A bismuth selenide electrode and its preparation method and application
The Bi2Se3 electrode was prepared by mechanical lift-off method and FIB technology, combined with dry transfer and van der Waals contact, which solved the problem of Fermi level pinning at the metal-semiconductor interface, improved the performance and stability of two-dimensional semiconductor devices, and achieved high quality electrode preparation.
Patent Information
- Application Number
- CN202210943546.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-08
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-08-08
AI Technical Summary
In the existing technology, the metal-semiconductor interface contact has a Fermi level pinning problem, which results in limited performance of semiconductor devices, especially in two-dimensional semiconductor devices, and lattice defects and chemical bonds are prone to occur during the preparation process of traditional electrodes. , affecting device performance.
Bi2Se3 electrodes were prepared using mechanical stripping, and local areas were removed to design channels through FIB technology. Combined with dry transfer and van der Waals contact methods, high-quality Bi2Se3 parallel electrodes were prepared and used on two-dimensional materials to form photodetectors.
It effectively solves the problem of Fermi level pinning at the metal-semiconductor interface, reduces the interface carrier recombination center, improves the reaction rate and device performance, avoids electrode short circuit, and improves the stability and performance of the device.
Smart Images

Figure CN115274883B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of topological material preparation, and in particular relates to a bismuth selenide (Bi2Se3) electrode and a preparation method and application thereof. Background Art
[0002] The contact problem of metal-semiconductor interface has become an increasingly important but unresolved problem in the semiconductor industry, which seriously hinders the ultimate structural scaling and performance of semiconductor devices. Ultra-thin two-dimensional semiconductor devices have excellent semiconductor properties, and good metal-semiconductor contact is essential. Compared with bulk semiconductor devices, the ultra-thin nature of two-dimensional semiconductors makes their metal-semiconductor contacts more susceptible to Fermi level pinning of chemical bonds and interface states.
[0003] Usually, a large number of lattice defects, chemical bonds and interface states are generated during the evaporation of metal electrodes, resulting in serious Fermi level. We avoid defects during the evaporation of electrodes by transferring the metallic two-dimensional electrode Bi2Se3. At the same time, van der Waals contact can effectively solve the Fermi level pinning problem of metal-two-dimensional semiconductor interface contact. Bi2Se3 is a member of topological materials. Due to strong spin-orbit coupling, it has conductive surface states that can effectively prevent time reversal perturbations such as crystal defects and non-magnetic impurities. Therefore, due to the unique characteristics of the surface states of topological materials, it is very attractive in basic research and applications in spin electronics, quantum information and low-energy dissipation electronics. Summary of the invention
[0004] In order to overcome the shortcomings and deficiencies in the prior art, the primary purpose of the present invention is to provide a method for preparing a topological material bismuth selenide semiconductor device electrode.
[0005] Another object of the present invention is to provide a bismuth selenide semiconductor device electrode prepared by the above preparation method.
[0006] Another object of the present invention is to provide an application of the above-mentioned bismuth selenide semiconductor device electrode.
[0007] The purpose of the present invention is achieved through the following technical solutions:
[0008] A method for preparing a bismuth selenide semiconductor device electrode comprises the following steps: sticking a Bi2Se3 single crystal to an adhesive tape, lightly pressing a side of the adhesive tape with the Bi2Se3 single crystal onto a Si / SiO2 substrate by a mechanical stripping method, and then separating the adhesive tape from the Si / SiO2 substrate, whereby a large block of uniform layered Bi2Se3 remains on the Si / SiO2 substrate; cutting off a local area of the Bi2Se3 on the Si / SiO2 substrate by FIB technology, making the length and width of a channel on the Bi2Se3, and obtaining a Bi2Se3 parallel electrode; and then using a dry transfer method to transfer the obtained Bi2Se3 parallel electrode to a two-dimensional material by using PVA to prepare a photodetector.
[0009] Preferably, the adhesive tape is a blue adhesive tape or a white adhesive tape.
[0010] Preferably, the thickness of the layered Bi2Se3 is 90-100 nm.
[0011] Preferably, the distance between two electrodes of the Bi2Se3 parallel electrodes is 0.1 to 1 micrometer.
[0012] Preferably, the two-dimensional material is WSe2 or WS2.
[0013] The above-mentioned method for preparing a bismuth selenide semiconductor device electrode specifically follows the following steps:
[0014] S1. Heat the Si / SiO2 substrate to 100°C and keep it warm for 5 minutes;
[0015] S2. The Bi2Se3 single crystal is adhered to the tape, and the side of the tape with the Bi2Se3 single crystal is gently pressed on the heated Si / SiO2 substrate for 15-60 seconds by mechanical stripping, and then the tape is separated from the Si / SiO2 substrate, and a large piece of uniform layered Bi2Se3 is left on the Si / SiO2 substrate;
[0016] S3. The Si / SiO2 substrate with Bi2Se3 was immersed in an acetone solution for 30 minutes to remove the residual glue on the substrate;
[0017] S4. Using FIB technology to cut off a local area of Bi2Se3 on the Si / SiO2 substrate, design the length and width of the channel according to the requirements, make the length and width of the channel on the Bi2Se3, and obtain Bi2Se3 parallel electrodes with different channel sizes;
[0018] S5. Using a dry transfer method, the Bi2Se3 parallel electrodes obtained in step S4 are transferred to the two-dimensional material using PVA;
[0019] S6. After annealing the Bi2Se3 parallel electrodes transferred to the two-dimensional material, a metal layer is deposited on the Bi2Se3 to obtain a photodetector.
[0020] Preferably, the temperature of the dry transfer in step S5 is 90°C.
[0021] Preferably, the annealing treatment in step S6 is performed at a temperature of 150° C. and for 30 minutes.
[0022] In step S6, a metal layer is deposited on Bi2Se3. The area of the metal layer can be larger than the area of Bi2Se3, so as to extend beyond the range of Bi2Se3. However, it should be noted that the metal layers deposited on the parallel electrodes of Bi2Se3 on both sides of the channel cannot be connected together, otherwise the electrodes will short-circuit. The purpose of depositing a metal layer on Bi2Se3 is that Bi2Se3 is easily damaged. In order to avoid this problem, a metal layer needs to be deposited on Bi2Se3, which is equivalent to protecting Bi2Se3 and extending the function of Bi2Se3.
[0023] A bismuth selenide semiconductor device electrode prepared by the above preparation method.
[0024] Application of the above-mentioned bismuth selenide semiconductor device electrode in the field of two-dimensional semiconductors.
[0025] The present invention can flexibly design the size of the channel by preparing the Bi2Se3 electrode, and can effectively solve the problem of traditional metal-semiconductor interface contact through van der Waals contact, reduce the recombination center of interface carriers, reduce the recombination of holes and electrons, thereby increasing the number of electrons and holes participating in the reaction and improving the reaction rate.
[0026] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0027] (1) The present invention adopts a mechanical stripping method to prepare Bi2Se3, and the Bi2Se3 prepared by the mechanical stripping method has high quality; at the same time, compared with traditional metal electrodes such as gold, platinum, palladium and silver, Bi2Se3 is not scarce and has a lower cost.
[0028] (2) The Bi2Se3 electrode of the present invention can effectively solve the Fermi level pinning problem at the metal-semiconductor interface through van der Waals contact, thereby improving the performance of the device.
[0029] (3) The equipment and preparation process required by the present invention are simple and low-cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 Schematic diagram of obtaining Bi2Se3 parallel electrodes with channels by cutting out a local area of Bi2Se3 using FIB technology.
[0031] Figure 2 This is an optical microscope image of the photodetector constructed with Bi2Se3 and WSe2 prepared in Example 1.
[0032] Figure 3 The IV curve measured for the photodetector constructed with Bi2Se3 and WSe2 prepared in Example 1.
[0033] Figure 4 This is an optical microscope image of the photodetector constructed with Bi2Se3 and WS2 prepared in Example 1.
[0034] Figure 5 This is the IV curve of the photodetector constructed with Bi2Se3 and WS2 prepared in Example 1. DETAILED DESCRIPTION
[0035] The content of the present invention is further described below in conjunction with specific examples, but it should not be construed as limiting the present invention. If not specifically indicated, the technical means used in the examples are conventional means well known to those skilled in the art. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0036] The dry transfer described in the following examples is to drop PVA (polyvinyl alcohol) on PDMS and scrape it flat, and keep it warm for 30 minutes. A PVA film is formed on the PDMS, and then the PDMS with the PVA film is glued to a glass slide, and lightly pressed on the target transfer material, and kept warm at 90-95 degrees for 5-7 minutes, and the target material will be transferred to the PVA film. Then the PVA film with the target material is glued to the PDMS again, and the PDMS is adhered to the glass slide, and then the target material on the PVA is transferred to another target material.
[0037] Example 1
[0038] 1. Stick the Bi2Se3 single crystal to the blue tape, and gently press the side of the tape with the Bi2Se3 single crystal on the Si / SiO2 substrate for 60 seconds by mechanical stripping, and then separate the tape from the Si / SiO2 substrate. At this time, large pieces of uniform layered Bi2Se3 remain on the Si / SiO2 substrate;
[0039] 2. Soak the Si / SiO2 substrate with Bi2Se3 in acetone solution for 30 minutes to remove the residual glue on the substrate;
[0040] 3. Use FIB technology to cut off the local area of Bi2Se3 on the Si / SiO2 substrate, design the length and width of the channel on Bi2Se3, and obtain Bi2Se3 parallel electrodes, such as Figure 1 As shown;
[0041] 4. Stick the WSe2 single crystal to the blue tape, and gently press the side of the tape with the WSe2 single crystal on the Si / SiO2 substrate for 40 seconds by mechanical stripping, and then separate the tape from the Si / SiO2 substrate. At this time, large pieces of uniform layered WSe2 remain on the Si / SiO2 substrate;
[0042] 5. Soak the Si / SiO2 substrate with WSe2 in acetone solution for 30 minutes to remove the residual glue on the substrate;
[0043] 6. Heat the Si / SiO2 substrate with WSe2 to 150℃ and keep it warm for 30min;
[0044] 7. Using the dry transfer method, transfer the Bi2Se3 parallel electrodes obtained in step 3 to the WSe2 dried in step 5 using PVA;
[0045] 8. After transfer, soak the sample in deionized water to remove PVA;
[0046] 9. After removing PVA, heat the sample to 150°C and keep warm for 30 minutes;
[0047] 10. After annealing, a metal layer is deposited on Bi2Se3 (Ti / Au is used for the metal layer in this embodiment). The area of the metal layer can be larger than the area of Bi2Se3, so as to extend beyond the range of Bi2Se3. However, it should be noted that the metal layers deposited on the parallel electrodes of Bi2Se3 on both sides of the channel cannot be connected together. In this way, a Bi2Se3-WSe2-Bi2Se3 sample is prepared, and the sample is placed on a probe station for photoelectric testing. The purpose of depositing a metal layer on Bi2Se3 is because Bi2Se3 is easily damaged. In order to avoid this problem, a metal layer needs to be deposited on Bi2Se3. In this embodiment, a titanium-gold electrode is obtained by photolithography and gold plating, which is equivalent to protecting Bi2Se3 and extending the function of Bi2Se3.
[0048] Figure 2 This is an optical microscope photograph of Bi2Se3-WSe2-Bi2Se3 prepared in this example. Figure 3 This is the IV curve of Bi2Se3-WSe2-Bi2Se3.
[0049] Example 2
[0050] 1. Stick the Bi2Se3 single crystal to the white tape, and gently press the side of the tape with the Bi2Se3 single crystal on the Si / SiO2 substrate for 15 seconds by mechanical stripping, and then separate the tape from the Si / SiO2 substrate. At this time, large pieces of uniform layered Bi2Se3 remain on the Si / SiO2 substrate;
[0051] 2. Soak the Si / SiO2 substrate with Bi2Se3 in acetone solution for 30 minutes to remove the residual glue on the substrate;
[0052] 3. Use FIB technology to cut off the local area of Bi2Se3 on the Si / SiO2 substrate, design the length and width of the channel on Bi2Se3, and obtain Bi2Se3 parallel electrodes, such as Figure 1 As shown;
[0053] 4. Stick the single crystal of WS2 to the white tape, and gently press the side of the tape with the WS2 single crystal on the Si / SiO2 substrate for 60 seconds by mechanical stripping, and then separate the tape from the Si / SiO2 substrate. At this time, a large piece of uniform layered WS2 remains on the Si / SiO2 substrate;
[0054] 5. Soak the Si / SiO2 substrate with WS2 in acetone solution for 30 minutes to remove the residual glue on the substrate;
[0055] 6. Heat the Si / SiO2 substrate with WS2 to 150°C and keep it warm for 30 minutes;
[0056] 7. Using the dry transfer method, transfer the Bi2Se3 parallel electrodes obtained in step 3 to the WS2 dried in step 5 using PVA;
[0057] 8. After transfer, soak the sample in deionized water to remove PVA;
[0058] 9. After removing PVA, heat the sample to 150°C and keep warm for 30 minutes;
[0059] 10. After annealing, a metal layer is deposited on Bi2Se3 (Ti / Au is used for the metal layer in this embodiment). The area of the metal layer can be larger than the area of Bi2Se3, so as to extend beyond the range of Bi2Se3. However, it should be noted that the metal layers deposited on the parallel electrodes of Bi2Se3 on both sides of the channel cannot be connected together. In this way, a Bi2Se3-WS2-Bi2Se3 sample is prepared, and the sample is placed on a probe station for photoelectric testing. The purpose of depositing a metal layer on Bi2Se3 is because Bi2Se3 is easily damaged. In order to avoid this problem, a metal layer needs to be deposited on Bi2Se3. In this embodiment, a titanium-gold electrode is obtained by photolithography and gold plating, which is equivalent to protecting Bi2Se3 and extending the function of Bi2Se3.
[0060] Figure 4 This is an optical microscope photograph of Bi2Se3-WS2-Bi2Se3 prepared in this example. Figure 5 This is the IV curve of Bi2Se3-WS2-Bi2Se3.
[0061] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principles of the present invention shall be equivalent replacement methods and shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a bismuth selenide semiconductor device electrode, characterized in that The method comprises the following steps: sticking a Bi2Se3 single crystal to an adhesive tape, lightly squeezing a side of the adhesive tape with the Bi2Se3 single crystal onto a Si / SiO2 substrate by a mechanical stripping method, and then separating the adhesive tape from the Si / SiO2 substrate, whereby large blocks of uniform layered Bi2Se3 remain on the Si / SiO2 substrate; using FIB technology to cut off a local area of the Bi2Se3 on the Si / SiO2 substrate, making the length and width of a channel on the Bi2Se3, and obtaining a Bi2Se3 parallel electrode; and then using a dry transfer method, using PVA to transfer the obtained Bi2Se3 parallel electrode to a two-dimensional material, wherein the two-dimensional material is WSe2 or WS2, and preparing a bismuth selenide semiconductor device electrode.
2. The method for preparing a bismuth selenide semiconductor device electrode according to claim 1, characterized in that: The adhesive tape is a blue adhesive tape or a white adhesive tape.
3. The method for preparing a bismuth selenide semiconductor device electrode according to claim 1, characterized in that: The thickness of the layered Bi2Se3 is 90-100 nm.
4. The method for preparing a bismuth selenide semiconductor device electrode according to claim 1, characterized in that: The distance between the two electrodes of the Bi2Se3 parallel electrodes is 0.1-1 micrometer.
5. The method for preparing a bismuth selenide semiconductor device electrode according to claim 1, characterized in that Follow these steps: S1. Heat the Si / SiO2 substrate to 100 °C and keep it at this temperature for 5 minutes; S2. The Bi2Se3 single crystal is adhered to the tape, and the side of the tape with the Bi2Se3 single crystal is gently pressed on the heated Si / SiO2 substrate for 15-60 seconds by mechanical exfoliation, and then the tape is separated from the Si / SiO2 substrate, and a large piece of uniform layered Bi2Se3 is left on the Si / SiO2 substrate; S3. The Si / SiO2 substrate with Bi2Se3 was immersed in an acetone solution for 30 minutes to remove the residual glue on the substrate; S4. Using FIB technology to cut off a local area of Bi2Se3 on a Si / SiO2 substrate, design the length and width of the channel according to the requirements, make the length and width of the channel on Bi2Se3, and obtain Bi2Se3 parallel electrodes with different channel sizes; S5. Using a dry transfer method, the Bi2Se3 parallel electrodes obtained in step S4 are transferred to the two-dimensional material using PVA; S6. After annealing the Bi2Se3 parallel electrodes transferred onto the two-dimensional material, a metal layer is deposited on the Bi2Se3 to obtain a photodetector.
6. The preparation method according to claim 5, characterized in that: The temperature of the dry transfer in step S5 is 90°C.
7. The preparation method according to claim 5, characterized in that: The annealing treatment in step S6 is performed at a temperature of 150° C. and for 30 min.
8. A bismuth selenide semiconductor device electrode prepared by the preparation method according to any one of claims 1 to 7.
9. Application of the bismuth selenide semiconductor device electrode according to claim 8 in the field of two-dimensional semiconductors.
Citation Information
Patent Citations
Method for stripping and transferring large-area layered two-dimensional material
CN113200523A
Topological insulator / molybdenum ditelluride heterojunction-based phototransistor, and production method and application thereof
CN113964219A