A bonding test structure suitable for micron-level metal bump array and preparation method
By designing a bonding test structure suitable for micron-level metal convex dot arrays, the bond yield and reliability test is simplified by using the four-probe test method, solving the problems of complex and low efficiency in the existing technology, and achieving rapid and Accurate test results.
Patent Information
- Application Number
- CN202210960149.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-11
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-08-11
AI Technical Summary
In the prior art, the flip chip bonding yield and reliability test scheme is complex and inefficient, and the detection means and equipment are expensive and inefficient.
A structure suitable for bonding test of micron-level metal convex dot arrays is designed, including top and bottom modules, and a transparent dielectric layer with hollow hole arrays and micron-level metals are prepared by magnetron sputtering, plasma chemical vapor deposition and other processes. and four-probe testing method is used to determine bond yield and reliability.
The test structure and methods are simplified, which significantly saves test time and cost, improves test accuracy, and reduces the error impact caused by the probe resistance value.
Smart Images

Figure CN115346961B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductor packaging, and in particular to a bonding test structure suitable for a micron-level metal bump array and a preparation method thereof. Background Art
[0002] Flip-Chip bonding (FC) technology refers to the preparation of a metal bump structure on one side of the chip active area, and then face down to achieve a stable and reliable mechanical and electrical connection with the substrate through the metal bump. As an advanced packaging process, FC technology realizes chip packaging technology with smaller packaging size, higher integration and stronger performance, and has important research value in the fields of Micro-LED micro-display, 3D integrated packaging, etc. However, the existing technology for flip-chip bonding yield and reliability testing is relatively complicated, and the main detection methods include X-ray technology, optical detection, and scanning ultrasonic microscopy. These detection methods are not only expensive, but also inefficient. Summary of the invention
[0003] In view of this, the purpose of the present invention is to provide a bonding yield and reliability test structure suitable for a micron-level metal bump array and a preparation method thereof, which can quickly determine the bonding yield of the micron-level metal bumps and perform reliability testing.
[0004] To achieve the above object, the present invention adopts the following technical solution:
[0005] A bonding test structure suitable for a micron-scale metal bump array comprises a top module and a bottom module; the top module comprises a first insulating substrate, a first patterned bottom metal layer, a first transparent medium layer having a hollow hole array, and a first micron-scale metal bump; the bottom module comprises a second insulating substrate, a second patterned bottom metal layer, a metal electrode, a second transparent medium layer having a hollow hole array, and a second micron-scale metal bump.
[0006] Furthermore, the first patterned bottom metal layer is arranged on the surface of the first insulating substrate; the first transparent medium layer having a hollow hole array is arranged on the surfaces of the first insulating substrate and the first patterned bottom metal layer, and the hollow hole array of the first transparent medium layer is located on the surface of the first patterned bottom metal layer; the first micron-sized metal bumps are vertically arranged on the hollow hole array of the first transparent medium layer and the surface of the first patterned bottom metal layer, and are tightly connected to the patterned bottom metal layer.
[0007] Furthermore, the second patterned bottom metal layer is arranged on the surface of the second insulating substrate; the metal electrode is led out from the second patterned bottom metal layer and arranged on the surface of the second insulating substrate; the second transparent medium layer having a hollow hole array is arranged on the second insulating substrate and the surface of the second patterned bottom metal layer, and the hollow hole array of the second transparent medium layer is located on the surface of the patterned bottom metal layer; the second micron-sized metal bumps are vertically arranged on the hollow hole array of the second transparent medium layer and the surface of the second patterned bottom metal layer, and are tightly connected to the second patterned bottom metal layer.
[0008] Furthermore, the area of the first insulating substrate is smaller than the area of the second insulating substrate.
[0009] Furthermore, the first patterned bottom metal layer includes a plurality of bottom metal layers, and the first micron-level metal bumps include a plurality of pairs of metal bumps; the top-level module is a repetitive array structure with a bottom metal layer connecting a pair of metal bumps as a unit; the bottom metal layer has a width greater than or equal to the diameter of the metal bump, and a length greater than the sum of the diameters of the two metal bumps.
[0010] Furthermore, the second patterned bottom metal layer includes several bottom metal layers, and the second micron-level metal bumps include several pairs of metal bumps; the bottom module is composed of a repetitive array structure with a bottom metal layer connecting a pair of metal bumps as a unit, a starting point metal bump structure, an end point metal bump structure and a test electrode; the starting point metal bump structure is composed of a bottom metal layer, a metal bump, a voltage input electrode and a current input electrode; the end point metal bump structure is composed of a bottom metal layer, a metal bump, a voltage output electrode and a current output electrode; the test electrodes are distributed at the end point positions of each column of metal bumps in the bottom module, and the voltage output electrode and the current output electrode are led out from the bottom metal layer.
[0011] Furthermore, the length and width of the first transparent medium and the second transparent medium layer with the hollow hole array are consistent with the size of the insulating substrate of the top module; the hollow hole array is composed of a number of circular openings of consistent size, with a diameter smaller than the width of the bottom metal layer and greater than or equal to the diameter of the metal bump.
[0012] Furthermore, the insulating substrate includes a quartz glass substrate and a sapphire substrate; the patterned base metal layer and the metal electrode include one or a combination of more than two of Cr, Al, Ti, Pt, Au, and Ag; the transparent dielectric layer includes one or a combination of more than two of SiO2, AlN, Al2O3, Si3N4, BN, and TiO2; and the micron-scale metal bumps include one or a combination of more than two of In, Cu, Sn, Ni, and Ag.
[0013] Furthermore, the thickness of the first and second base metal layers are both 500nm-2μm; the thickness of the first and second transparent medium layers are both 300nm-1μm; the diameter of the first and second micron-level metal bumps are both 3um-300um; the height of the first and second micron-level metal bumps are both 2um-500um.
[0014] A method for preparing a micron-scale metal bump array bonding test structure comprises the following steps:
[0015] S1, scribing, cleaning and drying the first and second insulating substrates;
[0016] S2, using magnetron sputtering or thermal evaporation process to prepare a first patterned bottom metal layer on the first insulating substrate of the top module, and a second patterned bottom metal layer and a metal electrode on the second insulating substrate prepared in the bottom module;
[0017] S3, using plasma enhanced chemical vapor deposition or atomic layer deposition to prepare a transparent dielectric layer having a hollow hole array on the transparent dielectric layer of the top module and the bottom module respectively;
[0018] S4, using chemical plating, electroplating or thermal evaporation process to prepare micron-level metal bumps on the top module and the bottom module respectively;
[0019] S5. Use the four-probe test method to test whether the resistance values of the first column, the first two columns, the first three columns...the Nth column increase in equal proportion to determine the bonding yield; after the test sample has been subjected to long-term current excitation, the resistance value is tested again and compared with the initial test result to determine the bonding reliability.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] 1. The test structure of the present invention has a simple preparation process and a simple test method. It can be combined with existing test methods to perform bonding yield and reliability tests, greatly saving test time and cost;
[0022] 2. The present invention adopts a four-probe test method to test the resistance value, which can effectively reduce the error influence caused by the resistance value of the test probe and improve the test accuracy. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a schematic diagram of the structure of the present invention;
[0024] Figure 2 It is a schematic diagram of the preparation process in one embodiment of the present invention;
[0025] Figure 3 It is a flow chart of the preparation method of the present invention;
[0026] In the figure, 100-top module, 101-insulating substrate of the top module, 102-transparent dielectric layer with hollow array of the top module, 103-bottom metal layer of the top module, 104-micron-scale metal bumps of the top module, 200-bottom module, 201-insulating substrate of the bottom module, 202-transparent dielectric layer with hollow array of the bottom module, 203-bottom metal layer of the bottom module, 204-micron-scale metal bumps of the bottom module, 205-metal electrodes of the bottom module. DETAILED DESCRIPTION
[0027] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.
[0028] Please refer to Figure 1 The present invention provides a bonding test structure suitable for a micron-scale metal bump array, comprising a top-level module 100, an insulating substrate 101 of the top-level module, a bottom metal layer 102 of the top-level module, a transparent medium layer 103 with a hollow array of the top-level module, micron-scale metal bumps 104 of the top-level module, a bottom-level module 200, an insulating substrate 201 of the bottom-level module, a bottom metal layer 202 of the bottom-level module, a transparent medium layer 203 with a hollow array of the bottom-level module, micron-scale metal bumps 204 of the bottom-level module, and a metal electrode 205 of the bottom-level module.
[0029] Reference Figure 2 In this embodiment, a method for preparing a structure suitable for testing the bonding yield and reliability of a micron-level metal bump array is also provided, comprising the following steps:
[0030] S1, providing an insulating substrate 101 of a top module and an insulating substrate 102 of a bottom module, dicing, cleaning and drying them;
[0031] In this embodiment, a sapphire substrate is selected as the insulating substrate, and the RCA standard cleaning method is used to clean the sample. The cleaning process is as follows: the first step is to use an SPM solution (the volume ratio of H2SO4 to H2O2 is 1:3) to clean the insulating substrate at a temperature of 100~130°C for 15 minutes; the second step is to place the insulating substrate in an APM solution (the volume ratio of H2SO4:H2O2:H2O is 1:2:7), and take it out after cleaning it at a temperature of 65~80°C for 10 minutes; the third step is to put the taken out insulating substrate into a solution (HF:H2O volume ratio is 1:10) and clean it at a temperature of 20~25°C for 10 minutes, then take it out and rinse it with water for use; finally, use an HPM reagent (HCl:H2O2:H2O volume ratio is 1:2:8) to clean it at a temperature of 65~80°C for 15 minutes, and finally rinse it with deionized water for 20 minutes.
[0032] S2, using magnetron sputtering or thermal evaporation process to prepare a patterned bottom metal layer 102 on the top module, and prepare a bottom metal layer 202 and a metal electrode 205 on the bottom module;
[0033] In this embodiment, magnetron sputtering is preferably used to prepare the base metal layer structure. First, a patterned photolithography mask layer is formed on the insulating substrate of the top module and the insulating substrate of the bottom module using a photolithography process. Then, a Ti base metal layer with a thickness of 150 nm is sputtered in the sputtering chamber of the magnetron sputtering equipment. After the metal deposition is completed, an acetone solution is used to strip the photoresist, forming a patterned base metal layer on the insulating substrate of the top module, and forming a patterned base metal layer and a metal electrode on the insulating substrate of the bottom module.
[0034] S3, forming a transparent medium layer 103 having a hollow array on the top module by using a plasma chemical vapor deposition method or an atomic layer deposition method, and forming a transparent medium layer 203 having a hollow array on the bottom film block;
[0035] In this embodiment, a plasma chemical vapor deposition method is preferably used to prepare a transparent dielectric layer having a hollow hole array. Two insulating substrates are placed in a machine with SiH4 and N2O gases to grow a 1μm thick SiO2 transparent dielectric layer. A photolithography process is then used to form a patterned photolithography mask layer on the surface of the dielectric layer. The insulating substrate that has completed the photolithography process is then placed in the chamber of an ICP etching device for etching. Finally, a hollow hole array is formed on the dielectric layer of the top module, and a hollow hole array is formed on the dielectric layer of the bottom module and the metal electrode is exposed.
[0036] S4, using chemical plating, electroplating or thermal evaporation process to prepare micron-sized metal bumps 104 on the top module and micron-sized metal bumps 204 on the bottom module;
[0037] In this embodiment, a thermal evaporation process is preferably used to prepare indium balls with a diameter and height of 10 um on the top module and the bottom module. First, a patterned photolithography mask layer is formed on the insulating substrate of the top module and the insulating substrate of the bottom module using a photolithography process, and then placed in a evaporation chamber for indium bump evaporation. After the evaporation is completed, the photoresists of the two are stripped with an acetone solution, and then placed in a vacuum chamber with formic acid for high-temperature reflux to form balls.
[0038] Please refer to Figure 3 , is the test principle diagram of the present invention. The specific test principle is as follows:
[0039] (1) If Figure 3In 3-1, the two pairs of metal bumps of the test module are bonded and tested using the four-probe test method. Pins a and d are used as current input and output ports, respectively, and pins b and c are connected to the positive and negative poles of the voltmeter, respectively. The current flows from pin a into the metal bump, passes through the bottom metal layer of the top module, flows back to the other metal bump, and then flows out from pin d. The voltage value measured in this process is the ratio of the current value flowing in, which is the resistance value of the bump after bonding.
[0040] (2) If Figure 3 As described in 3-2, after the metal bump array is made and bonded, the working principle is similar to that of the test module. It is only necessary to connect one end of the two electrodes at the initial position 0 to the positive pole of the voltmeter and the other end as the current input port, and connect one pin at the end of a certain column of resistance to be measured to the negative pole of the voltmeter and the other pin as the current output port. The current can flow through all the metal bumps of these types, and then calculate the sum of the resistance values of these columns. Compared with the first column or the test module, the bonding yield can be fed back. After the test module is subjected to long-term current excitation, the metal bumps will produce a series of phenomena such as voids, and then the resistance value is measured again. Compared with the original data, the reliability of the metal bumps is judged based on the change in resistance value.
[0041] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.
Claims
1. A bonding test structure suitable for micron-scale metal bump arrays, It is characterized in that It comprises a top module and a bottom module; the top module comprises a first insulating substrate, a first patterned bottom metal layer, a first transparent medium layer having a hollow hole array, and a first micron-scale metal bump; the bottom module comprises a second insulating substrate, a second patterned bottom metal layer, a metal electrode, a second transparent medium layer having a hollow hole array, and a second micron-scale metal bump; The first patterned bottom metal layer is disposed on the surface of the first insulating substrate; the first transparent medium layer having a hollow hole array is disposed on the surfaces of the first insulating substrate and the first patterned bottom metal layer, and the hollow hole array of the first transparent medium layer is located on the surface of the first patterned bottom metal layer; the first micron-sized metal bump is vertically disposed on the hollow hole array of the first transparent medium layer and the surface of the first patterned bottom metal layer, and is tightly connected to the patterned bottom metal layer; The second patterned bottom metal layer is arranged on the surface of the second insulating substrate; the metal electrode is led out from the second patterned bottom metal layer and arranged on the surface of the second insulating substrate; the second transparent medium layer having a hollow hole array is arranged on the second insulating substrate and the surface of the second patterned bottom metal layer, and the hollow hole array of the second transparent medium layer is located on the surface of the patterned bottom metal layer; the second micron-sized metal bump is vertically arranged on the hollow hole array of the second transparent medium layer and the surface of the second patterned bottom metal layer, and is tightly connected to the second patterned bottom metal layer; The area of the first insulating substrate is smaller than the area of the second insulating substrate; The first patterned bottom metal layer includes a plurality of bottom metal layers, and the first micron-scale metal bumps include a plurality of pairs of metal bumps; the top module is a repetitive array structure with a bottom metal layer connecting a pair of metal bumps as a unit; the bottom metal layer has a width greater than or equal to a diameter of a metal bump, and a length greater than the sum of the diameters of two metal bumps; The second patterned bottom metal layer includes a plurality of bottom metal layers, and the second micron-level metal bumps include a plurality of pairs of metal bumps; the bottom module is composed of a repetitive array structure with a bottom metal layer connecting a pair of metal bumps as a unit, a start-end metal bump structure, a terminal metal bump structure, and a test electrode; the start-end metal bump structure is composed of a bottom metal layer, a metal bump, a voltage input electrode, and a current input electrode; the terminal metal bump structure is composed of a bottom metal layer, a metal bump, a voltage output electrode, and a current output electrode; the test electrode is distributed at the end point position of each column of metal bumps in the bottom module, and the voltage output electrode and the current output electrode are led out from the bottom metal layer; The length and width of the first transparent medium and the second transparent medium layer with the hollow hole array are consistent with the size of the insulating substrate of the top module; the hollow hole array is composed of a number of circular openings of the same size, the diameter of which is smaller than the width of the bottom metal layer and greater than or equal to the diameter of the metal bump.
2. A bonding test structure suitable for micron-scale metal bump arrays according to claim 1, It is characterized in that The insulating substrate includes a quartz glass substrate and a sapphire substrate; the patterned base metal layer and the metal electrode include one or a combination of two or more of Cr, Al, Ti, Pt, Au, and Ag; the transparent medium layer includes one or a combination of two or more of SiO2, AlN, Al2O3, Si3N4, BN, and TiO2; the micron-scale metal bumps include one or a combination of two or more of In, Cu, Sn, Ni, and Ag.
3. A bonding test structure suitable for micron-scale metal bump array according to claim 1, It is characterized in that The thickness of the first and second base metal layers are both 500nm-2μm; the thickness of the first and second transparent medium layers are both 300nm-1μm; the diameter of the first and second micron-level metal bumps are both 3um-300um; the height of the first and second micron-level metal bumps are both 2um-500um.
4. A method for preparing a micron-scale metal bump array bonding test structure as claimed in any one of claims 1 to 3, It is characterized in that The following steps are involved: S1, scribing, cleaning and drying the first and second insulating substrates; S2, using magnetron sputtering or thermal evaporation process to prepare a first patterned bottom metal layer on the first insulating substrate of the top module, and a second patterned bottom metal layer and a metal electrode on the second insulating substrate prepared in the bottom module; S3, using plasma enhanced chemical vapor deposition or atomic layer deposition to prepare a transparent dielectric layer having a hollow hole array on the transparent dielectric layer of the top module and the bottom module respectively; S4, using chemical plating, electroplating or thermal evaporation process to prepare micron-level metal bumps on the top module and the bottom module respectively; S5. Use the four-probe test method to test whether the resistance values of the first column, the first two columns, the first three columns...the Nth column increase in equal proportion to determine the bonding yield; after the test sample has been subjected to long-term current excitation, the resistance value is tested again and compared with the initial test result to determine the bonding reliability.