[0003]铅的冶炼方法有火法和湿法两种,目前以火法为主,随着铅行业的不断发展,铅原料消耗越来越大,那么导致铅渣的堆积量也越来越多,铅金属属于危险废物,直接排放会危害人类身体健康,污染大自然
[0017] 1. This invention uses low-cost lead slag to remove arsenic. The raw materials are simple and easy to obtain, the process flow is simple, and the operation is convenient. The metal waste slag is reused to save resources;
Smart Images

Figure CN115259338B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of heavy metal pollution control, and specifically relates to a chloride-modified lead slag synergistic with SiO 2 Methods for removing arsenic. Background Art
[0002] Lead slag is the slag produced in the process of lead smelting. Lead itself is also a heavy metal, so the recycling of lead has become the focus of environmental protection. Lead leaching slag is composed of Pb, S, Si, O and other elements. The main components are lead and silicon oxides, accounting for 68.44% of the total slag, as well as 9.84% of CaO and 1.46% of ZnO oxide.
[0003] There are two methods for smelting lead: pyrometallurgy and hydrometallurgy. Currently, pyrometallurgy is the main method. With the continuous development of the lead industry, the consumption of lead raw materials is increasing, which leads to an increasing amount of lead slag accumulation. Lead metal is a hazardous waste, and direct discharge will harm human health and pollute nature. Therefore, there is a need for a method to reuse lead slag and remove arsenic from polluted acid. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a chloride-modified lead slag synergistic with SiO 2 The method for removing arsenic uses low-cost lead slag to remove arsenic, which not only reduces the discharge of sludge in the process of waste acid treatment, but also removes heavy metal Pb in the process of removing As, thus achieving the purpose of secondary resource utilization by treating waste with waste.
[0005] In order to achieve the technical effect of solving the above technical problems, the present invention is realized by the following technical scheme: a chloride-modified lead slag is synergistic with SiO 2 The method for removing arsenic is characterized in that it specifically comprises the following steps:
[0006] S1, sieving the lead slag to a particle size of 100-200 mesh to obtain lead leaching slag powder;
[0007] S2, dissolving NaCl particles in deionized water and mixing evenly;
[0008] S3, H 2 O 2 Add to the dirty acid and mix evenly;
[0009] S4, lead slag powder and HNO 3 The solution is added to step S3 to obtain a mixed solution A;
[0010] S5, adding the solution obtained in step S2 to step S4 and mixing evenly to obtain a mixed solution B;
[0011] S6. Using NaOH, adjust the pH of the mixed solution B to 9.7-10, shake and react at room temperature for 24 hours, and separate the solid and liquid to obtain the arsenic-containing solid and the filtrate;
[0012] Furthermore, in step S2, the mass ratio of NaCl particles to lead slag g:g is 1:2.5, and the solid-liquid ratio of NaCl particles to deionized water g:mL is 0.04:1;
[0013] Furthermore, the arsenic content of the waste acid in step S3 is 1340.0-2800.0 mg / L, H 2 O 2 The molar ratio of arsenic to arsenic in polluted acid is (1.1-1.2):1;
[0014] Furthermore, in step S4, the solid-liquid ratio of the lead slag to nitric acid is (0.27-0.4):1, and the solid-liquid ratio of the lead slag to the dirty acid is (0.02-0.03):1.
[0015] Furthermore, the oscillation rate of step S6 is 180-200 r / min;
[0016] The beneficial effects of the present invention are:
[0017] 1. The present invention utilizes low-cost lead slag to remove arsenic, the raw materials are simple and easy to obtain, the process flow is simple, the operation is convenient, the metal waste slag is reused, and resources are saved;
[0018] 2. The present invention utilizes Pb 2+ with AsO 4 3- , Cl - Combined to form less soluble Pb 5 (AsO 4 ) 3 Cl, and Pb-As-Cl coprecipitation and SiO in lead slag 2 The formed silica gel can better fix arsenic, promote the stability of As to achieve the purpose of arsenic removal, and improve the efficiency and quality of arsenic removal;
[0019] 3. Aiming at the problem of waste acid discharge from factories, the present invention provides a method for removing arsenic from lead slag. The present invention utilizes low-cost lead slag to remove arsenic, which not only reduces the discharge of sludge during the waste acid treatment process, but also removes heavy metal Pb in the process of removing As, thereby achieving the purpose of secondary resource utilization by treating waste with waste. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0021] Figure 1 Schematic diagram of arsenic-containing contaminated acid according to an embodiment of the present invention;
[0022] Figure 2 The filtrate after arsenic removal according to the embodiment of the present invention;
[0023] Figure 3 Lead slag according to an embodiment of the present invention;
[0024] Figure 4 The NaCl solid particles according to an embodiment of the present invention;
[0025] Figure 5 This is the solid arsenic slag according to an embodiment of the present invention. DETAILED DESCRIPTION
[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] Example 1
[0028] The lead slag in this example was taken from a smelting plant in the southwest, and its main components are shown in Table 1; the arsenic-containing waste acid was taken from the sulfuric acid workshop of a copper smelter in the southwest, and its main components are shown in Table 2;
[0029] Table 1 Lead slag composition
[0030]
[0031] Table 2 Composition of polluted acid
[0032]
[0033] In this embodiment, a chloride-modified lead slag is used in conjunction with SiO 2 The method for removing arsenic, the specific steps are as follows:
[0034] (1) Sieving the lead slag to a particle size of 100 to 200 mesh to obtain lead leaching slag powder,
[0035] (2) Dissolve NaCl particles in deionized water and mix well to obtain a mixed solution A.
[0036] (3) H 2 O 2 Add to 200 mL of waste acid and mix evenly to obtain mixed solution B.
[0037] (4) The lead slag and HNO 3 The solution was added to the mixed solution B to obtain a mixed solution C. The mixed solution A of step (2) was added to the mixed solution C, and finally the pH was adjusted to 9.72 with NaOH; the arsenic removal reaction was stirred at normal pressure and room temperature for 24 hours, and the solid-liquid separation was performed to obtain arsenic-containing slag and filtrate; the arsenic content of the waste acid was 2800.0 mg / L, and the H 2 O 2 The molar ratio of lead slag to arsenic in waste acid is (1.1-1.2):1, the solid-liquid ratio of lead slag to waste acid is (0.02-0.03):1, the solid-liquid ratio of lead slag to nitric acid is (0.27-0.4):1, and the solid-liquid ratio of NaCl particles to H 2 O 2 The solid-liquid ratio of the solution was 0.04:1 g:mL, the mass ratio of NaCl particles to lead slag powder was 1:2.5 g:g, and the stirring speed was 180-200 r / min; the concentration of metal ions in the filtrate was determined by ICP and is shown in Table 3;
[0038] Table 3 Filtrate composition
[0039]
[0040] The toxicity leaching test of arsenic-containing solids was conducted according to the USEPA "Method 1311-toxicity Characterisitic Leaching Procedure" method provided by the US Environmental Protection Agency. The toxicity leaching results are shown in Table 4;
[0041] Table 4 Toxicity leaching results of arsenic-containing solids
[0042]
[0043] The arsenic content in the filtrate of this embodiment is 20.1 mg / L, and the arsenic removal rate is 99.2%.
[0044] Example 1 Comparative test
[0045] Table 5 Lead slag composition
[0046]
[0047] Table 6 Polluted acid composition
[0048]
[0049] When no chloride is provided and other conditions are the same as in Example 1, the arsenic removal is as shown in Table 7.
[0050] Table 7 Filtrate composition
[0051]
[0052] The toxicity leaching test of arsenic-containing solids was conducted according to the USEPA "Method 1311-toxicity Characteristic Leaching Procedure" method provided by the US Environmental Protection Agency. The toxicity leaching results are shown in Table 8;
[0053] Table 8 Toxicity leaching results of arsenic-containing solids
[0054]
[0055] Although the arsenic removal effect of lead slag without chloride modification is excellent, the toxic leaching effect of arsenic-containing solids is quite different from that after modification, which is far higher than the toxic leaching standard. This is because arsenic exists in the solution in the form of unstable free arsenate.
[0056] Example 2
[0057] The lead slag in this example was taken from a smelting plant in the southwest, and its composition is shown in Table 9. The waste acid was produced from the waste acid containing a large amount of impurities such as arsenic produced by washing the smelting flue gas in the sulfuric acid workshop of a copper smelter in the southwest, and its main components are shown in Table 10.
[0058] Table 9 Lead leaching residue composition
[0059]
[0060] Table 10 Polluted acid composition
[0061]
[0062] In this embodiment, a chloride-modified lead slag is used in conjunction with SiO 2 The method for removing arsenic, the specific steps are as follows:
[0063] (1) Sieving the lead slag to a particle size of 100 to 200 mesh to obtain lead leaching slag powder,
[0064] (2) Dissolve NaCl particles in deionized water and mix well to obtain a mixed solution A.
[0065] (3) H 2 O 2 Add to 200 mL of waste acid and mix evenly to obtain mixed solution B.
[0066] (4) The lead slag and HNO 3 The solution was added to the mixed solution B to obtain a mixed solution C. The mixed solution A of step (2) was added to the mixed solution C, and finally the pH was adjusted to 9.72 with NaOH; the arsenic removal reaction was stirred at normal pressure and room temperature for 24 hours, and the solid-liquid separation was performed to obtain arsenic-containing slag and filtrate; the arsenic content of the waste acid was 2740.0 mg / L, and the H 2 O 2 The molar ratio of lead slag to arsenic in waste acid is (1.1-1.2):1, the solid-liquid ratio of lead slag to waste acid is (0.02-0.03):1, the solid-liquid ratio of lead slag to nitric acid is (0.27-0.4):1, and the solid-liquid ratio of NaCl particles to H 2 O 2 The solid-liquid ratio of the solution was 0.04:1 g:mL, the mass ratio of NaCl particles to lead slag powder was 1:2.5 g:g, and the stirring speed was 180-200 r / min; the concentration of metal ions in the filtrate was determined by ICP method, see Table 11;
[0067] Table 11 Filtrate composition
[0068]
[0069] The toxicity leaching test of arsenic solids was conducted according to the USEPA
[0070] The method of "Method 1311-toxicity Characteristic Leaching Procedure" was used, and the toxicity leaching results are shown in Table 12;
[0071] Table 12 Toxicity leaching results of arsenic-containing solids
[0072]
[0073] The arsenic content in the filtrate of this embodiment is 13.6 mg / L, and the arsenic removal rate is 99.5%.
[0074] Example 2 Comparative Test
[0075] Table 13 Lead slag composition
[0076]
[0077] Table 14 Polluted acid composition
[0078]
[0079] When no chloride is provided and other conditions are the same as in Example 2, the arsenic removal is as shown in Table 15:
[0080] Table 15 Filtrate composition
[0081]
[0082] The toxicity leaching test of arsenic-containing solids was conducted according to the USEPA "Method 1311-toxicity Characteristic Leaching Procedure" method provided by the US Environmental Protection Agency. The toxicity leaching results are shown in Table 16;
[0083] Table 16 Toxicity leaching results of arsenic-containing solids
[0084]
[0085] Although the arsenic removal effect of lead slag without chloride modification is excellent, the toxic leaching effect of arsenic-containing solids is quite different from that after modification, which is far higher than the toxic leaching standard. This is because arsenic exists in the solution in the form of unstable free arsenate.
[0086] Example 3
[0087] The lead slag in this example was taken from a smelting plant in the southwest, and its composition is shown in Table 17. The waste acid was produced from the waste acid containing a large amount of impurities such as arsenic produced by washing the smelting flue gas in the sulfuric acid workshop of a copper smelter in the southwest, and its main components are shown in Table 18.
[0088] Table 17 Lead leaching residue composition
[0089]
[0090] Table 18 Polluted acid composition
[0091]
[0092] In this embodiment, a chloride-modified lead slag is used in conjunction with SiO 2 The method for removing arsenic, the specific steps are as follows:
[0093] (1) Sieving the lead slag to a particle size of 100 to 200 mesh to obtain lead leaching slag powder,
[0094] (2) Dissolve NaCl particles in deionized water and mix well to obtain a mixed solution A.
[0095] (3) H 2 O 2 Add to 200 mL of waste acid and mix evenly to obtain mixed solution B.
[0096] (4) The lead slag and HNO 3The solution was added to the mixed solution B to obtain a mixed solution C. The mixed solution A of step (2) was added to the mixed solution C, and finally the pH was adjusted to 9.72 with NaOH; the arsenic removal reaction was stirred at normal pressure and room temperature for 24 hours, and the solid-liquid separation was performed to obtain arsenic-containing slag and filtrate; the arsenic content of the waste acid was 1340.0 mg / L, and the H 2 O 2 The molar ratio of lead slag to arsenic in waste acid is (1.1-1.2):1, the solid-liquid ratio of lead slag to waste acid is (0.02-0.03):1, the solid-liquid ratio of lead slag to nitric acid is (0.27-0.4):1, and the solid-liquid ratio of NaCl particles to H 2 O 2 The solid-liquid ratio of the solution is g:mL 0.04:1, the mass ratio of NaCl particles to lead slag powder is g:g 1:2.5, and the stirring speed is 180-200 r / min; the concentration of metal ions in the filtrate is determined by ICP method, see Table 19.
[0097] Table 19 Filtrate composition
[0098]
[0099] The toxicity leaching test of arsenic solids was conducted according to the USEPA
[0100] The toxicity test results were shown in Table 20.
[0101] Table 20 Toxicity leaching results of arsenic-containing solids
[0102]
[0103] The arsenic content in the filtrate of this embodiment is 1.5 mg / L, and the arsenic removal rate is 99.8%.
[0104] Example 3 Comparative Test
[0105] Table 21 Lead slag composition
[0106]
[0107] Table 22 Composition of polluted acid
[0108]
[0109] When no chloride is provided and other conditions are consistent with the example, the arsenic removal is as shown in Table 23.
[0110] Table 23 Filtrate composition
[0111]
[0112] The toxicity leaching test of arsenic-containing solids was conducted according to the USEPA "Method 1311-toxicity Characterisitic Leaching Procedure" method provided by the US Environmental Protection Agency. The toxicity leaching results are shown in Table 24;
[0113] Table 24 Toxicity leaching results of arsenic-containing solids
[0114]
[0115] Although the arsenic removal effect of lead slag without chloride modification is excellent, the toxic leaching effect of arsenic-containing solids is quite different from that after modification, which is far higher than the toxic leaching standard. This is because arsenic exists in the solution in the form of unstable free arsenate.
[0116] In summary, 1. The present invention utilizes low-cost lead slag to remove arsenic, the raw materials are simple and easy to obtain, the process flow is simple, the operation is convenient, the metal waste slag is reused, and resources are saved;
[0117] 2. The present invention utilizes Pb 2+ with AsO 4 3- , Cl - Combined to form less soluble Pb 5 (AsO 4 ) 3 Cl, and Pb-As-Cl coprecipitation and SiO in lead slag 2 The formed silica gel can better fix arsenic, promote the stability of As to achieve the purpose of arsenic removal, and improve the efficiency and quality of arsenic removal;
[0118] 3. Aiming at the problem of waste acid discharge from factories, the present invention provides a method for removing arsenic from lead slag. The present invention utilizes low-cost lead slag to remove arsenic, which not only reduces the discharge of sludge during the waste acid treatment process, but also removes heavy metal Pb in the process of removing As, thereby achieving the purpose of secondary resource utilization by treating waste with waste.
[0119] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0120] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A method for removing arsenic by using chloride-modified lead slag in cooperation with SiO2, characterized in that: The specific steps include: S1, sieving the lead slag to a particle size of 100-200 mesh to obtain lead leaching slag powder; S2, dissolving NaCl particles in deionized water and mixing evenly; S3, adding H2O2 to the dirty acid and mixing evenly; S4, adding the lead leaching slag powder and HNO3 solution into step S3 to obtain a mixed solution A; S5, adding the solution obtained in step S2 to step S4 and mixing evenly to obtain a mixed solution B; S6. Using NaOH, adjust the pH of the mixed solution B to 9.7-10, shake and react at room temperature for 24 hours, and separate the solid and liquid to obtain arsenic-containing solids and a filtrate; In step S2, the mass ratio of NaCl particles to lead slag g:g is 1:2.5, and the solid-liquid ratio of NaCl particles to deionized water g:mL is 0.04:1; The arsenic content of the waste acid in step S3 is 1340.0-2800.0 mg / L, and the molar ratio of H2O2 to arsenic in the waste acid is (1.1-1.2):1; In step S4, the solid-liquid ratio of the lead slag to nitric acid is (0.27-0.4):1, and the solid-liquid ratio of the lead slag to the dirty acid is (0.02-0.03):
1. The oscillation rate of step S6 is 180-200 r / min.
Citation Information
Patent Citations
Method for preferably removing arsenic in lead and antimony smoke
CN105039722A
Comprehensive utilization method of arsenic-containing materials
CN106834715A
Method for removing arsenic in waste acid by utilizing silica gel to reinforce zinc slag
CN112891811A