High-responsivity β-Ga2O3-based heterojunction self-powered ultraviolet detector and its preparation method and application

The low responsivity is solved by introducing the intrinsic β-Ga2O3 depletion layer, MgO:Na (or K) passivation layer and n+-β-Ga2O3:Sn electron collection layer into the β-Ga2O3-based heterojunction UV detector. and the problem of small open circuit voltage, achieving higher responsivity and current efficiency.

CN115295677BActive Publication Date: 2024-10-29BEIJING MING GALLIUM SEMICON CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210996460.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-19
Publication Date
2024-10-29
Estimated Expiration
2042-08-19

AI Technical Summary

Technical Problem

Existing β-Ga2O3-based heterojunction ultraviolet detectors have low responsivity, small open circuit voltage, and continuous photoconductivity, resulting in a light response speed of the order of seconds.

Method used

It is composed of a substrate, a first electrode, a p-type wide bandgap conductive film, an intrinsic β-Ga2O3 film depletion layer, an n-β-Ga2O3:Sn conductive film, an n+-β-Ga2O3:Sn electron collection layer and MgO: Highly responsive β-Ga2O3-based isoform composed of Na or MgO:K thin film passivation layer The mass-junction self-powered UV detector structure is prepared through vacuum film-making technology such as metal-organic vapor phase epitaxy, pulse laser deposition, etc., using intrinsic β-Ga2O3 as the depletion layer and absorption layer, and the MgO:Na (or K) film as Passivation layer, n+-β-Ga2O3:Sn film serves as electron collection layer.

Benefits of technology

The responsivity of the β-Ga2O3-based heterojunction UV detector is increased by nearly 2 times, the short-circuit current and open-circuit voltage are increased, the recombination of photogenerated carriers is reduced, and the electron collection efficiency is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115295677B_ABST
    Figure CN115295677B_ABST
Patent Text Reader

Abstract

The invention discloses a high-responsivity β-Ga2O3-based heterojunction self-powered ultraviolet detector and its preparation method and application, belonging to the field of semiconductor photoelectric devices. The ultraviolet detector comprises a substrate, a first electrode, a p-type wide bandgap conductive film, an intrinsic β-Ga2O3 film depletion layer, an n-β-Ga2O3:Sn conductive film, and an n-type conductive film. + β-Ga2O3:Sn electron collection layer, MgO:Na or MgO:K thin film passivation layer and second electrode, the bandgap width of the p-bandgap conductive film is greater than 3.0eV. The present invention uses vacuum film-making methods such as chemical vapor deposition, metal organic vapor phase epitaxy, pulsed laser deposition, etc. to obtain a high-responsivity β-Ga2O3-based heterojunction self-powered ultraviolet detector, which effectively improves the responsiveness of the β-Ga2O3-based heterojunction thin film ultraviolet detector, and has broad prospects for application in solar-blind band detection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of semiconductor optoelectronic devices, and in particular relates to a high-responsivity β-Ga2O3-based heterojunction self-powered ultraviolet detector and a preparation method and application thereof. Background Art

[0002] Due to the complete absorption of ultraviolet radiation in the 200-280nm band by the ozone layer, this band is almost non-existent in the atmosphere, so it is called the "solar blind" band. Ultraviolet detectors based on this band have the advantages of low background noise and low false alarm rate. They have broad application prospects in military fields such as ultraviolet guidance, ultraviolet space warning and missile warning, as well as in civil fields such as high-response fire warning, corona detection, and atmospheric environment monitoring, and have received extensive attention from researchers.

[0003] Although traditional semiconductor materials such as Si and Ge have the advantages of low cost and mature technology, due to their narrow bandgap width, they usually need to add cooling devices, resulting in large equipment size and unstable performance under high temperature and high pressure environments. In terms of "solar-blind" band detection, high-quality filters are required, which limits their responsiveness. Wide-bandgap semiconductor ultraviolet detectors directly respond to ultraviolet photons without the need for complex and expensive optical components. They have the advantages of small size, high stability, integration and high quantum efficiency. The bandgap width of β-Ga2O3 is 4.90eV, which is in the "solar-blind" band. It also has extremely high chemical stability and thermal stability, and is a natural solar-blind ultraviolet detection material. β-Ga2O3 has remarkable photoelectric performance as a solar-blind ultraviolet detector. Compared with other ultraviolet photodetectors, it has good spectral selectivity and small dark current [Zou R, Zhang Z, Liu Q, et al. High detectivity solar-blind high-temperature deep-ultraviolet photodetector based on multi-layered (l00) facet-oriented β-Ga2O3 nanobelts [J]. Small: 2014, 10 (9): 1848-56.].

[0004] At present, n-type β-Ga2O3 can be achieved by doping with elements such as Sn and Si. This method can be cited from the literature [SC Siah, RE Brandt, K. Lim, LT Schelhas, R. Jaramillo, MD Heinemann, D. Chua, J. Wright, JD Perkins, CUS Segre, RG Gordon, MF Toney, and T. Buonassisi. Dopant activation in Sn-doped Ga2O3 investigated by X-ray absorption spectroscopy. APPLIED PHYSICS LETTERS 107, 252103 (2015)]. P-type β-Ga2O3 is difficult to obtain, resulting in β-Ga2O3-based junction photodetectors mainly being heterojunctions. The currently known β-Ga2O3-based heterojunction detectors may have the following disadvantages: 1) low responsivity and low open-circuit voltage; 2) the existence of continuous photoconductivity, resulting in a light response speed of seconds. Summary of the invention

[0005] In order to solve the problem of low responsivity of existing β-Ga2O3-based heterojunction thin film ultraviolet detectors, the main purpose of the present invention is to provide a high-responsivity β-Ga2O3-based heterojunction self-powered ultraviolet detector.

[0006] Another object of the present invention is to provide a method for preparing the above-mentioned high-responsivity β-Ga2O3-based heterojunction self-powered ultraviolet detector.

[0007] Another object of the present invention is to provide the application of the above-mentioned high-responsivity β-Ga2O3-based heterojunction self-powered ultraviolet detector in solar-blind band detection.

[0008] To achieve the above object, the present invention adopts the following technical solutions:

[0009] The invention provides a high-responsivity β-Ga2O3-based heterojunction self-powered ultraviolet detector, which comprises, from bottom to top, a substrate, a first electrode, a p-type wide bandgap conductive film, an intrinsic β-Ga2O3 film depletion layer, an n-β-Ga2O3:Sn conductive film, and an n-β-Ga2O3:Sn conductive film. + -β-Ga2O3:Sn electron collection layer, MgO:Na or MgO:K thin film passivation layer and second electrode; wherein:

[0010] The bandgap width of the p-type wide bandgap conductive film is greater than 3.0 eV;

[0011] The intrinsic β-Ga2O3 film depletion layer is located between the p-type wide bandgap conductive film and the n-β-Ga2O3:Sn conductive film;

[0012] The MgO:Na or MgO:K thin film passivation layer covers the n-β-Ga2O3:Sn conductive film;

[0013] The + -β-Ga2O3:Sn electron collection layer is located between the n-β-Ga2O3:Sn conductive film and the second electrode.

[0014] Preferably, the substrate is selected from sapphire, silicon or metal material with a flat and smooth surface.

[0015] Preferably, the first electrode is a Ru / Ni / Ag / Pt / Au stacked alloy film, wherein the thickness of Ru is 5-50nm, the thickness of Ni is 10-100nm, the thickness of Ag is 10-100nm, the thickness of Pt is 10-100nm, and the thickness of Au is 50-1000nm.

[0016] Preferably, the second electrode is a Ti / Au laminated alloy film, the thickness of Ti is 10-500 nm, and the thickness of Au is 50-1000 nm.

[0017] Preferably, the thickness of the intrinsic β-Ga2O3 thin film depletion layer is 5-50 nm.

[0018] Preferably, the Sn atomic percentage in the n-β-Ga2O3:Sn conductive film is 0.01at%-1at%, and the thickness is 300-2000nm.

[0019] Preferably, the n + -β-Ga2O3:Sn electron collection layer has a strip structure, wherein the Sn atomic percentage is 1at%–10at% and the thickness is 50–500nm.

[0020] Preferably, the p-type wide bandgap conductive film is selected from one or more of p-GaN, p-SiC, and p-ZnO conductive films.

[0021] Preferably, the thickness of the MgO:Na or MgO:K thin film passivation layer is 50-500 nm, and the atomic percentage content of Na or K is 0.1 at%-5 at%.

[0022] The present invention also provides a method for preparing the above-mentioned high-responsivity β-Ga2O3-based heterojunction self-powered ultraviolet detector, comprising the following steps:

[0023] S101, cleaning the substrate;

[0024] S102, preparing a Ru / Ni / Ag / Pt / Au stacked alloy thin film as a first electrode on the cleaned substrate by vacuum magnetron sputtering;

[0025] S103, preparing a p-type wide bandgap conductive film on the first electrode by a vacuum film forming method selected from metal organic vapor phase epitaxy (MOVPE), pulsed laser deposition (PLD), magnetron sputtering or molecular beam epitaxy (MBE);

[0026] S104, preparing an intrinsic β-Ga2O3 thin film depletion layer on the p-type wide bandgap conductive film by PLD;

[0027] S105, preparing an n-β-Ga2O3:Sn conductive film on the intrinsic β-Ga2O3 film depletion layer by PLD;

[0028] S106, covering the n-β-Ga2O3:Sn conductive film with a mask plate, and preparing n-β-Ga2O3:Sn conductive film on the n-β-Ga2O3:Sn conductive film by PLD + -β-Ga2O3:Sn electron collection layer;

[0029] S107, vacuum film forming method using mask plate combined with magnetron sputtering in n + -Ti / Au alloy stacked film is prepared on the β-Ga2O3:Sn electron collection layer as the second electrode;

[0030] S108, covering the second electrode with a mask plate, and preparing a MgO:Na or MgO:K thin film passivation layer on the n-β-Ga2O3:Sn conductive film by a vacuum film forming method using magnetron sputtering.

[0031] Preferably, the preparation process parameters of the intrinsic β-Ga2O3 thin film depletion layer include: introducing O2 gas, a growth pressure of 0.01-0.1 Pa, a growth temperature of 380-650°C, a distance between the substrate and the target material of 20-50 mm, and a growth time of 1-10 min.

[0032] Preferably, the preparation process parameters of the n-β-Ga2O3:Sn conductive film include: introducing O2 gas, a growth pressure of 0.01-5 Pa, a growth temperature of 350-950°C, a distance between the substrate and the target material of 20-50 mm, and a growth time of 100-240 min.

[0033] Preferably, the n +The preparation process parameters of the -β-Ga2O3:Sn electron collection layer include: introducing O2 gas, growth pressure of 0.01–5Pa, growth temperature of 350–950℃, distance between substrate and target of 20–50mm, and growth time of 30–60min.

[0034] Preferably, the preparation process parameters of the MgO:Na or MgO:K thin film passivation layer include: introducing a mixed gas of Ar and O2, with a volume ratio of Ar:O2 of 1:0.1-10, a growth pressure of 0.5-5Pa, a sputtering power of 10-80W, a growth temperature of 200-600°C, and a growth time of 20-120min.

[0035] The present invention also provides the application of the above-mentioned high-responsivity β-Ga2O3-based heterojunction self-powered ultraviolet detector in solar-blind band detection.

[0036] The present invention utilizes vacuum film-making technologies such as chemical vapor deposition (CVD), metal organic vapor phase epitaxy (MOVPE), and pulsed laser deposition (PLD) to prepare a high-responsivity β-Ga2O3-based heterojunction self-powered ultraviolet detector on a substrate with a flat and smooth surface such as sapphire, silicon, or metal, and uses intrinsic β-Ga2O3 as a depletion layer and an absorption layer, and a MgO:Na (or K) film as a passivation layer. + -β-Ga2O3:Sn thin film is used as the electron collection layer, which makes the β-Ga2O3-based heterojunction solar-blind detector have higher responsivity. Compared with the existing β-Ga2O3-based heterojunction UV detector, the responsivity is increased by nearly 2 times, and it has the following advantages:

[0037] 1) When light is incident on intrinsic β-Ga2O3, since this film is not doped and the lattice distortion is small, the photogenerated carriers drift rapidly to the loop under the action of the built-in electric field, reducing the recombination of the photogenerated carriers and increasing the short-circuit current and open-circuit voltage.

[0038] 2) Using MgO:Na (or K) film as a passivation layer reduces surface recombination.

[0039] 3) Using n + -β-Ga2O3:Sn film acts as an electron collection layer, which improves the electron collection efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] The above and other objects, features and advantages of the exemplary embodiments of the present invention will become readily understood by reading the detailed description below with reference to the accompanying drawings. In the accompanying drawings, several embodiments of the present invention are shown in an exemplary and non-limiting manner, in which:

[0041] Figure 1The schematic diagram of the structure of the high-responsivity β-Ga2O3-based heterojunction self-powered ultraviolet detector in the embodiment; wherein:

[0042] 1——substrate;

[0043] 2——Ru / Ni / Ag / Pt / Au first electrode;

[0044] 3——p-type wide bandgap conductive film;

[0045] 4——Intrinsic β-Ga2O3 thin film depletion layer;

[0046] 5——n-β-Ga2O3:Sn conductive film;

[0047] 6——n + -β-Ga2O3:Sn electron collection layer;

[0048] 7——MgO:Na (or K) thin film passivation layer;

[0049] 8——Ti / Au second electrode.

[0050] Figure 2 Graph showing the relationship between wavelength and responsivity of the high-responsivity β-Ga2O3-based heterojunction self-powered ultraviolet detector (1) and the traditional β-Ga2O3-based heterojunction self-powered ultraviolet detector (2) in the embodiment. DETAILED DESCRIPTION

[0051] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described in conjunction with the drawings of the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.

[0052] like Figure 1 As shown, a high-responsivity β-Ga2O3-based heterojunction self-powered ultraviolet detector is exemplarily described, including a substrate 1, a first electrode 2, a p-type wide bandgap conductive film 3, an intrinsic β-Ga2O3 film depletion layer 4, an n-β-Ga2O3:Sn conductive film 5, and an n-β-Ga2O3:Sn conductive film 6. + -β-Ga2O3:Sn electron collection layer 6, MgO:Na (or K) thin film passivation layer 7 and second electrode 8; wherein: the first electrode 2 is arranged on the substrate 1, the p-type wide bandgap conductive film 3 is arranged on the first electrode 2, the intrinsic β-Ga2O3 thin film depletion layer 4 is arranged on the p-type wide bandgap conductive film 3, the n-β-Ga2O3:Sn conductive film 5 is arranged on the intrinsic β-Ga2O3 thin film depletion layer 4, and the n-β-Ga2O3:Sn conductive film 5 is arranged on the intrinsic β-Ga2O3 thin film depletion layer 4. +-β-Ga2O3:Sn electron collection layer 6 is a strip structure, and MgO:Na (or K) thin film passivation layer 7 is cross-arranged on n-β-Ga2O3:Sn conductive film 5, and the second electrode 8 is arranged on n + -β-Ga2O3:Sn electron collection layer 6, constructing "substrate / first electrode / p-type wide bandgap conductive film / intrinsic β-Ga2O3 film depletion layer / n-β-Ga2O3:Sn conductive film / n-β-Ga2O3:Sn conductive film" + -β-Ga2O3:Sn electron collection layer (MgO:Na (or K) thin film passivation layer) / second electrode" UV detector structure.

[0053] In some embodiments, the substrate 1 may be made of a smooth-surface substrate such as sapphire, quartz, or metal.

[0054] In some embodiments, the bandgap width of the p-type wide bandgap conductive film 3 is greater than 3.0 eV, and its thickness is 50-200 nm; the intrinsic β-Ga2O3 film depletion layer 4 is a high-quality β-Ga2O3 film without any other impurities, and its thickness is 5-50 nm; the Sn atomic percentage in the n-β-Ga2O3:Sn conductive film 5 is 0.01 at%-1 at%, and its thickness is 300-2000 nm; + The atomic percentage of Sn in the -β-Ga2O3:Sn electron collection layer 6 is 1at%-10at%, and its thickness is 50-500nm; the atomic percentage of Na or K in the MgO:Na (or K) thin film passivation layer 7 is 0.1at%-5at%, and its thickness is 50-500nm.

[0055] In some embodiments, if the p-type wide bandgap conductive film 3 is a p-GaN film, it is prepared by MOVPE and is a Mg-doped p-GaN film (p-GaN:Mg); if the p-type wide bandgap conductive film 3 is a p-ZnO film, it is prepared by magnetron sputtering and is an N-doped p-ZnO film (p-ZnO:N); the n-β-Ga2O3:Sn conductive film 5 or n + -β-Ga2O3:Sn electron collection layer 6 is prepared by PLD; MgO:Na (or K) thin film passivation layer 7 is prepared by magnetron sputtering.

[0056] In some embodiments, the first electrode 2 is a Ru / Ni / Ag / Pt / Au alloy stack, the thickness of Ru is 5-50nm; the thickness of Ni is 10-100nm; the thickness of Ag is 10-100nm; the thickness of Pt is 10-100nm; the thickness of Au is 50-1000nm; the second electrode 8 is a Ti / Au alloy, the thickness of Ti is 10-500nm, and the thickness of Au is 50-1000nm.

[0057] In some embodiments, the first electrode 2Ti / Au, Ru / Ni / Ag / Pt / Au alloy stack is prepared by using vacuum technology such as electron beam and magnetron sputtering combined with mask technology.

[0058] In the following examples, the following preparation method is used to prepare a high-responsivity β-Ga2O3-based heterojunction self-powered ultraviolet detector, and the steps are as follows:

[0059] a) Substrate cleaning: The substrate was cleaned with ethanol, acetone, and deionized water in sequence for a time period of t1, and then dried with nitrogen gas;

[0060] b) placing the cleaned substrate into a growth chamber of a magnetron sputtering device, setting process parameters such as atmosphere and vacuum, and preparing a Ru / Ni / Ag / Pt / Au alloy stack as a first electrode;

[0061] c) placing the "substrate / first electrode" on which the first electrode is deposited into a MOVPE reaction chamber or a magnetron sputtering growth chamber, setting process parameters such as growth temperature, atmosphere, and vacuum degree, and preparing a p-GaN or p-ZnO conductive film;

[0062] d) placing the “substrate / first electrode / p-GaN (or p-ZnO) film” into a pulsed laser deposition device (PLD) to prepare an intrinsic n-β-Ga2O3 film and a n-β-Ga2O3:Sn conductive layer film;

[0063] e) Using mask technology to cover the n-β-Ga2O3:Sn conductive layer film, use PLD equipment to deposit n + -β-Ga2O3:Sn electron collection layer;

[0064] f) Based on step e), using mask technology, magnetron sputtering equipment is used to deposit n + - On the β-Ga2O3:Sn electron collection layer, the second electrode is deposited;

[0065] g) Using mask technology to cover the second electrode film, a magnetron sputtering device is used to deposit a MgO:Na (or K) film passivation layer.

[0066] In step a), ethanol and acetone are first ultrasonicated for 15 minutes each, then washed with deionized water, and finally blown clean with nitrogen.

[0067] In steps e) and f), n + -β-Ga2O3:Sn electron collection layer and the second electrode mask plate covering it have the same shape, both of which are rectangular.

[0068] In step g), the MgO:Na (or K) thin film passivation layer mask plate is in a rectangular shape.

[0069] In steps e), f) and g), n + The ratio of the width of the β-Ga2O3:Sn electron collection layer and the second electrode mask to the width of the mask used for the MgO:Na (or K) thin film passivation layer is 1:2.

[0070] The above-mentioned production process also includes:

[0071] (A) The process parameters for PLD preparation of intrinsic β-Ga2O3 thin film depletion layer are: introduction of O2 gas, growth pressure of 0.01–0.1 Pa, growth temperature of 380–650°C, distance between substrate and target of 20–50 mm, and growth time of 1–10 min;

[0072] (B) The process parameters for preparing n-β-Ga2O3:Sn conductive thin films by PLD are: introduction of O2 gas, growth pressure of 0.01–5 Pa, growth temperature of 350–950 °C, distance between substrate and target of 20–50 mm, and growth time of 100–240 min;

[0073] (C)PLD preparation + -β-Ga2O3:Sn electron collection layer process parameters are: O2 gas, growth pressure of 0.01–5Pa, growth temperature of 350–950℃, distance between substrate and target of 20–50mm, growth time of 30–60min;

[0074] (D) The process parameters for preparing the MgO:Na (or K) thin film passivation layer by magnetron sputtering are: introducing a mixed gas of Ar and O2 with an Ar:O2 value ranging from 0 to 10:1, a growth pressure of 0.5–5 Pa, a sputtering power of 10–80 W, a growth temperature of 200–600 °C, and a growth time of 20–120 min.

[0075] Aiming at the problems of low responsiveness and low open-circuit voltage of β-Ga2O3-based heterojunction thin film solar-blind detector, the present invention prepares a high-responsiveness β-Ga2O3-based heterojunction self-powered ultraviolet detector. In the n-β-Ga2O3:Sn / p-wide-bandgap conductive film heterojunction, the intrinsic high-quality β-Ga2O3 film is used to increase the depletion layer width, thereby improving the light absorption rate and utilization rate; by adding a MgO:Na (or K) film passivation layer, the n-β-Ga2O3:Sn conductive layer is surface passivated and field passivated; by adding n + -β-Ga2O3:Sn electron collection reduces the current and voltage loss between the electrode and the conductive layer. Through the above method, the open circuit voltage and short circuit current of the β-Ga2O3 heterojunction thin film ultraviolet light detector are improved, thereby improving the responsivity.

[0076] Example 1

[0077] In this embodiment, a high-responsivity β-Ga2O3-based heterojunction self-powered ultraviolet detector is prepared, and the steps are as follows:

[0078] S201, sapphire substrate cleaning. First, ultrasonicate with ethanol and acetone for 15 minutes each, then soak with 80°C dilute hydrochloric acid for 10 minutes, and finally soak with a mixed acid solution of H3PO4:H2SO4=1:3 at 100°C for 10 minutes.

[0079] S202, placing the cleaned substrate into a growth chamber of a magnetron sputtering device, setting process parameters such as atmosphere and vacuum, and preparing a Ru / Ni / Ag / Pt / Au stacked first electrode;

[0080] S203, placing the substrate with the first electrode deposited thereon into the MOVPE reaction chamber, using trimethylgallium (TMGa), bismuth magnesium (Cp2Mg) and high-purity ammonia (NH3) as Ga, Mg and N sources respectively. High-purity hydrogen (H2) is used as the carrier gas. The sapphire substrate is baked at 1050°C in H2 atmosphere, nitrided in H2 / NH3 atmosphere, and grown at 550°C for 180 minutes to prepare a p-GaN:Mg conductive layer.

[0081] S204. Place the "substrate / first alloy metal film electrode / p-GaN conductive film" into the growth chamber of the PLD equipment, introduce O2 gas, the growth pressure is 0.085Pa, the growth temperature is 480°C, the distance between the substrate and the target is 40mm, the target is high-purity (99.999%) Ga2O3, the growth time is 3min, and an intrinsic β-Ga2O3 thin film depletion layer is prepared.

[0082] S205. Based on step S204, the growth process is changed. O2 gas is introduced, the growth pressure is 1 Pa, the growth temperature is 500° C., the distance between the substrate and the target is 45 mm, the target is Ga2O3 with a Sn atomic percentage of 0.5 at%, and the growth time is 120 min to prepare an n-β-Ga2O3:Sn conductive film.

[0083] S206, using mask technology, cover the n-β-Ga2O3:Sn conductive layer film, put it into the growth chamber of the PLD equipment, introduce O2 gas, the growth pressure is 0.85Pa, the growth temperature is 500℃, the target material is Ga2O3 with a Sn atomic percentage of 3at%, the distance between the substrate and the target material is 40mm, the growth time is 40min, and the n-β-Ga2O3:Sn conductive layer film is prepared. + -β-Ga2O3:Sn electron collection layer.

[0084] S207, based on step S206, using mask technology and magnetron sputtering equipment, + -β-Ga2O3:Sn electron collection layer, prepare the second electrode.

[0085] S208, using mask technology, using magnetron sputtering equipment, introducing Ar:O2=5:1 mixed gas, the growth pressure is 0.8Pa, the target material is MgO with 1at% Na atomic content, the sputtering power is 15W, the growth temperature is 450℃, the growth time is 40min, at n + -β-Ga2O3:Sn electron collection layer, and a MgO:Na thin film passivation layer is prepared to obtain "sapphire substrate / (Ru / Ni / Ag / Pt / Au) stacked first electrode / p-GaN:Mg conductive layer / intrinsic β-Ga2O3 thin film depletion layer / n-β-Ga2O3:Sn conductive film / n-β-Ga2O3:Sn conductive film / n-β-Ga2O3:Sn conductive film" + -β-Ga2O3:Sn electron collection layer / MgO:Na thin film passivation layer / (Ti / Au) stacked second electrode" ultraviolet light detector.

[0086] The photoelectric performance of the above-mentioned β-Ga2O3-based pn heterojunction UV detector was tested. The results showed that the device has a maximum responsivity near a wavelength of 254nm under a 0V bias. When the wavelength is greater than 270nm, the responsivity value decreases significantly. Figure 2 As shown, it is indicated that the ultraviolet detector obtained by the present invention has a solar-blind characteristic.

[0087] Example 2

[0088] Under the same process conditions as Example 1, this example prepares a "sapphire substrate / (Ru / Ni / Ag / Pt / Au) stacked first electrode / p-GaN:Mg conductive layer / n-β-Ga2O3:Sn conductive film / (Ti / Au) stacked second electrode" ultraviolet detector, and the specific process is as follows:

[0089] S301, sapphire substrate cleaning. First, ultrasonicate with ethanol and acetone for 15 minutes each, then soak with 80℃ dilute hydrochloric acid for 10 minutes, and finally soak with a mixed acid solution of H3PO4:H2SO4=1:3 at 100℃ for 10 minutes.

[0090] S302, placing the cleaned substrate into a growth chamber of a magnetron sputtering device, setting process parameters such as atmosphere and vacuum, and preparing a Ru / Ni / Ag / Pt / Au stacked first electrode;

[0091] S303, placing the substrate with the first electrode deposited thereon into the MOVPE reaction chamber, using trimethylgallium (TMGa), bismuth magnesium (Cp2Mg) and high-purity ammonia (NH3) as Ga, Mg and N sources respectively. High-purity hydrogen (H2) is used as the carrier gas. The sapphire substrate is baked at 1050°C in H2 atmosphere, nitrided in H2 / NH3 atmosphere, and grown at 550°C for 180 minutes to prepare a p-GaN:Mg conductive layer.

[0092] S304. Place the "substrate / first alloy metal film electrode / p-GaN (or p-ZnO) film" into the growth chamber of the PLD equipment, introduce O2 gas, the growth pressure is 1Pa, the growth temperature is 500°C, the distance between the substrate and the target is 45mm, the target is Ga2O3 with a Sn atomic percentage of 0.5at%, the growth time is 120min, and prepare n-β-Ga2O3:Sn conductive film.

[0093] S305, using mask technology, magnetron sputtering equipment, in n + -β-Ga2O3:Sn electron collection layer, prepare the second electrode to obtain "sapphire substrate / (Ru / Ni / Ag / Pt / Au) stacked first electrode / p-GaN:Mg conductive layer / n-β-Ga2O3:Sn conductive film / (Ti / Au) stacked second electrode" ultraviolet light detector.

[0094] S306, the photoelectric performance test of the β-Ga2O3-based pn heterojunction ultraviolet detector obtained in step S305 is performed. The results show that the device has a maximum responsivity near a wavelength of 254nm under a bias voltage of 0V, and when the wavelength is greater than 270nm, the responsivity value decreases slowly. Figure 2 As shown, it is indicated that the ultraviolet detector obtained by the present invention has a solar-blind characteristic.

[0095] In summary, the high-responsivity β-Ga2O3-based heterojunction self-powered ultraviolet detector in the present invention uses intrinsic β-Ga2O3 as a depletion layer and an absorption layer, and a MgO:Na (or K) film as a passivation layer. + -β-Ga2O3:Sn thin film is used as the electron collection layer, which makes the β-Ga2O3-based heterojunction solar-blind detector have higher responsivity. Compared with the existing β-Ga2O3-based heterojunction UV detector, the responsivity is increased by nearly 2 times, and it has the following advantages:

[0096] 1) When light is incident on intrinsic β-Ga2O3, since this film is not doped and the lattice distortion is small, the photogenerated carriers drift rapidly to the loop under the action of the built-in electric field, which reduces the recombination of photogenerated carriers and increases the short-circuit current and open-circuit voltage;

[0097] 2) Using MgO:Na (or K) film as a passivation layer reduces surface recombination;

[0098] 3) Using n + -β-Ga2O3:Sn film acts as an electron collection layer, which improves the electron collection efficiency.

[0099] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. Highly responsive β-Ga2O3 based heterojunction self-powered UV detector, characterized in that: The ultraviolet detector comprises a substrate, a first electrode, a p-type wide bandgap conductive film, an intrinsic β-Ga2O3 film depletion layer, an n-β-Ga2O3:Sn conductive film, and an n-β-Ga2O3:Sn conductive film. + -β-Ga2O3:Sn electron collection layer, MgO:Na or MgO:K thin film passivation layer and second electrode; wherein: The bandgap width of the p-type wide bandgap conductive film is greater than 3.0 eV; The intrinsic β-Ga2O3 film depletion layer is located between the p-type wide bandgap conductive film and the n-β-Ga2O3:Sn conductive film; The MgO:Na or MgO:K thin film passivation layer covers the n-β-Ga2O3:Sn conductive film; The + -β-Ga2O3:Sn electron collection layer is located between the n-β-Ga2O3:Sn conductive film and the second electrode; The first electrode is a Ru / Ni / Ag / Pt / Au laminated alloy film, wherein the thickness of Ru is 5-50nm, the thickness of Ni is 10-100nm, the thickness of Ag is 10-100nm, the thickness of Pt is 10-100nm, and the thickness of Au is 50-1000nm; The second electrode is a Ti / Au laminated alloy film, the thickness of Ti is 10-500nm, and the thickness of Au is 50-1000nm; The method for preparing the high-responsivity β-Ga2O3-based heterojunction self-powered ultraviolet detector comprises the following steps: S101, cleaning the substrate; S102, preparing a Ru / Ni / Ag / Pt / Au stacked alloy thin film as a first electrode on the cleaned substrate by vacuum magnetron sputtering; S103, preparing a p-type wide bandgap conductive film on the first electrode by a vacuum film forming method selected from metal organic vapor phase epitaxy, pulsed laser deposition, magnetron sputtering or molecular beam epitaxy; S104, preparing an intrinsic β-Ga2O3 thin film depletion layer on the p-type wide bandgap conductive film by pulsed laser deposition; S105, preparing an n-β-Ga2O3:Sn conductive film on the depletion layer of the intrinsic β-Ga2O3 film by pulsed laser deposition; S106, covering the n-β-Ga2O3:Sn conductive film with a mask plate, and preparing n-β-Ga2O3:Sn conductive film on the n-β-Ga2O3:Sn conductive film by pulsed laser deposition. + -β-Ga2O3:Sn electron collection layer; S107, vacuum film forming method using mask plate combined with magnetron sputtering in n + -Ti / Au stacked alloy film is prepared on the β-Ga2O3:Sn electron collection layer as the second electrode; S108, covering the second electrode with a mask plate, and preparing a MgO:Na or MgO:K thin film passivation layer on the n-β-Ga2O3:Sn conductive film by a vacuum film forming method using magnetron sputtering; The preparation process parameters of the intrinsic β-Ga2O3 thin film depletion layer include: introducing O2 gas, a growth pressure of 0.01-0.1Pa, a growth temperature of 380-650°C, a distance between the substrate and the target material of 20-50mm, and a growth time of 1-10min; The preparation process parameters of the n-β-Ga2O3:Sn conductive film include: introducing O2 gas, a growth pressure of 0.01-5Pa, a growth temperature of 350-950°C, a distance between the substrate and the target material of 20-50mm, and a growth time of 100-240min; The + - The preparation process parameters of the β-Ga2O3:Sn electron collection layer include: introducing O2 gas, the growth pressure is 0.01-5Pa, the growth temperature is 350-950℃, the distance between the substrate and the target is 20-50mm, and the growth time is 30-60min; The preparation process parameters of the MgO:Na or MgO:K thin film passivation layer include: introducing Ar and O2 mixed gas, and the volume ratio of Ar:O2 is 1:0.1-10, the growth pressure is 0.5-5Pa, the sputtering power is 10-80W, the growth temperature is 200-600℃, and the growth time is 20-120min.

2. The high-responsivity β-Ga2O3-based heterojunction self-powered ultraviolet detector according to claim 1, characterized in that: The substrate is selected from sapphire, silicon or metal material with a flat and smooth surface.

3. The high-responsivity β-Ga2O3-based heterojunction self-powered ultraviolet detector according to claim 1, characterized in that: The thickness of the intrinsic β-Ga2O3 thin film depletion layer is 5-50nm; And / or the Sn atomic percentage in the n-β-Ga2O3:Sn conductive film is 0.01at%-1at%, and the thickness is 300-2000nm.

4. The high-responsivity β-Ga2O3-based heterojunction self-powered ultraviolet detector according to claim 1, characterized in that: The + -β-Ga2O3:Sn electron collection layer is a strip structure, wherein the Sn atomic percentage is 1at%-10at%, and the thickness is 50-500nm.

5. The high-responsivity β-Ga2O3-based heterojunction self-powered ultraviolet detector according to claim 1, characterized in that: The p-type wide bandgap conductive film is selected from one or more of p-GaN, p-SiC, and p-ZnO conductive films.

6. The high-responsivity β-Ga2O3-based heterojunction self-powered ultraviolet detector according to claim 1, characterized in that: The thickness of the MgO:Na or MgO:K thin film passivation layer is 50-500nm, and the atomic percentage of Na or K is 0.1at%-5at%.

7. Application of the high-responsivity β-Ga2O3-based heterojunction self-powered ultraviolet detector according to any one of claims 1 to 6 in detection in the solar-blind band.

Citation Information

Patent Citations

  • MPS diode of n-type gallium oxide and p-type diamond and preparation method thereof

    CN114823919A

  • Photoelectric conversion element and method for manufacturing the same

    JP2014209538A