in combination with an online rolling device; specifically, the following steps are included: (1) Measure the curvature of the sidewall wear-resistant rubber of each specification and record the measurement data; measure and record the width of the sidewall rubber and the wear-resistant rubber; In the step (1), after the sidewall is extruded in normal production, the left and right sidewalls are cut and sampled respectively, and the sampling length is greater than 1m; the cut sidewall samples are shaken to shrink them as quickly as possible to reach a curved state, and when the curvature no longer changes, the curvature value of the highest point of the sidewall curvature is measured and recorded; the curvature value of the wear-resistant rubber of each specification of the sidewall is measured according to the above operation, and the wear-resistant rubber is classified according to the curvature value and the ratio of the wear-resistant rubber to the sidewall rubber width to form a preliminary corresponding relationship; (2) Correlate the die plate opening ratio with the wear-resistant rubber bending value of each specification of the tire sidewall measured, and set the die plate opening ratio; In the step (2), according to the bending value of the sidewall wear-resistant rubber, the sidewall is classified according to the sidewall rubber and the wear-resistant rubber width to form a preliminary corresponding relationship, and the ratio of the sidewall rubber width to the wear-resistant rubber width is calculated; the linear relationship between the bending value of the sidewall wear-resistant rubber of each specification and the die plate opening rate is y=-0.114x+1.0504, wherein y is the die plate opening rate of the wear-resistant rubber part, and x is the ratio of the sidewall rubber width to the wear-resistant rubber width; (3) A chamfer is set at the wear-resistant rubber part of the die plate, the width of the chamfer corresponds to the width of the die plate, the height of the chamfer is set according to the opening height of the wear-resistant rubber part, and the depth of the chamfer is three quarters of the thickness of the die plate; (4) The double sidewalls are extruded through the die plate and transported to the online rolling device for rolling.

2. The method according to claim 1, characterized in that In the step (3), according to the differences in width and thickness of the sidewall wear-resistant rubber of each specification, the spacing between different thickness measurement points of the wear-resistant rubber part of the die plate is set as the sub-width; chamfers are set at corresponding sub-width positions of the upper plate or the lower plate of the die plate whose opening rate has been set, and the width of each chamfer is consistent with the sub-width.

3. The method according to claim 2, characterized in that Three sub-widths are set at the wear-resistant rubber part of the die plate, including the first sub-width, the second sub-width and the third sub-width. The height value of the first chamfer set at the first sub-width position is 2 to 3 times the maximum opening height of the die plate at that position; the height values ​​of the second chamfer and the third chamfer set at the second sub-width and the third sub-width positions are both 1 times the corresponding opening height of the die plate.

4. The method according to claim 2, characterized in that: The depth of the chamfer at each width position is three quarters of the thickness of the die plate.

5. The method according to claim 1, characterized in that The online rolling device includes a device frame and a fixed rod installed above the device frame, and a left cylinder and a right cylinder are symmetrically installed at both ends of the fixed rod. The left cylinder is connected to the left pressure roller angle adjustment bolt and the left pressure roller in sequence, and the right cylinder is connected to the right pressure roller angle adjustment bolt and the right pressure roller in sequence; a left screw and a right screw are arranged between the device frames, and a left screw rotating handle for adjusting the rotation of the left screw and a right screw rotating handle for adjusting the rotation of the right screw are installed on one side of the device frame; a digital display air pressure valve for setting and displaying the air pressure value is also installed on the device frame.

6. The method according to claim 5, characterized in that The online rolling device is installed on a linkage line conveying roller, and the linkage line conveying roller is composed of a plurality of rollers, and the distance between every two rollers is 45 mm.

7. The method according to claim 6, characterized in that The steps of rolling the tire side and improving the side curvature of the tire by the online rolling device are as follows: S1. The tapers of the left and right pressure rollers are adjusted respectively by the left and right pressure roller angle adjustment bolts. After the double sidewalls are extruded through the die plate, they are conveyed to the bottom of the online roller pressing device. The left and right screw rotating handles are rotated to adjust the left and right screws, so that the left and right pressure rollers with a certain taper on the left and right sides are located above the wear-resistant rubber part of the sidewalls. S2. Open the air pressure valve switch, the left cylinder and the right cylinder extend, push the left pressure roller and the right pressure roller down to the middle of the two rollers, press the pressure rollers onto the left and right tire sides being transported, support the tire sides being transported with the two rollers, and roll the wear-resistant rubber parts of the left and right tire sides with the left pressure roller and the right pressure roller respectively, so that the wear-resistant rubber parts after rolling appear in an extended state; S3. According to the rolling conditions of the left and right pressure rollers on the wear-resistant rubber part, the air pressure value of the digital air pressure valve is adjusted to control the rolling effect of the pressure rollers on the sidewall wear-resistant rubber; S4. When the tire sidewall production is finished, the air pressure valve is closed, the left and right cylinders are raised, and the rolling of the wear-resistant rubber part is finished.

Citation Information

Patent Citations

  • Design method for development size of novel extruded die plate

    CN110228151A

  • Method for establishing plate opening standard of tread extrusion die plate

    CN112231843A

  • Design method, application of sizing material extrusion die plate, and equipment and computer program product

    CN113919061A

  • White sidewall extrusion pre-die structure

    CN213137733U

  • Device and method for molding rubber strip material for tire production and method for producing tire

    JP2005238799A