Foamable adhesive sheet and method for producing article
By using a high peeling force adhesive and an intermediate layer in the foam adhesive sheet, the problem of floating of the adhesive layer during bending and cutting is solved, the adhesion and operability are improved, and it is suitable for heat-resistant applications. Bonding applications to substrates.
Patent Information
- Application Number
- CN202180023191.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-03-25
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-03-25
AI Technical Summary
The adhesive layer of the existing foam adhesive sheet is easy to float and peel off during the bending and cutting process, and because it contains a foaming agent, the adhesive layer has low adhesion and poor operability and workability, especially This is because the adhesion is even more insufficient when using a heat-resistant base material.
A foamed adhesive sheet with an adhesive layer side peeling force of 2.0N or more measured by the SAICAS method. It contains a curable adhesive and a foaming agent, and has an intermediate layer on the base material to improve adhesion and heat resistance. properties, the adhesive layer is non-adhesive to improve operability.
It achieves high adhesion between the adhesive layer and the base material, suppresses the floating and peeling of the adhesive layer during bending and cutting, improves operability and workability, and maintains good adhesion on the heat-resistant base material. performance.
Smart Images

Figure CN115348998B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a foamable adhesive sheet and a method for producing an article using the foamable adhesive sheet. Background Art
[0002] Adhesives for bonding members to each other are used in various fields, and various bonding methods are known.
[0003] For example, adhesive sheets containing foaming agents (foamable adhesive sheets) are disclosed in Patent Documents 1 and 2. Patent Document 1 discloses an adhesive sheet having expandable adhesive layers on both sides or one side of a substrate, the expandable adhesive layers containing epoxy resins including multifunctional epoxy resins, phenolic resins as curing agents, imidazole compounds as curing catalysts, and thermosensitive foaming agents, and a release agent is applied on the surface of at least one expandable adhesive layer. In addition, Patent Document 2 discloses an adhesive sheet having a substrate, heat-expandable adhesive layers disposed on both sides of the substrate, and adhesive permeable layers disposed on the surfaces of each adhesive layer and through which the adhesive can permeate when the adhesive thermally expands.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: International Publication No. 2016 / 163514
[0007] Patent Document 2: Japanese Patent Application Publication No. 2019-203062 Summary of the invention
[0008] Problems to be solved by the invention
[0009] As a method of using a foamable adhesive sheet, for example, a method of placing the foamable adhesive sheet between members and then foaming and curing the foamable adhesive sheet to bond the members to each other is known.
[0010] In the case where the foamable adhesive sheet has an adhesive layer on one or both sides of the substrate, the adhesive layer sometimes floats and peels off from the substrate during the processing steps such as bending the foamable adhesive sheet or cutting the foamable adhesive sheet. In addition, when there are burrs on the components, the foamable adhesive sheet is inserted into the gap between the components or the gap between the components, or another component is inserted into the gap after the foamable adhesive sheet is arranged in one component, because the foamable adhesive sheet is hooked on the burrs of the components, the adhesive layer sometimes floats and peels off from the substrate. Therefore, in the foamable adhesive sheet, it is desired to further improve the adhesion of the adhesive layer to the substrate.
[0011] However, in the foamable adhesive sheet, since a foaming agent is contained in the adhesive layer, there is a tendency that the adhesion of the adhesive layer decreases compared to the adhesive layer without a foaming agent. In addition, in order to improve operability and workability, it is desired that the adhesive layer before the foaming and curing is non-adhesive (non-viscous), but in this case, there is a tendency that the adhesion of the adhesive layer decreases. In addition, for example, when the adhesive layer is foamed and cured by heating, a substrate with heat resistance is used, but usually most of the heat-resistant substrates have low adhesion.
[0012] The present invention has been made in view of the above-mentioned actual situation, and a main object of the present invention is to provide a foamable adhesive sheet having an adhesive layer having excellent adhesion to a substrate.
[0013] Means for solving problems
[0014] One embodiment of the present invention provides a foamable adhesive sheet, which has a substrate and an adhesive layer disposed on at least one side of the substrate, the adhesive layer contains a curable adhesive and a foaming agent, and the peeling force of the side on which the adhesive layer is disposed measured by the SAICAS method is 2.0 N or more. It should be noted that, hereinafter, the surface and interface cutting analysis system (Surface And Interfacial Cutting Analysis System) is referred to as SAICAS.
[0015] Another embodiment of the present invention provides a method for manufacturing an article, comprising: a placement step of placing the foamable adhesive sheet between a first member and a second member; and a bonding step of foaming and curing the foamable adhesive sheet to bond the first member to the second member.
[0016] Effects of the Invention
[0017] The foamable adhesive sheet in the present invention exerts an effect that the adhesive layer has excellent adhesion to the substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a schematic cross-sectional view showing an example of the foamable adhesive sheet in the present invention.
[0019] Figure 2 This is a schematic cross-sectional view showing another example of the foamable adhesive sheet in the present invention.
[0020] Figure 3 This is a schematic cross-sectional view showing another example of the foamable adhesive sheet in the present invention.
[0021] Figure 4 It is a schematic perspective view showing another example of the foamable adhesive sheet in the present invention.
[0022] Figure 5This is a schematic cross-sectional view showing an example of a method for producing an article in the present invention.
[0023] Figure 6 It is a schematic cross-sectional view for explaining the test method of adhesion. DETAILED DESCRIPTION
[0024] Hereinafter, the embodiments of the present invention will be described with reference to the accompanying drawings, etc. However, the present invention can be implemented in a variety of different ways and should not be construed as being limited to the contents of the embodiments described below. In addition, in order to make the description clearer, the drawings sometimes schematically show the width, thickness, shape, etc. of each part compared to the actual method, but this is only an example and does not limit the interpretation of the present invention. In addition, in this specification and each figure, the same elements as those described previously with respect to the figures that have already appeared are sometimes marked with the same figure numbers, and the detailed description is appropriately omitted.
[0025] In this specification, when expressing the manner of arranging other members on a certain member, if it is simply expressed as "above" or "below", unless otherwise specified, it is assumed that the following two situations are included: the situation where other members are arranged directly above or directly below in a manner of contacting with a certain member, and the situation where other members are arranged above or below a certain member with another member further interposed therebetween. In addition, in this specification, when expressing the manner of arranging other members on the surface of a certain member, if it is simply expressed as "on the surface side" or "on the surface", unless otherwise specified, it includes the situation where other members are arranged directly above or directly below in a manner of contacting with a certain member, and the situation where other members are arranged above or below a certain member with another member further interposed therebetween.
[0026] In this specification, a “sheet” also includes a member called a “film.” In addition, a “film” also includes a member called a “sheet.” In addition, the numerical range in this specification is a range of average values.
[0027] The inventor of the present invention etc. has carried out in-depth research on the adhesion of adhesive layer to substrate in the foaming adhesive sheet with adhesive layer on one side or both sides of substrate.For example, in patent documentation 1, about the evaluation of adhesion of adhesive layer to substrate, disclose the evaluation of adhesion based on the L word bending test of bending the foaming adhesive sheet 90 ° once into L font.But, as mentioned above, in foaming adhesive sheet, the requirement level of adhesion of adhesive layer to substrate is high, therefore it is clear that only the adhesion based on L word bending test is not sufficient, sometimes can not tolerate practical.In addition, the inventor of the present invention etc. has been studied repeatedly, and it is found that, in order to obtain the foaming adhesive sheet that can tolerate practicality, it is necessary to meet the adhesion based on the adhesion test under the condition stricter than L word bending test, specifically for the adhesion of the cross bending test of bending the foaming adhesive sheet 180 ° twice into cross-shaped as described later. It was also found that in a foamable adhesive sheet, by making the peeling force of the surface on the adhesive layer side measured by the SAICAS method to be above a predetermined value, not only the adhesion based on the L-shaped bending test but also the adhesion based on the cross bending test can be satisfied, and a foamable adhesive sheet that can withstand practical use can be obtained. The present invention is based on such knowledge.
[0028] Hereinafter, the foamable adhesive sheet and the method for producing an article using the foamable adhesive sheet in the present invention will be described in detail.
[0029] A. Foam adhesive sheet
[0030] The foamable adhesive sheet of the present invention comprises a substrate and an adhesive layer disposed on at least one surface of the substrate, wherein the adhesive layer contains a curable adhesive and a foaming agent, and the peeling force of the surface on which the adhesive layer is disposed measured by the SAICAS method is 2.0 N or more.
[0031] Figure 1 and Figure 2 This is a schematic cross-sectional view illustrating the foamable adhesive sheet in the present invention. Figure 1 The foamable adhesive sheet 10 in the embodiment includes a substrate 2 and an adhesive layer 1 disposed on one surface side of the substrate 2 . Figure 2 The foamable adhesive sheet 10 includes a substrate 2, a first adhesive layer 1a disposed on one surface of the substrate 2, and a second adhesive layer 1b disposed on the other surface of the substrate 2. The adhesive layer 1, the first adhesive layer 1a, and the second adhesive layer 1b contain a curable adhesive and a foaming agent. Figure 1 The peeling force of the foamable adhesive sheet 10 on the surface on which the adhesive layer 1 is disposed measured by the SAICAS method is greater than or equal to a predetermined value. Figure 2The peeling force of the surface side provided with the first adhesive layer 1a and the peeling force of the surface side provided with the second adhesive layer 1b measured by the SAICAS method of the foaming adhesive sheet 10 are above the prescribed value. It should be noted that, in the case where the foaming adhesive sheet has adhesive layers on both sides, it is preferred that the peeling force of both sides is above the prescribed value, but the foaming adhesive sheet in the present invention can sometimes be used by paying attention to the bending direction and the direction in which the surface faces, so it is sufficient as long as the peeling force of any one side is above the prescribed value.
[0032] In the foamable adhesive sheet of the present invention, the peeling force of the face side of the adhesive layer measured by the SAICAS method is more than the specified value, so the foamable adhesive sheet with excellent adhesion of the adhesive layer to the base material can be made. Specifically, as described later, the foamable adhesive sheet of the present invention can not only meet the adhesion based on the L-shaped bending test, but also meet the adhesion based on the cross bending test. Therefore, for example, when the foamable adhesive sheet is configured between components, even when the foamable adhesive sheet is bent, the generation of the adhesive layer floating from the base material and peeling off can be suppressed. In addition, when the foamable adhesive sheet is configured between components, even when there is burr in the component, the generation of the adhesive layer floating from the base material and peeling off can be suppressed. Therefore, a foamable adhesive sheet that can withstand practicality can be provided.
[0033] Hereinafter, each structure of the foamable adhesive sheet in the present invention will be described.
[0034] 1. Characteristics of foam adhesive sheets
[0035] In the foamable adhesive sheet of the present invention, the peeling force of the face side of the adhesive layer measured by the SAICAS method is more than 2.0N, can be more than 3.0N, can be more than 3.5N, can also be more than 4.0N. In addition, the peeling force of the face side of the adhesive layer of the above-mentioned foamable adhesive sheet is, for example, less than 6.0N, can be less than 5.5N, can also be less than 5.0N. By making the peeling force of the face side of the adhesive layer of the above-mentioned foamable adhesive sheet be within the above-mentioned range, the foamable adhesive sheet with excellent adhesion of the adhesive layer to the substrate can be made. In addition, the higher the adhesion of the adhesive layer to the substrate, the more preferred, but the material of the adhesive layer whose peeling force of the face side of the adhesive layer of the above-mentioned foamable adhesive sheet becomes large has a trend of being difficult to cut.
[0036] When adhesive layers are disposed on both sides of the substrate, as described above, the release force on either side of the foamable adhesive sheet may be within the above range, and preferably the release force on both sides of the foamable adhesive sheet is within the above range.
[0037] The peeling force of the face side of the foaming adhesive sheet with the adhesive layer can be carried out based on the SAICAS method. The SAICAS method is also referred to as the surface interface cutting method, etc. When the peeling force of the face side of the foaming adhesive sheet with the adhesive layer is measured by the SAICAS method, first, the cutting edge is contacted with the face of the adhesive layer side of the foaming adhesive sheet, and the cutting edge is relatively moved at a constant speed relative to the foaming adhesive sheet in the horizontal direction and the vertical direction at the same time to cut. That is, the cutting edge is used to cut into the adhesive layer obliquely. Next, if the cutting edge reaches a prescribed depth above the thickness of the adhesive layer from the face of the adhesive layer side of the foaming adhesive sheet, it is observed that the force applied to the cutting edge changes greatly, and the horizontal force applied to the cutting edge is reduced. At this moment, the cutting edge is relatively moved only in the horizontal direction relative to the foaming adhesive sheet and cut. The horizontal force applied to the cutting edge when the cutting edge is relatively moved only in the horizontal direction relative to the foaming adhesive sheet and cuts is equivalent to the peeling force of the face side of the foaming adhesive sheet with the adhesive layer. In the present invention, the peeling force is set to 2.0 N or more.
[0038] It should be noted that, in the foaming adhesive sheet of the present invention, for example, there is a case where an adhesive layer is directly arranged on the substrate, and as described later, there is a case where an intermediate layer is arranged between the substrate and the adhesive layer. In either case, after the cutting edge is relatively moved at a constant speed in the horizontal direction and the vertical direction relative to the foaming adhesive sheet to cut, at the moment when a large change in the force applied to the cutting edge is observed and the horizontal force applied to the cutting edge is reduced, the cutting edge is relatively moved only in the horizontal direction relative to the foaming adhesive sheet to cut. In this case, the interface when the cutting edge is relatively moved only in the horizontal direction relative to the foaming adhesive sheet to cut becomes the interface between the adhesive layer and the layer adjacent to the adhesive layer, or the interface between the adhesive layer and the substrate, and this interface easily becomes a peeling interface.
[0039] The details of the method for measuring the peeling force of the surface of the foamable adhesive sheet on which the adhesive layer is disposed based on the SAICAS method are described in the section of Examples described later.
[0040] In the present invention, the peeling force of the surface side of the foaming adhesive sheet provided with the adhesive layer measured by the SAICAS method can be set to a predetermined value or more by, for example, disposing an intermediate layer between the substrate and the adhesive layer, subjecting the surface of the substrate provided with the adhesive layer to a surface treatment, adjusting the composition of the adhesive layer, adjusting the average thickness of the adhesive layer, or adjusting the combination of materials of the substrate, the intermediate layer and the adhesive layer.
[0041] For example, as described later, by disposing an intermediate layer between the substrate and the adhesive layer or performing a surface treatment on the surface of the substrate on which the adhesive layer is disposed, the adhesion of the adhesive layer to the substrate can be improved, thereby improving the above-mentioned peeling force.
[0042] In addition, when adjusting the composition of the adhesive layer, for example, by containing a polymer component with a soft structure in the adhesive layer containing epoxy resin and a curing agent, the flexibility and toughness of the adhesive layer can be improved, the adhesion of the adhesive layer to the base material can be improved, and the above-mentioned peeling force can be improved. As the above-mentioned polymer component with a soft structure, specifically, as described later, an acrylic resin compatible with epoxy resin can be enumerated. In addition, for example, in the adhesive layer containing epoxy resin and a curing agent, by not containing the component that reduces toughness, the reduction of the toughness of the adhesive layer can be suppressed, the adhesion of the adhesive layer to the base material can be improved, and the above-mentioned peeling force can be improved. As the component that reduces the above-mentioned toughness, specifically, as described later, a phenolic resin can be enumerated. In addition, for example, by increasing the molecular weight of the component contained in the adhesive layer, the viscosity and cohesion of the adhesive layer can be improved, the adhesion of the adhesive layer to the base material can be improved, and the above-mentioned peeling force can be improved. Specifically, the molecular weight of at least one of the epoxy resin and the curing agent is increased in an adhesive layer containing the epoxy resin and the curing agent, or the molecular weight of at least one of the epoxy resin, the acrylic resin and the curing agent is increased in an adhesive layer containing the epoxy resin, the acrylic resin and the curing agent.
[0043] Furthermore, when adjusting the average thickness of the adhesive layer, for example, as described later, by increasing the average thickness of the adhesive layer, the adhesion of the adhesive layer to the substrate can be improved, and the above-mentioned peeling force can be improved.
[0044] In addition, when adjusting the combination of materials of the substrate, the intermediate layer and the adhesive layer, for example, as described later, when the substrate contains polyphenylene sulfide or polyethylene, the intermediate layer contains a cross-linked polyester resin, and the adhesive layer contains an epoxy resin and a curing agent, there is a tendency for the adhesion of the adhesive layer to the substrate to become higher, which can improve the above-mentioned peeling force.
[0045] In the foamable adhesive sheet in the present invention, it is preferred that the adhesive layer is substantially non-adhesive (non-tack). In this case, it is preferred that the adhesive layer is configured at the outermost surface. By the adhesive layer being substantially non-adhesive (non-tack), it is possible to make a foamable adhesive sheet with good slidability and anti-blocking properties. Therefore, it is possible to improve the operability and workability of the foamable adhesive sheet. Specifically, when the foamable adhesive sheet is configured between components and components are bonded to each other, the foamable adhesive sheet can be smoothly inserted in the gap between components, the gap between components, or another component can be smoothly inserted in the gap after the foamable adhesive sheet is configured in a component.
[0046] Here, the term "non-adhesive" is generally used to mean low adhesive strength. In the present invention, "non-adhesive" means a state in which the foamable adhesive sheet is rolled up and then easily unrolled without resistance.
[0047] In addition, "adhesion" is a concept included in "bonding". Sometimes there is a difference in the following point: adhesion is used to mean a temporary bonding phenomenon, while bonding is used to mean a substantially permanent bonding phenomenon (Iwanami Shoten Physical and Chemical Dictionary 5th edition). "Adhesion" and "adhesive force" refer to the property of bonding by pressure sensitivity and the adhesive force at that time.
[0048] It should be noted that, in this specification, unless otherwise specified, "the adhesiveness of the adhesive layer" and "the adhesive strength of the adhesive layer" refer to the adhesiveness and adhesive strength of the adhesive layer before foaming and curing. In addition, in this specification, unless otherwise specified, "the adhesiveness of the adhesive layer" and "the adhesive strength of the adhesive layer" refer to the adhesiveness and adhesive strength of the adhesive layer after foaming and curing.
[0049] When the adhesive layer is substantially non-adhesive, specifically, the adhesive force of the adhesive layer is preferably 0 N / 25 mm or more and 0.1 N / 25 mm or less, and may be 0.05 N / 25 mm or less, or 0.02 N / 25 mm or less. When the adhesive force of the adhesive layer is within the above range, the adhesive layer can be substantially non-adhesive, and a foamable adhesive sheet with good sliding properties and anti-blocking properties can be prepared.
[0050] For example, Patent Document 1 discloses that a release layer is provided on the surface of an expandable adhesive layer. However, if a release layer is provided on the surface of an adhesive layer, the adhesiveness of the adhesive layer after foaming and curing may be reduced. In contrast, a foamable adhesive sheet whose adhesive layer is substantially non-adhesive does not need to be provided with a release layer or a release sheet for the purpose of imparting anti-adhesion and sliding properties, and the adhesive layer can be provided on the outermost surface. Therefore, a foamable adhesive sheet with good adhesiveness of the adhesive layer after foaming and curing can be made.
[0051] In the case where adhesive layers are arranged on both sides of the substrate, the adhesive force of at least one adhesive layer can be within the above range. For example, when a foamable adhesive sheet is arranged between components to bond the components to each other, sometimes the foamable adhesive sheet is first arranged on one component, and then another component is inserted into the gap after the foamable adhesive sheet is arranged on one component. In such a case, when another component is inserted into the gap after the foamable adhesive sheet is arranged on one component, as long as the sliding property of the surface of the foamable adhesive sheet on one side in contact with the other component is good. Therefore, as long as the adhesive force of at least one adhesive layer is within the above range.
[0052] When adhesive layers are disposed on both surfaces of the substrate, for example, the adhesive strength of either adhesive layer or both adhesive layers may be within the above range, and preferably, the adhesive strength of both adhesive layers is within the above range.
[0053] The adhesive strength of the adhesive layer can be measured according to JIS Z0237:2009 (test method for adhesive tapes and adhesive sheets) based on ISO 29862 and method 1 of the test method for adhesive strength (a test method in which the tape and sheet are peeled off at 180° from a stainless steel test plate at a temperature of 23°C and a humidity of 50%). It should be noted that the details of the method for measuring the adhesive strength of the adhesive layer are described in the section of the Examples described later.
[0054] In the present invention, the adhesive force of the adhesive layer can be set to a value below a predetermined value by, for example, adjusting the composition of the adhesive layer. Specifically, in an adhesive layer containing an epoxy resin and a curing agent, the adhesiveness of the adhesive layer can be reduced by using an epoxy resin that is solid at room temperature, or by using a curing agent that is solid at room temperature. In addition, in an adhesive layer containing an epoxy resin and a curing agent, the adhesiveness of the adhesive layer can be reduced by containing an epoxy resin with a high softening temperature, or containing an epoxy resin with a large weight-average molecular weight. For example, by making the adhesive layer contain a plurality of epoxy resins with different softening temperatures, that is, when the adhesive layer contains one epoxy resin, it further contains other epoxy resins with a softening temperature of 25°C or more and 10°C or more higher than the softening temperature of the above-mentioned one epoxy resin, the adhesiveness of the adhesive layer can be reduced. In addition, for example, by making the adhesive layer contain a plurality of epoxy resins with different weight average molecular weights, that is, when the adhesive layer contains one epoxy resin, it further contains another epoxy resin with a weight average molecular weight of 370 or more and 300 or more greater than the weight average molecular weight of the above-mentioned one epoxy resin, the adhesiveness of the adhesive layer can be reduced. More specifically, in an adhesive layer containing an epoxy resin and a curing agent, as described later, by containing a first epoxy resin with a low softening temperature and a low molecular weight and a second epoxy resin with a high softening temperature and a high molecular weight as epoxy resins, the adhesiveness of the adhesive layer can be reduced. In addition, in an adhesive layer containing an epoxy resin and a curing agent, as described later, by containing an acrylic resin compatible with the epoxy resin, the adhesiveness of the adhesive layer can be reduced.
[0055] In the foamable adhesive sheet of the present invention, the pencil hardness of the surface on the adhesive layer side can be, for example, HB or more, or F or more. When the pencil hardness of the surface on the adhesive layer side of the foamable adhesive sheet of the present invention is F or more, the sliding property and the insertion property can be further improved. Specifically, if the pencil hardness of the surface on the adhesive layer side of the foamable adhesive sheet is within the above range, there is a tendency that the friction resistance becomes smaller, and the sliding property can be improved. In addition, when inserting the foamable adhesive sheet into the gap between components and the gap between components, and when inserting another component into the gap after the foamable adhesive sheet is arranged in one component, by making the above pencil hardness within the above range, the end face of the component can be suppressed from biting into the adhesive layer, and particularly when there are burrs on the end face of the component, the adhesive layer can be prevented from being hooked on the burrs on the end face of the component, and the insertion property can be improved. Therefore, for example, when the foamable adhesive sheet is configured between the components and the components are bonded to each other, the foamable adhesive sheet can be smoothly inserted into the gap between the components or the gap between the components, or another component can be smoothly inserted into the gap after the foamable adhesive sheet is configured in one component. In addition, by making the above-mentioned pencil hardness the above-mentioned range, the surface wear of the adhesive layer side of the foamable adhesive sheet can be suppressed when the foamable adhesive sheet is configured between the components. In addition, the above-mentioned pencil hardness can be, for example, below 2H. If the above-mentioned pencil hardness is too high, sometimes the adhesion of the adhesive layer to the base material is reduced.
[0056] When adhesive layers are disposed on both sides of the substrate, the pencil hardness of at least one of the two sides of the foamable adhesive sheet may be within the above range. For example, the pencil hardness of any one side may be within the above range, or the pencil hardness of both sides may be within the above range. It is preferred that the pencil hardness of both sides of the foamable adhesive sheet be within the above range.
[0057] The pencil hardness can be determined in accordance with JIS K5600 corresponding to ISO 15184. The details of the method for measuring the pencil hardness are described in the section of Examples described later.
[0058] The pencil hardness of the surface on the adhesive layer side of the foamable adhesive sheet in the present invention can be controlled, for example, by the composition of the adhesive layer. Specifically, the pencil hardness can be controlled by the average particle size and content of the foaming agent contained in the adhesive layer. More specifically, the pencil hardness can be increased by increasing the average particle size of the foaming agent. In addition, the pencil hardness can be increased by increasing the content of the foaming agent. In addition, for example, by making the adhesive layer contain an inorganic filler, the pencil hardness can be increased. In addition, for example, by making the adhesive layer contain a component having a rigid structure, the pencil hardness can be increased. Specifically, in the adhesive layer containing an epoxy resin and a curing agent, a phenolic resin can be cited as a component having a rigid structure.
[0059] In the foamable adhesive sheet of the present invention, the static friction coefficient of the surface of the adhesive layer side can be, for example, less than 0.34, less than 0.30, or less than 0.26. In addition, the above-mentioned static friction coefficient can be, for example, more than 0.16. In the case where the static friction coefficient of the surface of the adhesive layer side of the foamable adhesive sheet of the present invention is less than 0.30, it is possible to make the sliding property and the insertability further good. Therefore, for example, when the foamable adhesive sheet is configured between the components and the components are bonded to each other, the foamable adhesive sheet can be smoothly inserted in the gap between the components, the gap between the components, or another component can be smoothly inserted in the gap after the foamable adhesive sheet is configured in a component.
[0060] When adhesive layers are disposed on both sides of the substrate, the static friction coefficient of at least one side of the two sides of the foamable adhesive sheet may be within the above range, for example, the static friction coefficient of any one side may be within the above range, or the static friction coefficient of both sides may be within the above range. Preferably, the static friction coefficient of both sides of the foamable adhesive sheet is within the above range.
[0061] The static friction coefficient can be determined in accordance with JIS K7125 corresponding to ISO 8295. The details of the method for measuring the static friction coefficient are described in the section of Examples described later.
[0062] The static friction coefficient of the surface on the adhesive layer side of the foamable adhesive sheet in the present invention can be controlled by, for example, adjusting the composition of the adhesive layer, or adjusting the pencil hardness of the surface on the adhesive layer side of the foamable adhesive sheet. Specifically, the static friction coefficient can be controlled by the average particle size and content of the foaming agent contained in the adhesive layer. More specifically, if the average particle size of the foaming agent becomes larger, there is a trend that the static friction coefficient becomes smaller. In addition, if the content of the foaming agent becomes more, there is a trend that the static friction coefficient becomes smaller. In addition, if the pencil hardness of the surface on the adhesive layer side of the foamable adhesive sheet becomes higher, there is a trend that the static friction coefficient becomes smaller.
[0063] The foamable adhesive sheet in the present invention preferably has good shape retention. With respect to the bending moment based on JIS P8125, the bending moment based on JIS P8125 corresponding to ISO 2493 is, for example, 3gf·cm or more, and can be 5gf·cm or more. On the other hand, the bending moment is, for example, less than 40gf·cm, and can also be less than 30gf·cm. In the past, for the foamable adhesive sheet, a method of increasing the bending moment to improve the shape retention and the insertability into a narrow gap was usually adopted. In contrast, the inventors of the present invention found that the shape retention can be ensured by thinking of a way in terms of shape, and other undesirable conditions may exist if the bending moment is high, so in view of other characteristics, the bending moment is preferably within the above range. If the bending moment is less than the above range, it is possible to be difficult to maintain the shape even by folding back or the like. In addition, if the bending moment is greater than the above range, the shape will return to its original state after the bending process, so it is necessary to heat during the bending process or form an indentation at the fold line. If heating is performed, the sheet life is reduced, and if an indentation is formed, the insulation of the portion is likely to be reduced. In addition, in the foamable adhesive sheet of the present invention, the surface hardness is increased, so that even if high-speed insertion is performed, the surface is not damaged.
[0064] The foamable adhesive sheet of the present invention preferably has high adhesion after foaming and curing. The shear strength (adhesive strength) based on JIS K6850 corresponding to ISO 4587 can be, for example, 2.10MPa or more, 2.40MPa or more, or 3.0MPa or more at 23°C. In addition, the above-mentioned shear strength (adhesive strength) can be, for example, 0.27MPa or more, 0.55MPa or more, or 0.58MPa or more at 200°C. For example, in a high-strength acrylic foam adhesive tape that does not require heating, the shear strength (adhesive strength) is about 1MPa or more and 2MPa or less at room temperature, and has no heat resistance at 200°C. Therefore, if the above-mentioned shear strength (adhesive strength) is in the above-mentioned range at 23°C, it has an advantage in strength. In addition, if the above-mentioned shear strength (adhesive strength) is in the above-mentioned range at 200°C, it can be applied to the engine surrounding of an automobile and the use that requires heat resistance close to it.
[0065] The foamable adhesive sheet of the present invention preferably has high electrical insulation after foaming and curing. The insulation breakdown voltage based on JIS C2107 corresponding to IEC 60454-2 is preferably 3kV or more, and more preferably 5kV or more. By making the above-mentioned insulation breakdown voltage into the above-mentioned range, it can be rust-proof and applied around copper wires. In addition, the thermal conductivity of the adhesive sheet after foaming and curing is preferably 0.1W / mK or more, and more preferably 0.15W / mK or more. By making the above-mentioned thermal conductivity into the above-mentioned range, the miniaturization of the components can be sought, and the curing reaction during heating can be promoted.
[0066] 2. Adhesive layer
[0067] The adhesive layer in the present invention is disposed on at least one surface side of the substrate and contains a curable adhesive and a foaming agent.
[0068] (1) Adhesive layer material
[0069] (a) Curable adhesive
[0070] As the curable adhesive included in the adhesive layer of the present invention, a curable adhesive commonly used in the adhesive layer of the foamable adhesive sheet can be used. As the curable adhesive, for example, heat-curable adhesives and light-curable adhesives can be cited. Among them, heat-curable adhesives are preferred. Heat-curable adhesives can also be used when the components do not have transparency, such as metal components.
[0071] The curable adhesive is preferably an epoxy resin adhesive. That is, the curable adhesive preferably contains epoxy resin and curing agent. Usually, the cured film of the epoxy resin adhesive is hard and tough, and is suitable for bonding components of hard raw materials such as metal and glass components. Metal components are prone to burrs in the processing process, so for example, when inserting a foaming adhesive sheet in the gap between components or inserting another component in the gap after the foaming adhesive sheet is configured in one component, it is worried that the foaming adhesive sheet will be hooked on the burrs of the metal component, and the adhesive layer will float and peel off from the substrate. On the contrary, in the present invention, since the adhesive layer is excellent in adhesion to the substrate, the floating and peeling of the adhesive layer as described above from the substrate can be suppressed. Therefore, when using an epoxy resin adhesive, the present invention is useful. In addition, epoxy resin adhesives are usually excellent in heat resistance, insulation, chemical resistance, etc., and have little curing shrinkage, and can be used for a wide range of purposes.
[0072] In addition, when the curable adhesive is an epoxy resin adhesive, the curable adhesive preferably also contains an acrylic resin compatible with the epoxy resin. By further using an acrylic resin compatible with the epoxy resin, the toughness of the adhesive layer can be increased, and the adhesion of the adhesive layer to the substrate can be increased.
[0073] (i) Epoxy resin
[0074] The epoxy resin in the present invention is a compound having at least one epoxy group or glycidyl group, which undergoes a cross-linking polymerization reaction and cures when used in combination with a curing agent. The epoxy resin also includes a monomer having at least one epoxy group or glycidyl group.
[0075] As the epoxy resin, an epoxy resin commonly used for the adhesive layer of a foamable adhesive sheet can be used. Among them, the curable adhesive preferably contains a first epoxy resin having a softening temperature of 50°C or more and an epoxy equivalent of 5000g / eq or less, and a second epoxy resin having a softening temperature higher than the first epoxy resin and a weight average molecular weight of 20,000 or more as epoxy resins. By using the first epoxy resin and the second epoxy resin in combination, a foamable adhesive sheet having good anti-blocking properties and good adhesion after foaming and curing can be obtained. In addition, the adhesion (stickiness) of the adhesive layer can be reduced, and a foamable adhesive sheet with good sliding properties can be obtained.
[0076] For example, when only seeking to improve the adhesiveness after foaming and curing, it is effective to use low molecular weight (low epoxy equivalent) epoxy resins compared to high molecular weight (high epoxy equivalent) epoxy resins. However, when using low molecular weight (low epoxy equivalent) epoxy resins, for example, when the foamable adhesive sheet is wound into a roll, the low molecular weight (low epoxy equivalent) epoxy resins assimilate each other and are prone to adhesion.
[0077] In contrast, when using the first epoxy resin with a relatively low softening temperature (relatively high crystallinity) and low molecular weight (low epoxy equivalent), if the first epoxy resin becomes a temperature above the softening temperature, it rapidly melts and changes into a low-viscosity liquid state. Therefore, it is easy to improve the adhesion after foaming and curing. On the other hand, the first epoxy resin is relatively high in crystallinity, so compared with the epoxy resin with relatively low crystallinity or the epoxy resin without crystallinity, it is possible to suppress the generation of adhesion. However, when only using the first epoxy resin, there is the possibility that the generation inhibition effect of adhesion is insufficient, and the adhesion (viscosity) of the adhesive layer becomes too high. Therefore, by further using the second epoxy resin with a relatively high softening temperature (relatively low crystallinity) and high molecular weight, it is possible to improve the generation inhibition effect of adhesion, and the adhesion (viscosity) of the adhesive layer is suppressed to be low.
[0078] (i-1) First epoxy resin
[0079] The softening temperature of the first epoxy resin is above 50°C, and the epoxy equivalent is below 5000g / eq. Compared with the second epoxy resin described later, the first epoxy resin has a relatively low softening temperature (relatively high crystallinity). Since the first epoxy resin has relatively high crystallinity and low molecular weight, it is easy to improve the adhesion and anti-blocking properties after foaming and curing. In addition, since the first epoxy resin has a low molecular weight, it is possible to increase the crosslinking density, and an adhesive layer with good mechanical strength, chemical resistance, and curability can be obtained. In addition, the first epoxy resin is preferably an epoxy resin that is solid at room temperature (23°C).
[0080] The softening temperature of the first epoxy resin is usually 50° C. or higher, and may be 55° C. or higher, or 60° C. or higher. On the other hand, the softening temperature of the first epoxy resin is, for example, 150° C. or lower. The softening temperature can be measured by a ring and ball method in accordance with JIS K7234.
[0081] The epoxy equivalent of the first epoxy resin is, for example, less than 5000 g / eq, less than 3000 g / eq, less than 1000 g / eq, or less than 600 g / eq. On the other hand, the epoxy equivalent of the first epoxy resin is, for example, greater than 90 g / eq, greater than 100 g / eq, or greater than 110 g / eq. The epoxy equivalent can be measured by a method according to JIS K7236 corresponding to ISO 3001 (Plastics-Epoxy compounds-Determination of epoxy equivalent), and is the number of grams of resin containing 1 gram equivalent of epoxy groups.
[0082] The first epoxy resin may be a monofunctional epoxy resin, a difunctional epoxy resin, a trifunctional epoxy resin, or a tetrafunctional or higher-functional epoxy resin.
[0083] In addition, the weight average molecular weight (Mw) of the first epoxy resin is usually less than the weight average molecular weight (Mw) of the second epoxy resin described later. The Mw of the first epoxy resin is, for example, 6,000 or less, 4,000 or less, or 3,000 or less. On the other hand, the Mw of the first epoxy resin is, for example, 400 or more. Mw is a value converted to polystyrene when measured by gel permeation chromatography (GPC).
[0084] The melt viscosity of the first epoxy resin at 150°C is, for example, 0.005 Pa·s or more, 0.015 Pa·s or more, 0.03 Pa·s or more, 0.05 Pa·s or more, or 0.1 Pa·s or more. If the melt viscosity is too low, good foaming may not be obtained. In addition, if the melt viscosity of the first epoxy resin is too low (if the crystallinity of the first epoxy resin is too high), there is a possibility that the adhesion (viscosity) of the resulting adhesive layer becomes higher. It is speculated that the reason is that if the melt viscosity of the first epoxy resin is too low (if the crystallinity of the first epoxy resin is too high), when it is compatible with the second epoxy resin or the acrylic resin, its crystallinity is greatly reduced, and the Tg of the adhesive composition as a whole is reduced. On the other hand, the melt viscosity of the first epoxy resin at 150°C is, for example, 10 Pa·s or less, 5 Pa·s or less, or 2 Pa·s or less. If the melt viscosity is too high, there is a possibility that the uniformity of the resulting adhesive layer is reduced. The melt viscosity can be determined by measuring in accordance with JIS K6862 corresponding to ISO 2555 (Resins in the liquid state or as emulsions or dispersions - Determination of Brookfield RV viscosity) using a Brookfield single cylinder rotational viscometer and a thermocouple for heating the solution.
[0085] Next, the composition of the first epoxy resin is described. As the first epoxy resin, for example, aromatic epoxy resins, aliphatic epoxy resins, alicyclic epoxy resins, and heterocyclic epoxy resins can be cited. As specific examples of the first epoxy resin, bisphenol-type epoxy resins such as bisphenol A epoxy resin and bisphenol F epoxy resin; linear phenolic epoxy resins such as bisphenol A linear novolac epoxy resin and cresol linear novolac epoxy resin; modified epoxy resins such as urethane modified epoxy resins and rubber modified epoxy resins can be cited. In addition, as other specific examples, biphenyl epoxy resins, stilbene epoxy resins, trisphenol methane epoxy resins, alkyl-modified trisphenol methane epoxy resins, epoxy resins containing triazine cores, dicyclopentadiene-modified phenolic epoxy resins, naphthalene epoxy resins, glycol epoxy resins, and pentaerythritol epoxy resins can be cited. The first epoxy resin can be one kind or two or more kinds.
[0086] Depending on the number of repeating units of the bisphenol skeleton, the bisphenol A type epoxy resin may exist in a liquid state at room temperature, or may exist in a solid state at room temperature. A bisphenol A type epoxy resin having a main chain bisphenol skeleton of, for example, 2 or more and 10 or less is solid at room temperature. In particular, bisphenol A type epoxy resin is preferred in that it can improve heat resistance.
[0087] In particular, the first epoxy resin is preferably a bisphenol A novolac type epoxy resin represented by the following general formula (1).
[0088] [Chemical formula 1]
[0089]
[0090] In the general formula (1), R 1 C m H 2m (m is 1 or more and 3 or less), R 2 and R 3 Each independently is C p H 2p+1 In the group represented by (p is 1 to 3), n is 0 to 10.
[0091] In the general formula (1), preferably R 1 The m in is 1, that is, R 1 is -CH2-. Similarly, R 2 and R 3 p in is 1, that is, R 2 and R 3 In addition, the hydrogen bonded to the benzene ring of the general formula (1) may be substituted by other elements or other groups.
[0092] When the resin component contained in the adhesive layer is set to 100 mass parts, the content of the first epoxy resin is, for example, more than 1 mass part, can be more than 3 mass parts, can also be more than 5 mass parts, can also be more than 10 mass parts, can also be more than 15 mass parts, can also be more than 25 mass parts.If the content of the first epoxy resin is too little, there is the possibility that the adhesion and anti-blocking after foaming and curing are reduced.On the other hand, when the resin component contained in the adhesive layer is set to 100 mass parts, the content of the first epoxy resin is, for example, less than 90 mass parts, can be less than 80 mass parts, can also be less than 70 mass parts, can also be less than 60 mass parts, can also be less than 50 mass parts, can also be less than 40 mass parts.If the content of the first epoxy resin is too much, the content of the second epoxy resin and acrylic resin decreases relatively, and it is possible that the adhesion of the adhesive layer to the substrate, the anti-blocking and the adhesion after foaming and curing can not be balanced.
[0093] (i-2) Second epoxy resin
[0094] The softening temperature of the second epoxy resin is higher than that of the first epoxy resin, and the weight average molecular weight is greater than 20,000. Compared with the above-mentioned first epoxy resin, the second epoxy resin has a relatively high softening temperature (relatively low crystallinity). Since the second epoxy resin has relatively low crystallinity and high molecular weight, it is easy to improve anti-blocking properties. In addition, since the second epoxy resin has relatively low crystallinity and high molecular weight, it is possible to suppress the increase in adhesion (tack) caused by the first epoxy resin. In addition, the second epoxy resin is preferably an epoxy resin that is solid at room temperature (23°C).
[0095] The weight average molecular weight (Mw) of the second epoxy resin is usually greater than the weight average molecular weight (Mw) of the first epoxy resin. The Mw of the second epoxy resin is usually 20,000 or more, and may be 30,000 or more, or 35,000 or more. On the other hand, the Mw of the second epoxy resin is, for example, 100,000 or less.
[0096] The epoxy equivalent of the second epoxy resin may be larger, smaller, or the same as that of the first epoxy resin. The epoxy equivalent of the second epoxy resin is, for example, 4000 g / eq or more, 5000 g / eq or more, or 6000 g / eq or more. On the other hand, the epoxy equivalent of the second epoxy resin is, for example, 20000 g / eq or less.
[0097] The second epoxy resin may be a monofunctional epoxy resin, a difunctional epoxy resin, a trifunctional epoxy resin, or a tetrafunctional or higher-functional epoxy resin.
[0098] The softening temperature of the second epoxy resin is usually higher than the softening temperature of the first epoxy resin. The difference between the two is, for example, 10°C or more, 20°C or more, or 30°C or more. The softening temperature of the second epoxy resin is, for example, 80°C or more, or 90°C or more. On the other hand, the softening temperature of the second epoxy resin is, for example, 180°C or less.
[0099] The configuration of the second epoxy resin is the same as that of the first epoxy resin described above, and therefore description thereof is omitted here.
[0100] When the resin component contained in the bonding layer is set to 100 mass parts, the content of the second epoxy resin is, for example, more than 10 mass parts, can be more than 15 mass parts, can also be more than 20 mass parts, can also be more than 25 mass parts, can also be more than 30 mass parts, can also be more than 35 mass parts, can also be more than 40 mass parts, can also be more than 45 mass parts.If the content of the second epoxy resin is too little, then there is the possibility that anti-blocking property reduces.On the other hand, when the resin component contained in the bonding layer is set to 100 mass parts, the content of the second epoxy resin is, for example, less than 90 mass parts, can be less than 85 mass parts, can also be less than 80 mass parts, can also be less than 75 mass parts.If the content of the second epoxy resin is too much, then the content of the first epoxy resin and acrylic resin decreases relatively, and it is possible that the bonding layer cannot be balanced to the adhesion of the substrate, anti-blocking property and the adhesion after foaming and curing.
[0101] The ratio of the first epoxy resin to the total of the first epoxy resin and the second epoxy resin is, for example, 5% by mass or more, 10% by mass or more, 15% by mass or more, or 20% by mass or more. On the other hand, the ratio of the first epoxy resin is, for example, 80% by mass or less, 75% by mass or less, or 60% by mass or less.
[0102] The ratio of the total of the first epoxy resin and the second epoxy resin to the total epoxy resin contained in the adhesive layer may be, for example, 50 mass % or more, 70 mass % or more, 90 mass % or more, or 100 mass %.
[0103] (ii) Acrylic resin
[0104] Acrylic resin in the present invention is a resin compatible with epoxy resin. Acrylic resin is compatible with epoxy resin, so it is easy to improve the toughness of adhesive layer. As a result, the adhesion of adhesive layer to substrate can be improved. In addition, by improving the toughness of adhesive layer, the improvement of adhesiveness after foaming and curing can be sought. In addition, it is believed that the compatibilizer as a foaming agent (for example, the foaming agent of the resin of the shell portion being acrylonitrile copolymer) plays a role by acrylic resin, and evenly disperses and foams, thereby the adhesiveness after foaming and curing improves. In addition, by acrylic resin and epoxy resin compatible, the hardness on the adhesive layer surface can be kept high. On the other hand, if acrylic resin is incompatible with epoxy resin, soft position is formed on the adhesive layer surface, so sometimes the interface with adherend becomes difficult to slide, and workability reduces.
[0105] The acrylic resin in the present invention is compatible with the epoxy resin. Here, the compatibility of the acrylic resin with the epoxy resin can be confirmed, for example, by observing the cross section of the adhesive layer of the foaming adhesive sheet with a scanning electron microscope (SEM) or a transmission electron microscope (TEM) without producing micron-sized islands. More specifically, the average particle size of the island is preferably less than 1 μm. Among them, the average particle size of the island can be less than 0.5 μm, or less than 0.3 μm. The number of samples is preferably large, for example, more than 100. The area of the observed region is carried out in the range of 100 μm×100 μm, or, when the average thickness of the adhesive layer is less than 100 μm, it is carried out in the range of average thickness×100 μm.
[0106] The weight average molecular weight (Mw) of the acrylic resin is, for example, 50,000 or more, 70,000 or more, or 100,000 or more. The first epoxy resin has relatively high crystallinity, and the melt viscosity (or dynamic viscoelasticity) when heated may become too low, and shrinkage may occur during curing after foaming (from the end of foaming of the foaming agent to the curing of the adhesive composition). However, by using an acrylic resin with a certain molecular weight, the melt viscosity can be prevented from becoming too low, and shrinkage is less likely to occur during curing after foaming. On the other hand, the Mw of the acrylic resin is, for example, 1,500,000 or less. The weight average molecular weight of the acrylic resin can be measured by GPC (eluent: THF, standard substance: PS, sample: 20 μL, flow rate: 1 mL / min, column temperature: 40°C).
[0107] The glass transition temperature (Tg) of the acrylic resin is, for example, 90° C. or higher, or 100° C. or higher. On the other hand, the Tg of the acrylic resin is, for example, 180° C. or lower. Tg can be measured by thermal analysis such as differential scanning calorimetry (DSC) in accordance with JIS K7121 corresponding to ISO 3146.
[0108] The storage modulus (E') of acrylic resin at the foaming starting temperature can be 1×10 6 Pa or less. By lowering E' at the start of foaming, fluidity is improved, and good foaming properties can be obtained. On the other hand, E' at the foaming start temperature is, for example, 1×10 5 Pa or more. It should be noted that the foaming initiation temperature is a temperature that varies depending on the type of foaming agent. In addition, when two or more foaming agents are used as the foaming agent, the initiation temperature of the main foaming reaction is taken as the foaming initiation temperature.
[0109] The storage modulus (E') of acrylic resin at the curing starting temperature can be 1×10 5Pa or more. As mentioned above, sometimes shrinkage occurs during the curing after foaming (from the end of the foaming of the foaming agent to the curing of the adhesive composition), but by making E' at the curing start temperature large, shrinkage can be suppressed and good shape retention can be obtained. It should be noted that the curing start temperature is a temperature that varies according to the type of curing agent. In addition, when using two or more curing agents as curing agents, the starting temperature of the main curing reaction is used as the curing start temperature.
[0110] In addition, the average value of the storage modulus (E') of the acrylic resin at 0°C or higher and 100°C or lower can be 1×10 6 Pa or more. By making the average value of E' before foaming high, good anti-blocking properties can be obtained. On the other hand, the average value of the storage modulus (E') at 0°C or higher and 100°C or lower is, for example, 1×10 8 Below Pa.
[0111] The acrylic resin may have a polar group. Examples of the polar group include an epoxy group, a hydroxyl group, a carboxyl group, a nitrile group, and an amide group.
[0112] The acrylic resin is a homopolymer of an acrylate monomer, and may be a mixed component containing two or more of the above homopolymers, or a copolymer of two or more acrylate monomers, or a component containing one or more copolymers. In addition, the acrylic resin may be a mixed component of the above homopolymer and the above copolymer. The "acrylic acid" of the acrylate monomer also includes the concept of methacrylic acid. Specifically, the acrylic resin may be a mixture of a methacrylate polymer and an acrylate polymer, or may be an acrylate polymer such as acrylate-acrylate, methacrylate-methacrylate, or methacrylate-acrylate. Among them, the acrylic resin preferably contains a copolymer of two or more acrylate monomers (a (meth)acrylate copolymer).
[0113] As the monomer components constituting the (meth)acrylate copolymer, for example, the monomer components described in Japanese Patent Publication No. 2014-065889 can be cited. The above-mentioned monomer components may have the above-mentioned polar groups. As the above-mentioned (meth)acrylate copolymer, for example, ethyl acrylate-butyl acrylate-acrylonitrile copolymer, ethyl acrylate-acrylonitrile copolymer, butyl acrylate-acrylonitrile copolymer can be cited. It should be noted that "acrylic acid" of methyl acrylate, ethyl acrylate, etc. also includes "methacrylic acid" of methyl methacrylate, ethyl methacrylate, etc.
[0114] As the above-mentioned (meth)acrylate copolymer, a block copolymer is preferred, and an acrylic block copolymer such as a methacrylate-acrylate copolymer is more preferred. Examples of the (meth)acrylate constituting the acrylic block copolymer include methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, cyclohexyl acrylate, and benzyl acrylate. These "acrylic acids" also include "methacrylic acids".
[0115] Specific examples of methacrylate-acrylate copolymers include acrylic copolymers such as methyl methacrylate-butyl acrylate-methyl methacrylate (MMA-BA-MMA) copolymers. MMA-BA-MMA copolymers also include block copolymers of polymethyl methacrylate-polybutyl acrylate-polymethyl methacrylate (PMMA-PBA-PMMA).
[0116] The acrylic copolymer may not have a polar group, or may be a modified product in which the polar group is introduced partially. The modified product is easily compatible with the epoxy resin, and thus the adhesiveness is further improved.
[0117] Among them, the acrylic resin is preferably a (meth)acrylate copolymer having a first polymer portion having a glass transition temperature (Tg) of 10° C. or less and a second polymer portion having a glass transition temperature (Tg) of 20° C. or more. Such a (meth)acrylate copolymer has a first polymer portion that is a soft segment and a second polymer portion that is a hard segment.
[0118] The above effects can be inferred as follows: by using an acrylic resin having both soft segments and hard segments such as the (meth)acrylate copolymer, the hard segments contribute to heat resistance and the soft segments contribute to toughness or flexibility, thereby obtaining an adhesive layer having good heat resistance, toughness and flexibility.
[0119] At least one of the first polymer part and the second polymer part contained in the (meth)acrylate copolymer is compatible with the epoxy resin. When the first polymer part is compatible with the epoxy resin, the flexibility can be improved. In addition, when the second polymer part is compatible with the epoxy resin, the cohesion and toughness can be improved.
[0120] In the case where one of the first polymer part or the second polymer part is not compatible with the epoxy resin, the (meth)acrylate copolymer has a compatible part which is a polymer part compatible with the epoxy resin and an incompatible part which is a polymer part incompatible with the epoxy resin. In this case, if the (meth)acrylate copolymer is added to the adhesive composition, the compatible part is compatible with the epoxy resin and the incompatible part is incompatible with the epoxy resin, so fine phase separation occurs. As a result, a fine sea-island structure is formed. The sea-island structure varies depending on the type of (meth)acrylate copolymer, the compatibility of the first polymer part and the second polymer part contained in the (meth)acrylate copolymer, and the presence or absence of modification based on the introduction of polar groups. For example, there can be cited a sea-island structure in which the compatible parts of the cured epoxy resin and the (meth)acrylate copolymer are the sea and the incompatible parts of the (meth)acrylate copolymer are the islands; a sea-island structure in which the incompatible parts of the (meth)acrylate copolymer are the sea and the compatible parts of the cured epoxy resin and the (meth)acrylate copolymer are the islands; and a sea-island structure in which the (meth)acrylate copolymer is the sea and the cured epoxy resin is the islands. By having such a sea-island structure, stress can be easily dispersed, so that interface damage can be avoided, and excellent adhesion can be obtained after foaming and curing.
[0121] As for the above-mentioned (meth) acrylate copolymer, among them, block copolymers are preferred, and ABA block copolymers in which the compatible part is set as polymer block A and the incompatible part is set as polymer block B are particularly preferred. In addition, ABA block copolymers in which the first polymer part is the incompatible part, the second polymer part is the compatible part, the first polymer part is set as polymer block B, and the second polymer part is set as polymer block A are preferred. By using such an ABA block copolymer as an acrylic resin, in the case of a sea island structure in which the compatible part of the cured product of epoxy resin and the (meth) acrylate copolymer is the sea and the incompatible part of the (meth) acrylate copolymer is the island, the island part can be reduced. In addition, in the case of a sea island structure in which the incompatible part of the (meth) acrylate copolymer is the sea, the compatible part of the cured product of epoxy resin and the (meth) acrylate copolymer is the island, or in the case of a sea island structure in which the (meth) acrylate copolymer is the sea and the cured product of epoxy resin is the island, the sea part can be reduced.
[0122] The (meth)acrylate copolymer may be a modified product in which the polar group is introduced into a part of the first polymer portion or the second polymer portion.
[0123] The Tg of the first polymer part contained in the above-mentioned (meth)acrylate copolymer is below 10°C, and can be set in the range of -150°C to 10°C, especially in the range of -130°C to 0°C, and particularly in the range of -110°C to -10°C.
[0124] The Tg of the first polymer portion can be calculated by the following formula based on the Tg (K) of each homopolymer described in "POLYMER HANDBOOK 3rd Edition" (published by John Wiley & Sons, Ink.).
[0125] 1 / Tg(K)=W1 / Tg1+W2 / Tg2+····+W n / Tg n
[0126] W n ; Mass fraction of each monomer
[0127] Tg n ; The Tg (K) of the homopolymer of each monomer may be a value generally disclosed, such as the value in the Polymer Handbook (3rd Ed., J. Brandrup and E. H. Immergut, WILEY INTERSCIENCE). The same applies to the Tg of the second polymer portion described later.
[0128] The first polymer part contained in the above-mentioned (meth)acrylate copolymer may be a homopolymer or a copolymer, and preferably a homopolymer. The monomer components and polymer components constituting the first polymer part may be monomer components and polymer components that can obtain the first polymer part having a Tg within a predetermined range, and examples thereof include acrylate monomers such as butyl acrylate, 2-ethylhexyl acrylate, isononyl acrylate, and methyl acrylate, other monomers such as vinyl acetate, acetal, and urethane, polar group-containing monomers containing the above-mentioned polar groups, and copolymers such as EVA.
[0129] The Tg of the second polymer part contained in the above-mentioned (meth)acrylate copolymer is higher than 20°C, and can be set in the range of higher than 20°C and lower than 150°C, especially in the range of higher than 30°C and lower than 150°C, and particularly in the range of higher than 40°C and lower than 150°C.
[0130] The second polymer part contained in the (meth)acrylate copolymer may be a homopolymer or a copolymer, and preferably a homopolymer. The monomer component constituting the second polymer part may be any monomer component that can obtain a second polymer part having a Tg within a predetermined range, and examples thereof include acrylic acid ester monomers such as methyl methacrylate, acrylamide, styrene, vinyl chloride, amide, acrylonitrile, cellulose acetate, phenol, carbamate, vinylidene chloride, methylene chloride, methacrylonitrile and other monomers, and polar group-containing monomers containing the above-mentioned polar groups.
[0131] Specific examples of the (meth)acrylate copolymer having the first polymer part and the second polymer part include the above-mentioned MMA-BA-MMA copolymer.
[0132] When the resin composition contained in the bonding layer is made into 100 mass parts, the content of acrylic resin is, for example, more than 1 mass part, can be more than 3 mass parts, can also be more than 5 mass parts, can also be more than 7 mass parts, can also be more than 10 mass parts.If the content of acrylic resin is too little, then there is the possibility that the bonding layer reduces the adhesion of the substrate and the adhesion after the foaming and curing.On the other hand, when the resin composition contained in the bonding layer is made into 100 mass parts, the content of acrylic resin is, for example, below 60 mass parts, can be below 50 mass parts, can also be below 40 mass parts, can also be below 35 mass parts, can also be below 30 mass parts.If the content of acrylic resin is too much, then the content of the first epoxy resin and the second epoxy resin tapers relatively, and it is possible that the bonding layer cannot be balanced to the adhesion of the substrate, the anti-blocking and the adhesion after the foaming and curing.
[0133] (iii) Curing agent
[0134] As the curing agent in the present invention, it can be appropriately selected according to the type of curable adhesive. When the curable adhesive is, for example, an epoxy resin adhesive, as the curing agent, a curing agent commonly used in epoxy resin adhesives can be used. The curing agent is preferably solid at 23°C. A curing agent that is solid at 23°C can extend the storage stability (applicable life) compared to a curing agent that is liquid at 23°C. In addition, the curing agent may be a latent curing agent. In addition, the curing agent may be a curing agent that undergoes a curing reaction by heat, or a curing agent that undergoes a curing reaction by light. In addition, in the present invention, the curing agent may be used alone, or two or more types may be used.
[0135] The reaction starting temperature of the curing agent is, for example, above 110°C, and may be above 130°C. If the reaction starting temperature is too low, the reaction starts at an early stage, and curing occurs in a state where the softness and fluidity of the resin component are low, and it may be difficult to uniformly cure. On the other hand, the reaction starting temperature of the curing agent is, for example, below 200°C. If the reaction starting temperature is too high, there is a possibility that the resin component deteriorates. It should be noted that, in the case of using a resin with high heat resistance such as a phenolic resin in addition to an epoxy resin, the reaction starting temperature of the curing agent may be, for example, below 300°C due to the small deterioration of the resin component. The reaction starting temperature of the curing agent can be obtained by differential scanning calorimetry (DSC).
[0136] Specific examples of the curing agent include imidazole-based curing agents, phenol-based curing agents, amine-based curing agents, acid anhydride-based curing agents, isocyanate-based curing agents, and thiol-based curing agents.
[0137] As imidazole curing agents, for example, imidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-isopropylimidazole, 2-phenylimidazole, carboxylates of imidazole compounds, and adducts with epoxy compounds can be cited. In addition, the imidazole curing agent preferably has a hydroxyl group. Crystallization occurs through hydrogen bonding between hydroxyl groups, so there is a tendency for the reaction starting temperature to become higher.
[0138] As the phenolic curing agent, for example, phenolic resin can be mentioned. In addition, as the phenolic resin, for example, resol type phenolic resin and linear phenolic resin can be mentioned. From the viewpoint of the adhesion of the adhesive layer to the substrate, linear phenolic resin with a Tg of 110° C. or less is particularly preferred. In addition, a phenolic curing agent and an imidazole curing agent can also be used in combination. In this case, it is preferred to use an imidazole curing agent as a curing catalyst.
[0139] It should be noted that, in adhesive layer, by containing phenolic resin, can seek the raising of thermotolerance, but on the other hand, toughness reduces, and there may be the adhesive layer from the floating of base material, peeling off when for example the foamable adhesive sheet is bent, cut off.On the contrary, in the present invention, because adhesive layer is excellent to the adhesion of base material, so even when adhesive layer contains phenolic resin, the generation of adhesive layer from the floating of base material, peeling off when also can suppress bending.As a result, the foamable adhesive sheet of the suppression of adhesive layer from the floating of base material, peeling off when can obtain taking into account the raising of thermotolerance and bending.
[0140] From the aspect of heat resistance, the phenolic resin is preferably a biphenyl type. In addition, the phenolic resin may be a resin in which the phenol core is modified. By modifying the phenol core, for example, heat resistance can be further improved.
[0141] On the other hand, when the adhesive layer does not contain a phenol resin, the adhesive layer can be effectively prevented from floating or peeling off from the substrate during bending or cutting, and the adhesion of the adhesive layer to the substrate can be improved.
[0142] Examples of amine curing agents include aliphatic amines such as diethylenetriamine (DETA), triethylenetetramine (TETA), and meta-xylylenediamine (MXDA); aromatic amines such as diaminodiphenylmethane (DDM), meta-phenylenediamine (MPDA), and diaminodiphenylsulfone (DDS); alicyclic amines; and polyamide amines. In addition, amine curing agents that can be used include dicyandiamide curing agents such as dicyandiamide (DICY), organic acid dihydrazide curing agents, amine adduct curing agents, and ketimine curing agents.
[0143] Examples of the acid anhydride curing agent include alicyclic acid anhydrides (liquid acid anhydrides) such as hexahydrophthalic anhydride (HHPA) and methyltetrahydrophthalic anhydride (MTHPA); and aromatic acid anhydrides such as trimellitic anhydride (TMA), pyromellitic anhydride (PMDA), and benzophenonetetracarboxylic dianhydride (BTDA).
[0144] As an isocyanate type curing agent, blocked isocyanate is mentioned, for example.
[0145] Examples of the thiol-based curing agent include ester bond type thiol compounds, aliphatic ether bond type thiol compounds, and aromatic ether bond type thiol compounds.
[0146] When the resin component contained in the adhesive layer is set to 100 parts by mass, the content of the curing agent is, for example, more than 1 part by mass and less than 40 parts by mass. For example, when an imidazole curing agent is used as a curing agent as the main component, when the resin component contained in the adhesive layer is set to 100 parts by mass, the content of the curing agent is, for example, preferably more than 1 part by mass and less than 15 parts by mass. On the other hand, when a phenol curing agent is used as a curing agent as the main component, when the resin component contained in the adhesive layer is set to 100 parts by mass, the content of the curing agent is, for example, preferably more than 5 parts by mass and less than 40 parts by mass. It should be noted that using an imidazole curing agent or a phenol curing agent as the main component as a curing agent means that the mass proportion of the imidazole curing agent or the phenol curing agent in the curing agent is the largest.
[0147] (b) Foaming agent
[0148] As the foaming agent in the present invention, a foaming agent commonly used in the adhesive layer of a foamable adhesive sheet can be used. In addition, the foaming agent may be a foaming agent that generates a foaming reaction by heat or a foaming agent that generates a foaming reaction by light.
[0149] The foaming starting temperature of the foaming agent is preferably above the softening temperature of the main agent of the curable adhesive such as epoxy resin and below the activation temperature of the curing reaction of the main agent of the curable adhesive such as epoxy resin. The foaming starting temperature of the foaming agent is, for example, above 70°C, and can be above 100°C. If the reaction starting temperature is too low, the reaction starts too early, and foaming occurs in a state where the softness and fluidity of the resin component are low, and it may be difficult to produce uniform foaming. On the other hand, the reaction starting temperature of the foaming agent is, for example, below 210°C. If the reaction starting temperature is too high, there is a possibility that the resin component will deteriorate.
[0150] The softening temperature of the main component of a curable adhesive such as an epoxy resin can be measured using the ring and ball softening temperature test method specified in JIS K7234.
[0151] Examples of the foaming agent include organic foaming agents and inorganic foaming agents. Examples of the organic foaming agent include azodicarbonamide (ADCA), azobiscarbonamide, azobisisobutyronitrile and other azo foaming agents, trichloromonofluoromethane and other fluorinated alkane foaming agents, p-toluenesulfonylhydrazide and other hydrazine foaming agents, p-toluenesulfonylsemicarbazide and other semicarbazide foaming agents, 5-morpholinyl-1,2,3,4-thiotriazole and other triazole foaming agents, N,N-dinitrosoterephthalamide and other N-nitroso foaming agents. On the other hand, examples of the inorganic foaming agent include ammonium carbonate, ammonium bicarbonate, ammonium nitrite, ammonium borohydride, and azides.
[0152] In addition, a microcapsule type foaming agent can be used as the foaming agent. The microcapsule type foaming agent preferably has a thermal expansion agent such as hydrocarbon as a core and a resin such as acrylonitrile copolymer as a shell.
[0153] The average particle size of the foaming agent can be, for example, 7 μm or more, 10 μm or more, 13 μm or more, or 17 μm or more. When the average particle size of the foaming agent is 10 μm or more, the pencil hardness of the surface on the adhesive layer side of the foamable adhesive sheet can be increased, and the static friction coefficient of the surface on the adhesive layer side of the foamable adhesive sheet can be reduced, so that the sliding property and the insertion property can be further improved. On the other hand, the average particle size of the foaming agent is preferably less than the average thickness of the adhesive layer.
[0154] In addition, the average particle size of the foaming agent is preferably, for example, greater than 10 μm and less than 24 μm. The average particle size of the foaming agent may be, for example, greater than 13 μm, or greater than 17 μm. In addition, the average particle size of the foaming agent may be, for example, less than 21 μm, or less than 20 μm. By making the average particle size of the foaming agent within the above range, the adhesion can be improved even when the gap between the components is relatively wide. The reason is not clear, but it is speculated as follows. That is, if the average particle size of the foaming agent is too small, there is a tendency for the foaming ratio of the adhesive layer to become smaller. Therefore, when the gap between the components is narrow, good adhesion can be obtained. In contrast, when the gap between the components is wide, the adhesion is sometimes reduced. In addition, it is believed that when the average particle size of the foaming agent is small, the foaming ratio of the adhesive layer can be increased by increasing the content of the foaming agent, but if the content of the foaming agent is increased, the content of the curable adhesive becomes relatively small, so the wall between the bubbles in the adhesive layer after foaming and curing becomes thinner, and the cohesive force decreases, and the adhesiveness in the case where the gap between the components is wide is reduced. On the other hand, it is believed that if the average particle size of the foaming agent is too large, the bubbles after foaming become larger, so the wall between the bubbles in the adhesive layer after foaming and curing becomes thinner, and the cohesive force decreases, and the adhesiveness is reduced even when the gap between the components is narrow. In contrast, it is speculated that when the average particle size of the foaming agent is within the above range, the foaming ratio of the adhesive layer will not be too small, so the gaps between the components can be fully filled. In addition, the bubbles after foaming will not be too large, so the walls between the bubbles in the adhesive layer after foaming and curing become thicker, which can increase the contact area between the walls between the bubbles in the adhesive layer after foaming and curing and the components. As a result, good adhesion can be obtained not only when the gap between the components is narrow, but also when the gap between the components is wide.
[0155] It should be noted that the average particle size of the foaming agent is the particle size at the cumulative value of 50% in the particle size distribution obtained by the laser diffraction scattering method. In addition, when measuring the average particle size of the foaming agent, the adhesive layer is dissolved in a solvent to separate the foaming agent. As the solvent, there is no particular limitation as long as it is a solvent that can dissolve the components other than the foaming agent contained in the adhesive layer. It can be appropriately selected according to the type of curable adhesive contained in the adhesive layer, for example, the solvent used in the adhesive composition for forming the adhesive layer can be used. Specifically, methyl ethyl ketone, ethyl acetate, toluene, etc. can be used.
[0156] When the resin composition contained in the adhesive layer is set to 100 mass parts, the content of the whipping agent is, for example, more than 0.5 mass parts, can be more than 2 mass parts, can also be more than 3 mass parts, can also be more than 4 mass parts, can also be more than 5 mass parts. On the other hand, relative to 100 mass parts of resin composition contained in the adhesive layer, the content of the whipping agent is, for example, below 25 mass parts, can be below 20 mass parts, can also be below 15 mass parts. If the content of the whipping agent is too little, the static friction coefficient of the face of the adhesive layer side of the foamable adhesive sheet becomes large, or the pencil hardness of the face of the adhesive layer side of the foamable adhesive sheet decreases, and there is the possibility that slidability and insertion reduce. In addition, if the content of the whipping agent is too little, the expansion ratio of the adhesive layer decreases, and when the gap between components is wide, there is the possibility that adhesiveness reduces. On the other hand, if the content of the foaming agent is too much, the content of the curable adhesive becomes relatively small, so the wall between the bubbles in the adhesive layer after foaming and curing becomes thinner, and the cohesive force is reduced, and there is a possibility of reduced adhesion. It should be noted that when the average particle size of the foaming agent is 10 μm or more and 24 μm or less, by making the content of the foaming agent 3 parts by mass or more and 25 parts by mass or less relative to 100 parts by mass of the resin component contained in the adhesive layer, the adhesion can be made better in the case where the gap between the components is narrow and the gap between the components is wide.
[0157] (c) Other ingredients
[0158] When the curable adhesive is an epoxy resin adhesive, the adhesive layer in the present invention may contain only epoxy resin and acrylic resin as resin components, or may further contain other resins. Examples of other resins include urethane resins.
[0159] The total ratio of the first epoxy resin, the second epoxy resin and the acrylic resin to the resin component contained in the adhesive layer is, for example, 70 mass % or more, 80 mass % or more, 90 mass % or more, or 100 mass %.
[0160] The content of the resin component contained in the adhesive layer may be, for example, 60% by mass or more, 70% by mass or more, 80% by mass or more, or 90% by mass or more.
[0161] The adhesive layer may contain, for example, a silane coupling agent, a filler, an antioxidant, a light stabilizer, an ultraviolet absorber, a lubricant, a plasticizer, an antistatic agent, a crosslinking agent, and a colorant as required. As the silane coupling agent, for example, an epoxy silane coupling agent may be mentioned. As the filler, for example, inorganic fillers such as calcium carbonate, aluminum hydroxide, magnesium hydroxide, antimony trioxide, zinc borate, molybdenum compounds, and titanium dioxide may be mentioned. As the antioxidant, for example, a phenolic antioxidant and a sulfur antioxidant may be mentioned.
[0162] (2) Composition of adhesive layer
[0163] The adhesive layer can be foamed at a foaming ratio of, for example, 1.5 times or more and 15 times or less. The above-mentioned foaming ratio can be, for example, 3.5 times or more, 4 times or more, or 4.5 times or more. In addition, the above-mentioned foaming ratio can be, for example, 9 times or less, 8.5 times or less, or 8 times or less. When the average particle size of the foaming agent is within a specified range, by making the above-mentioned foaming ratio 3.5 times or more and 9 times or less, there is a tendency that the adhesion becomes higher when the gap between the components is wide. On the other hand, if the above-mentioned foaming ratio is too small, there is a possibility that the adhesion is reduced when the gap between the components is wide. In addition, if the above-mentioned foaming ratio is too large, the adhesion is sometimes reduced even when the gap between the components is narrow.
[0164] Here, the expansion ratio can be calculated by the following formula.
[0165] Foaming ratio (times) = thickness of adhesive layer after foaming and curing / thickness of adhesive layer before foaming and curing
[0166] The average thickness of the adhesive layer is not particularly limited, and is preferably above the average particle size of the foaming agent, for example, above 10 μm, above 15 μm, or above 20 μm. If the adhesive layer is too thin, there is a possibility that the adhesion to the substrate and the adhesion after foaming and curing cannot be fully obtained. On the other hand, the average thickness of the adhesive layer is, for example, below 200 μm, below 150 μm, or below 100 μm. If the adhesive layer is too thick, there is a possibility that the surface quality deteriorates or the pencil hardness decreases.
[0167] Here, the average thickness of the adhesive layer is a value measured based on a cross section in the thickness direction of the foamable adhesive sheet observed using a transmission electron microscope (TEM), a scanning electron microscope (SEM) or a scanning transmission electron microscope (STEM), and can be set as the average value of the thicknesses at 10 randomly selected locations. It should be noted that the method for measuring the average thickness of other layers of the foamable adhesive sheet can also be set in the same manner.
[0168] The adhesive layer may be a continuous layer or a discontinuous layer. Examples of the discontinuous layer include patterns such as stripes and dots. In addition, the surface of the adhesive layer may have a concave-convex shape such as embossing.
[0169] The adhesive layer can be formed, for example, by applying an adhesive composition containing the above-mentioned curable adhesive and a foaming agent and removing the solvent. Examples of the coating method include roll coating, reverse roll coating, transfer roll coating, gravure coating, gravure reverse coating, comma coating, rod coating, blade coating, rod coating, wire bar coating, die coating, die lip coating, and dip coating.
[0170] The adhesive composition may contain a solvent or may not contain a solvent. It should be noted that the solvent in this specification not only includes a strict solvent (a solvent that dissolves a solute), but also includes the broad meaning of a dispersion medium. In addition, the solvent contained in the adhesive composition evaporates and is removed when the adhesive composition is applied and dried to form an adhesive layer.
[0171] The adhesive composition can be obtained by mixing the above-mentioned components and kneading and dispersing as needed. As a mixing and dispersing method, a common kneading disperser can be used, such as a double-roll mill, a triple-roll mill, a gravel mill, a drum mill, a Szegvari grinder, a high-speed impeller disperser, a high-speed stone mill, a high-speed impact mill, a disperser, a high-speed mixer, a ribbon mixer, a bidirectional kneader, a strong mixer, a rotary drum, a stirrer, a dispensing machine, a homogenizer, and an ultrasonic disperser.
[0172] 3. Substrate
[0173] The substrate in the present invention preferably has insulating properties. In addition, the substrate is preferably in sheet form. The substrate sheet may have a single-layer structure or a multi-layer structure. In addition, the substrate sheet may have a porous structure inside or may not have a porous structure.
[0174] Examples of the substrate include a resin substrate and a nonwoven fabric.
[0175] As the resin contained in the resin substrate, for example, polyester resins such as polyethylene terephthalate (PET), polybutylene terephthalate, polyethylene naphthalate (PEN), and aromatic polyesters; polycarbonate; polyarylate; polyurethane; polyamide resins such as polyamide and polyether amide; polyimide resins such as polyimide, polyetherimide, and polyamideimide; polysulfone resins such as polysulfone and polyethersulfone; polyetherketone resins such as polyetherketone and polyetheretherketone; polyphenylene sulfide (PPS); modified polyphenylene ether, etc. The glass transition temperature of the resin is, for example, above 80°C, above 140°C, or above 200°C. In addition, a liquid crystal polymer (LCP) can be used as the resin.
[0176] Examples of the nonwoven fabric include nonwoven fabrics composed of fibers such as cellulose fibers, polyester fibers, nylon fibers, aramid fibers, polyphenylene sulfide fibers, liquid crystal polymer fibers, glass fibers, metal fibers, and carbon fibers.
[0177] Wherein, the substrate preferably contains polyphenylene sulfide (PPS) or polyethylene naphthalate (PEN). Polyphenylene sulfide and polyethylene naphthalate have high heat resistance, and are suitable for the situation that the foamable adhesive sheet is foamed and solidified by heating. In addition, polyphenylene sulfide and polyethylene naphthalate have high insulation, for example, the components can be insulated from each other by the adhesive sheet after foaming and solidification. In addition, polyphenylene sulfide and polyethylene naphthalate usually have poor wettability with adhesives, and have poor adhesion with adhesive layers, but in the present invention, the adhesion of adhesive layers to substrates can be improved. Therefore, a foamable adhesive sheet that balances heat resistance, insulation and adhesion between substrate and adhesive layer can be obtained.
[0178] In order to improve the adhesion with the adhesive layer, the surface of the substrate with the adhesive layer can be subjected to surface treatment. As surface treatment, for example, corona treatment, sandblasting, plasma treatment, flame treatment, silicon dioxide deposition (ITRO) treatment, hydrophilization treatment utilizing fluorine gas, etc. can be cited. In the above-mentioned surface treatment, preferably sandblasting. By making the adhesive layer fall into the fine concavo-convex of the sandblasted face of the substrate, the adhesion of the substrate and the adhesive layer becomes high, namely, the anchoring effect is obtained. In addition, sandblasting is a roughening treatment, and it is believed that compared with the surface activation treatments such as corona treatment, the adhesion of the substrate and the adhesive layer is stable.
[0179] In addition, a surface treatment layer may be arranged on the surface of the substrate on which the adhesive layer of the substrate is arranged. Examples of the surface treatment layer include silicon oxide films, etc. Examples of methods for forming the surface treatment layer include CVD methods, PVD methods, etc.
[0180] The average thickness of the substrate is not particularly limited, and is, for example, 2 μm or more, 5 μm or more, or 9 μm or more. The average thickness of the substrate is, for example, 200 μm or less, 100 μm or less, or 50 μm or less.
[0181] 4. Middle layer
[0182] The foamable adhesive sheet among the present invention preferably has an intermediate layer between base material and the adhesive layer.By configuring the intermediate layer, the adhesion of the adhesive layer to the base material can be further improved.In addition, by configuring the intermediate layer, the stress applied to the bending portion when the foamable adhesive sheet is bent can be relaxed, or the stress applied to the cut-off portion when the foamable adhesive sheet is cut can be relaxed.As a result, not only when the foamable adhesive sheet is bent, but also when cutting, the adhesive layer can be effectively suppressed from floating, peeling off of the base material.
[0183] For example, in Figure 3 In the foamable adhesive sheet 10 shown, the substrate 2, the intermediate layer 3 and the adhesive layer 1 are arranged in this order in the thickness direction. Figure 4In the foamable adhesive sheet 10 shown, a first adhesive layer 1a is disposed on one side of a substrate 2, a second adhesive layer 1b is disposed on the other side of the substrate 2, a first intermediate layer 3a is disposed between the substrate 2 and the first adhesive layer 1a, and a second intermediate layer 3b is disposed between the substrate 2 and the second adhesive layer 1b. Figure 4 In the embodiment, the foamable adhesive sheet 10 includes both the first intermediate layer 3a and the second intermediate layer 3b, but may include only one of them.
[0184] When adhesive layers are disposed on both sides of the substrate, it is sufficient to dispose an intermediate layer between the substrate and at least one adhesive layer. For example, an intermediate layer may be disposed only between the substrate and one adhesive layer, or between the substrate and two adhesive layers. Preferably, an intermediate layer is disposed between the substrate and the two adhesive layers.
[0185] The material contained in the intermediate layer is not particularly limited as long as it can improve the adhesion between the substrate and the adhesive layer and can relax the stress, and can be appropriately selected according to the materials of the substrate and the adhesive layer, etc. For example, polyester, polyvinyl chloride, polyvinyl acetate, polyurethane, polymers obtained by copolymerizing at least two of them, crosslinked products thereof, and mixtures thereof, etc. can be cited.
[0186] The crosslinked product is a crosslinked product formed by crosslinking the above-mentioned resin using a curing agent. As the curing agent, for example, an isocyanate curing agent can be cited. In addition, for example, when the reactive group / NCO equivalent is set to 1, the isocyanate curing agent is preferably added at a ratio of 0.5 mass % or more and 20 mass % or less relative to the resin.
[0187] Wherein, the middle layer preferably contains crosslinked resin.It should be noted that crosslinked resin refers to a resin that is not molten even if it is made into high temperature.Thus, it is possible to improve the bonding force at high temperature, i.e. heat resistance.In addition, when the crosslinked resin is for example crosslinked by an isocyanate curing agent, the flexibility of the middle layer becomes good, and it is possible to suppress the rupture of the adhesive layer when the foamable adhesive sheet is bent, the floating and peeling of the adhesive layer from the base material.
[0188] As the cross-linked resin, for example, the above-mentioned cross-linked products can be cited. Among them, the intermediate layer preferably contains a cross-linked polyester resin. If the intermediate layer contains a cross-linked polyester resin, there is a tendency that the adhesion between the substrate and the adhesive layer becomes higher. In particular, when the substrate contains polyphenylene sulfide (PPS) or polyethylene naphthalate (PEN) and the adhesive layer contains an epoxy resin-based adhesive as a curable adhesive, the adhesion between the substrate and the adhesive layer can be improved by containing a cross-linked polyester resin in the intermediate layer.
[0189] The cross-linked polyester resin is a cross-linked product of polyester, a copolymer containing polyester, or a mixture containing polyester, and specifically, a cross-linked product formed by cross-linking polyester, a copolymer containing polyester, or a mixture containing polyester using a curing agent. Examples of the polyester include polyester polyols, etc. Examples of the curing agent include isocyanate curing agents. It should be noted that the amount of the curing agent added is as described above.
[0190] The average thickness of the intermediate layer is not particularly limited as long as the peeling force of the surface side of the foamable adhesive sheet configured with the adhesive layer measured by the SAICAS method can be more than the specified value, for example, more than 0.1 μm, more than 0.5 μm, or more than 1 μm. If the intermediate layer is too thin, there is the possibility that the adhesive layer can not be fully obtained from the effect of peeling off from the substrate when the foamable adhesive sheet is bent and cut. On the other hand, the average thickness of the intermediate layer is, for example, less than 4 μm, and can be less than 3.5 μm. The intermediate layer itself is usually not high in heat resistance, so if the intermediate layer is too thick, there is the possibility that heat resistance (adhesion at high temperature) is reduced. It should be noted that, in the case of a substrate with a relatively high heat resistance such as polyethylene naphthalate (PEN), polyphenylene sulfide (PPS), by setting the average thickness of the intermediate layer to more than 0.5 μm and less than 4 μm, it is possible to make adhesion and heat resistance further good.
[0191] The intermediate layer can be formed, for example, by applying the resin composition and removing the solvent. Examples of the coating method include roll coating, reverse roll coating, transfer roll coating, gravure coating, gravure reverse coating, comma coating, rod coating, blade coating, rod coating, wire bar coating, die coating, die lip coating, and dip coating.
[0192] 5. Foam adhesive sheet
[0193] The average thickness of the foamable adhesive sheet in the present invention is, for example, 10 μm or more, or 20 μm or more. On the other hand, the average thickness of the foamable adhesive sheet is, for example, 1000 μm or less, or 200 μm or less.
[0194] The purpose of the foamable adhesive sheet in the present invention is not particularly limited. The foamable adhesive sheet in the present invention can be used in the case where the components are bonded to each other, for example, by disposing the foamable adhesive sheet between the components and then foaming and curing the foamable adhesive sheet. In addition, in the present invention, when the foamable adhesive sheet is disposed between the components, even when there are burrs on the components, the floating and peeling of the adhesive layer from the substrate can be suppressed, so it can be used for bonding metal components and resin components that are prone to burrs during processing. Among them, the foamable adhesive sheet in the present invention can be preferably used for disposing the foamable adhesive sheet between metal components and bonding the components to each other.
[0195] 6. Method for manufacturing foamable adhesive sheet
[0196] The manufacture method of the foamable adhesive sheet in the present invention is not particularly limited. For example, a method for forming an adhesive layer by applying the above-mentioned adhesive composition on a side of a substrate and drying it can be enumerated. In the case where a first adhesive layer is formed on a side of a substrate and a second adhesive layer is formed on another side of the substrate, the first adhesive layer and the second adhesive layer can be formed sequentially or simultaneously. By forming the second adhesive layer after forming the first adhesive layer, the first adhesive layer can be further dried, and the peeling force on the side of the first adhesive layer of the foamable adhesive sheet can be higher than the peeling force on the side of the second adhesive layer.
[0197] B. How the item is made
[0198] The method for manufacturing an article in the present invention comprises a placement step of placing the foamable adhesive sheet between a first member and a second member, and a bonding step of foaming and curing the foamable adhesive sheet to bond the first member and the second member.
[0199] Figure 5 1 is a process diagram showing an example of a method for manufacturing an article of the present invention. Figure 5 As shown in (a), a foamable adhesive sheet 10 is disposed between the first member 20a and the second member 20b. Figure 5 As shown in (b), the foamable adhesive sheet 10 is foamed and cured by heating, for example. The first member 20a and the second member 20b are bonded (joined) by the foamed and cured adhesive sheet 11. Thus, the article 100 having the adhesive sheet 11 disposed between the first member 20a and the second member 20b is obtained.
[0200] In the manufacturing method of the article of the present invention, since the above-mentioned foamable adhesive sheet is used, the adhesive layer has excellent adhesion to the substrate. Even if there are burrs on at least one of the first component and the second component, when the foamable adhesive sheet is inserted into the gap of one component or the gap between two components, when the foamable adhesive sheet is inserted into the gap after the foamable adhesive sheet is arranged in one component and another component is inserted, it is possible to suppress the adhesive layer from floating or peeling off from the substrate. In addition, when the foamable adhesive sheet is arranged between the first component and the second component, even if the foamable adhesive sheet is bent in advance, it is possible to suppress the adhesive layer from floating or peeling off from the substrate. Therefore, an article with good adhesion between the first component and the second component can be obtained.
[0201] Hereinafter, the method for producing the article of the present invention will be described.
[0202] 1. Foam adhesive sheet
[0203] In the manufacturing method of the article in the present invention, as the foamable adhesive sheet, the above-mentioned foamable adhesive sheet can be used, which is sequentially provided with an adhesive layer and a substrate, and the peeling force measured by the SAICAS method on the side provided with the adhesive layer is 2.0N or more. In addition, as the foamable adhesive sheet, a foamable adhesive sheet having a first adhesive layer and a second adhesive layer as adhesive layers, and sequentially provided with the first adhesive layer, a substrate, and a second adhesive layer in the thickness direction can be used. In this case, the peeling force of at least one of the side provided with the first adhesive layer and the side provided with the second adhesive layer of the foamable adhesive sheet measured by the SAICAS method is 2.0N or more.
[0204] In addition, since the details of the foamable adhesive sheet are described in the above-mentioned section "A. Foamable adhesive sheet", the description here is omitted.
[0205] 2. Configuration process
[0206] In the configuration process of the present invention, there is no particular limitation on the method for configuring the foaming adhesive sheet between the first component and the second component. For example, there can be cited a method of inserting the foaming adhesive sheet into the gap between the first component and the second component, a method of configuring the foaming adhesive sheet in the first component and then inserting the second component into the gap after configuring the foaming adhesive sheet in the first component, etc.
[0207] 3. Bonding process
[0208] In the bonding process of the present invention, as a method for foaming and curing the foamable adhesive sheet, heating or light irradiation can be cited. Among them, it is preferred to foam and cure the foamable adhesive sheet by heating. The method based on heating can also be applied when the first member and the second member are not transparent, such as metal members.
[0209] The heating conditions are appropriately set according to the curable adhesive contained in the adhesive layer, the type of the foaming agent, the type of the substrate, etc. The heating temperature can be set to, for example, 130° C. to 200° C. The heating time can be set to, for example, 3 minutes to 3 hours.
[0210] It should be noted that the present invention is not limited to the above-mentioned embodiments. The above-mentioned embodiments are for illustration only, and any technical solution having substantially the same structure and having the same function and effect as the technical solution described in the present invention is included in the technical scope of the present invention.
[0211] Example
[0212] [Example 1]
[0213] First, an adhesive composition having a composition (mass %) shown in the following Table 1 was prepared. Table 2 shows the details of each material described in Table 1.
[0214] In addition, as a substrate, a polyphenylene sulfide film (PPS film, manufactured by Toray Industries, TORELINA 100-3A30, thickness 100 μm) with high insulation is used, and a corona treatment is implemented in a manner where the surface tension is 70 dynes or more. The above-mentioned adhesive composition is applied to one surface of the substrate using an applicator in a manner where the thickness after coating is 45 μm. Then, it is dried in an oven at 100° C. for 3 minutes to form a first adhesive layer. In addition, on the other side of the substrate, the second adhesive layer is formed in the same manner as the above-mentioned first adhesive layer. Thus, a foamable adhesive sheet having a first adhesive layer and a second adhesive layer formed on both sides of the substrate is obtained.
[0215] [Example 2]
[0216] A foamable adhesive sheet was produced in the same manner as in Example 1 except that the substrate was subjected to sandblasting so as to have an arithmetic mean roughness of Ra 0.64 μm.
[0217] [Comparative Example 1]
[0218] A foamable adhesive sheet was prepared in the same manner as in Example 1 except that an adhesive composition having a composition (mass %) shown in Table 1 below was used.
[0219] [Example 3]
[0220] An adhesive composition having a composition (mass %) shown in the following Table 1 was used. In addition, as a substrate, a highly insulating polyphenylene sulfide film (PPS film, thickness 100 μm, arithmetic mean roughness Ra 0.64 μm) subjected to the same sandblasting treatment as in Example 2 was used. Otherwise, the same operation as in Example 1 was carried out to produce a foamable adhesive sheet.
[0221] [Example 4]
[0222] As a substrate, a polyphenylene sulfide film (PPS film, thickness 100 μm) with high insulation properties was prepared in the same manner as in Example 1. In addition, a curing agent (polyisocyanate) was added in a ratio of 2 parts by mass to 100 parts by mass of a mixture of polyester and polyvinyl chloride, and the mixture was further diluted with methyl ethyl ketone (MEK) in such a manner that the solid content became 15% by mass to prepare a resin composition. The resin composition was applied to one side of the substrate using a rod coater, and dried in an oven at 120° C. for 3 minutes to form a first intermediate layer with a thickness of 2 μm. In addition, on the other side of the substrate, a second intermediate layer was formed in the same manner as the first intermediate layer.
[0223] Next, the same adhesive composition as in Example 3 was used to form the first adhesive layer and the second adhesive layer for the first intermediate layer and the second intermediate layer, respectively, by the same method as in Example 1. Thus, a foamable adhesive sheet having the first adhesive layer, the first intermediate layer, the substrate, the second intermediate layer, and the second adhesive layer arranged in this order was obtained.
[0224] [Comparative Example 2]
[0225] A foamable adhesive sheet was prepared in the same manner as in Comparative Example 1 except that a highly insulating polyethylene naphthalate film (PEN film, manufactured by Toyobo Film Solutions, Teonex Q51-100, thickness 100 μm) was used as the substrate and corona treatment was performed so that the surface tension became 70 dynes or more.
[0226] [Example 5]
[0227] The same adhesive composition as in Example 3 was used. In addition, as a substrate, a highly insulating polyethylene naphthalate film (PEN film, thickness 100 μm) was used as in Comparative Example 2. Sandblasting was performed so that the arithmetic mean roughness Ra became 0.77 μm. Except for this, the same operation was performed as in Example 1 to produce a foamable adhesive sheet.
[0228] [Example 6]
[0229] A foamable adhesive sheet was prepared in the same manner as in Example 4 except that a polyethylene naphthalate film (PEN film, thickness 100 μm) having high insulation properties similar to that in Comparative Example 2 was used as the substrate.
[0230] [Comparative Example 3]
[0231] A foamable adhesive sheet was prepared in the same manner as in Example 1 except that an adhesive composition having a composition (mass %) shown in Table 1 below was used.
[0232] [Example 7]
[0233] A foamable adhesive sheet was prepared in the same manner as in Example 2 except that an adhesive composition having a composition (mass %) shown in Table 1 below was used.
[0234] [Example 8]
[0235] As a substrate, a highly insulating polyphenylene sulfide film (PPS film, manufactured by Toray Industries, TORELINA 115-3F00, thickness 115 μm) was used. In addition, with respect to 100 parts by mass of the polyester polymer, 15 parts by mass of a curing agent (polyisocyanate) and 0.3 parts by mass of a catalyst (tris(dimethylaminomethylphenol)) were mixed, and further diluted with methyl ethyl ketone (MEK) to make the solid content 15% by mass to prepare a resin composition. On one side of the above-mentioned substrate, the above-mentioned resin composition was applied with a rod coater, and dried in an oven at 100°C for 1 minute to form a first intermediate layer with a thickness of 2 μm. In addition, on the other side of the substrate, the second intermediate layer was formed in the same manner as the above-mentioned first intermediate layer.
[0236] Next, on the surface opposite to the substrate of the first intermediate layer, an adhesive composition of the composition (mass %) shown in the following Table 1 was applied using an applicator in such a manner that the thickness after coating became 38 μm. Then, it was dried in an oven at 100° C. for 3 minutes to form a first adhesive layer. In addition, on the surface opposite to the substrate of the second intermediate layer, the second adhesive layer was formed in the same manner as the first adhesive layer. Thus, a foamable adhesive sheet having a first adhesive layer, a first intermediate layer, a substrate, a second intermediate layer, and a second adhesive layer was obtained.
[0237] [Example 9]
[0238] A foamable adhesive sheet was prepared in the same manner as in Example 8 except that an adhesive composition having a composition (mass %) shown in Table 1 below was used.
[0239] [Evaluation 1]
[0240] (Peel force)
[0241] The peeling force of the surface side of the foaming adhesive sheet with the first adhesive layer and the peeling force of the surface side with the second adhesive layer are measured using a surface interface cutting test device. First, the foaming adhesive sheet is cut into 5cm×5cm, the foaming adhesive sheet is fixed to a vacuum holder, and the adhesive layer is cut using a cutting edge. Specifically, first, after the adhesive layer is cut from one surface of the foaming adhesive sheet in an inclined direction using a cutting edge, at the moment when the force applied to the cutting edge has just changed significantly and the horizontal force applied to the cutting edge has decreased, it is cut only in a direction horizontal to the foaming adhesive sheet. Then, the horizontal force applied to the cutting edge during cutting is measured. The horizontal force applied to the cutting edge when the cutting edge is only cut in a direction horizontal to the foaming adhesive sheet is equivalent to the above-mentioned peeling force. The above-mentioned peeling force is measured on the surface of the first adhesive layer side and the surface of the second adhesive layer side of the foaming adhesive sheet, respectively. The surface interface cutting test device uses the SAICASDN-GS type manufactured by DAIPLA WINTES. The cutting edge used was made of borazon alloy and had a blade width of 1.0 mm, a rake angle of 20°, and a relief angle of 10°. The measurement conditions were as follows.
[0242] Measurement mode: Constant speed mode
[0243] Horizontal speed: 2μm / sec
[0244] Vertical speed: 0.1μm / sec
[0245] Temperature: 23℃
[0246] (L-shaped bending test)
[0247] Cut the foamable adhesive sheet into 3 cm × 3 cm pieces, and bend the foamable adhesive sheet in half by 90° so that the surface with the adhesive layer to be tested is on the inside, and the size is 3 cm × 1.5 cm. Then, check whether the adhesive layer floats from the substrate. The adhesion based on the L-shaped bending test is evaluated according to the following criteria.
[0248] A: The bent part does not float
[0249] B: The bent part is floating
[0250] (Cross bending test)
[0251] Cut the foamable adhesive sheet into 3 cm × 3 cm, and bend the foamable adhesive sheet in half 180° so that the surface with the adhesive layer to be tested is inside and the size is 3 cm × 1.5 cm. Next, bend the foamable adhesive sheet in this state in half 180° so that the size is 1.5 cm × 1.5 cm. Then, check whether the adhesive layer floats from the substrate. The adhesion based on the cross bending test is evaluated according to the following criteria.
[0252] A: The bent part does not float
[0253] B: The bent part is floating
[0254] (Cutter cutting test)
[0255] The surface of the foamable adhesive sheet with the adhesive layer to be tested was cut with a cutter (Orpha, Cutter A Plus) at a speed of 20 mm / s or more and 100 mm / s or less to a length of 100 mm, and it was confirmed whether the adhesive layer floated from the substrate on the cut surface. The adhesion based on the cutter cutting test was evaluated according to the following criteria.
[0256] A: The cut surface has no floating at all
[0257] B: The cut surface has a little floating
[0258] C: The cut surface is completely floated
[0259] (Adhesion)
[0260] The foamable adhesive sheet was cut into a width of 24 mm and a length of 300 mm, and one adhesive layer of the foamable adhesive sheet was attached to a stainless steel plate (SUS304) using a hand roller. Then, the adhesive strength (N / 25 mm) to the stainless steel plate surface was measured using a tensile tester (TensilonRTF1150, manufactured by A&D Co., Ltd.) under the conditions of JIS Z0237:2009 (Testing methods for adhesive tapes and adhesive sheets) based on ISO 29862 and method 1 of the adhesive strength test method (testing method in which the tape and sheet are peeled off 180° from the stainless steel test plate at a temperature of 23°C and a humidity of 50%) (tensile speed: 300 mm / min, peeling distance: 150 mm, peeling angle: 180°).
[0261] [Table 1]
[0262]
[0263] [Table 2]
[0264]
[0265] As shown in Table 1, in Examples 1 to 9, the adhesion based on the L-shaped bending test and the adhesion based on the cross bending test are both good. In addition, in Examples 2, 3, 5, and 7, since the substrate is subjected to sandblasting, the adhesion based on the cutter cutting test is also good. In addition, in Examples 4, 6, 8, and 9, since an intermediate layer is disposed between the substrate and the adhesive layer, the adhesion based on the cutter cutting test is excellent. In contrast, in Comparative Examples 1 to 3, since the peeling force measured by the SAICAS method is small, the adhesion based on the L-shaped bending test and the adhesion based on the cross bending test are both poor. It should be noted that the test results of the surface side of the first adhesive layer of the foaming adhesive sheet are the same as the test results of the surface side of the second adhesive layer.
[0266] [Examples 10 to 23]
[0267] First, an adhesive composition having a composition (mass %) shown in the following Table 3 was prepared. Details of each material other than the foaming agent described in Table 3 are shown in Table 2. As the foaming agent, the following thermal foaming agents 1 to 8 were used.
[0268] Thermal foaming agent 1: thermally expandable microcapsules, average particle size 7 μm, expansion starting temperature 120-145°C, maximum expansion temperature 155-175°C, core: hydrocarbon, shell: thermoplastic polymer
[0269] Thermal foaming agent 2: thermally expandable microcapsules, average particle size 13 μm, expansion starting temperature 123-133°C, maximum expansion temperature 168-178°C, core: hydrocarbon, shell: thermoplastic polymer
[0270] Thermal foaming agent 3: thermally expandable microcapsules, average particle size 17 μm, expansion starting temperature 120-130°C, maximum expansion temperature 160-170°C, core: hydrocarbon, shell: acrylonitrile copolymer
[0271] Thermal foaming agent 4: thermally expandable microcapsules, average particle size 20 μm, expansion starting temperature 115-125°C, maximum expansion temperature 155-165°C, core: hydrocarbon, shell: thermoplastic polymer
[0272] Thermal foaming agent 5: thermally expandable microcapsules, average particle size 21 μm, expansion starting temperature 130-140°C, maximum expansion temperature 160-170°C, core: hydrocarbon, shell: acrylonitrile copolymer
[0273] Thermal foaming agent 6: thermally expandable microcapsules, average particle size 25 μm, expansion starting temperature 125-135°C, maximum expansion temperature 165-180°C, core: hydrocarbon, shell: thermoplastic polymer
[0274] Thermal foaming agent 7: thermally expandable microcapsules, average particle size 30 μm, expansion starting temperature 120-130°C, maximum expansion temperature 160-170°C, core: hydrocarbon, shell: acrylonitrile copolymer
[0275] Thermal foaming agent 8: thermally expandable microcapsules, average particle size 41 μm, expansion starting temperature 115-125°C, maximum expansion temperature 165-175°C, core: hydrocarbon, shell: acrylonitrile copolymer
[0276] As a substrate, a highly insulating polyphenylene sulfide film (PPS film, manufactured by Toray Industries, TORELINA 115-3F00, thickness 115 μm) was used. In addition, with respect to 100 parts by mass of the polyester polymer, 15 parts by mass of a curing agent (polyisocyanate) and 0.3 parts by mass of a catalyst (tris(dimethylaminomethylphenol)) were mixed, and further diluted with methyl ethyl ketone (MEK) to make the solid content 15% by mass to prepare a resin composition. On one side of the above-mentioned substrate, the above-mentioned resin composition was applied with a rod coater, and dried in an oven at 100°C for 1 minute to form a first intermediate layer with a thickness of 2 μm. In addition, on the other side of the substrate, the second intermediate layer was formed in the same manner as the above-mentioned first intermediate layer.
[0277] Next, the adhesive composition is applied to the surface of the first intermediate layer opposite to the substrate using an applicator in a manner such that the thickness after application becomes 38 μm. Then, it is dried in an oven at 100° C. for 3 minutes to form a first adhesive layer. In addition, the surface of the second intermediate layer opposite to the substrate is operated in the same manner as the first adhesive layer to form a second adhesive layer. Thus, a foamable adhesive sheet having a first adhesive layer, a first intermediate layer, a substrate, a second intermediate layer, and a second adhesive layer arranged in sequence is obtained.
[0278] [Reference example]
[0279] Production of an adhesive sheet containing no foaming agent Specifically, an adhesive sheet was produced in the same manner as in Example 10 except that an adhesive composition having a composition (mass %) shown in Table 3 below was used.
[0280] [Evaluation 2]
[0281] (Peel force)
[0282] In the same manner as in Example 1, the peeling force of the foamable adhesive sheet on the side where the first adhesive layer was arranged and the peeling force of the foamable adhesive sheet on the side where the second adhesive layer was arranged were measured.
[0283] (L-shaped bending test)
[0284] In the same manner as in Example 1, the adhesion was evaluated by the L-shaped bending test.
[0285] (Cross bending test)
[0286] In the same manner as in Example 1, the adhesion was evaluated by the cross bending test.
[0287] (Cutter cutting test)
[0288] In the same manner as in Example 1, the adhesion was evaluated by a cutter cutting test.
[0289] (Adhesion)
[0290] In the same manner as in Example 1, the adhesive strength was measured.
[0291] (Coefficient of friction)
[0292] According to JIS K7125 corresponding to ISO 8295, the dynamic friction coefficient and static friction coefficient between the surface of the foamable adhesive sheet with the adhesive layer to be tested and the metal plate are measured. First, the foamable adhesive sheet is cut into 80mm×200mm. Next, the foamable adhesive sheet is placed on a horizontal rectangular metal plate, and a sliding sheet (63mm×63mm, weight 200g, bottom surface: felt) is placed on the surface of the foamable adhesive sheet with the adhesive layer to be tested. The friction force is measured under the conditions of a test speed of 100mm / min, a test length of 50mm, a force sensor of 10N, and a temperature of 23°C, and the dynamic friction coefficient and static friction coefficient are calculated. The device uses a friction measuring machine FRICTION TESTER TR-2 manufactured by Toyo Seiki Co., Ltd. In addition, the material of the stainless steel plate used as the metal plate is SUS304, and the surface roughness Ra is 0.05μm.
[0293] (Pencil hardness)
[0294] Prepare an A4-sized foaming adhesive sheet and place it on a glass plate. According to JIS K5600 corresponding to ISO 15184, use a pencil hardness tester (with a level) to measure the pencil hardness of the surface of the foaming adhesive sheet where the adhesive layer to be tested is arranged. The measurement conditions are set to an angle of 45° from the horizontal state of the pencil, a load of 750g, a test speed of 1mm / sec, a test length of 20mm, and a temperature of 23°C. Then, the hardness of the largest pencil that does not cause damage to the foaming adhesive sheet under visual observation is taken as the pencil hardness. The pencil hardness tester used is KT-VF2378-12 made by TQC.
[0295] (Insert weight)
[0296] Prepare 2 foam adhesive sheets cut into 5.5cm×6.0cm, a hollow cylinder 1 with an outer diameter of 22mm, a thickness of 1.5mm, and a length of 60mm, and a hollow cylinder 2 with an outer diameter of 18mm, a thickness of 1.0mm, and a length of 80mm. The two foam adhesive sheets are arranged inside the cylinder 1 in a state of overlapping and rolling up in such a way that the surfaces of the adhesive layers to be tested are all arranged inside. Next, a cylinder 2 of about 1mm is pre-inserted into the gap inside the foam adhesive sheet in the cylinder 1. Then, a weight is placed on the cylinder 2, and the weight of the weight when the cylinder 2 is completely inserted into the gap inside the foam adhesive sheet in the cylinder 1 is measured. The weight of the weight at this time is used as the insertion weight. The smaller the insertion weight, the better the insertion property.
[0297] (Foaming ratio)
[0298] The foamable adhesive sheet was cut into a size of 5 cm × 5 cm, hung in the vertical direction in a hot air dryer, foamed and cured at 180°C or 150°C for 30 minutes, and then cooled at room temperature for 2 hours to obtain a foamed and cured adhesive sheet. Then, the thickness of the foamed and cured adhesive sheet was measured using a thickness gauge according to the method of JIS Z0237. The foaming ratio was calculated by the following formula.
[0299] Foaming ratio (times) = {thickness of adhesive sheet after foaming and curing - (thickness of substrate + thickness of first intermediate layer + thickness of second intermediate layer)} / (total thickness of first adhesive layer and second adhesive layer of foamable adhesive sheet before foaming and curing)
[0300] (Adhesion)
[0301] like Figure 6 As shown in (a) and (b), two metal plates 31 (cold-rolled steel plate SPCC-SD) with a thickness of 1.6 mm, a width of 25 mm, and a length of 100 mm are prepared. A spacer 32 (Kapton tape) is arranged at a predetermined interval at one front end of one of the metal plates 31. The thickness of the spacer is set to about 280 μm or about 350 μm (the thickness of 4 or 5 overlapping Kapton Tape P-221 manufactured by Nitto Denko Corporation). A foam adhesive sheet 10 cut into 12.5 mm × 25 mm is arranged between the spacers 32, and another metal plate 31 is arranged in a manner that one front end overlaps.
[0302] For some, such as Figure 6 As shown in (a), a support member 33 having the same thickness as the total thickness of the metal plate 31 and the spacer 32 is respectively arranged at the front end of the other of the two metal plates 31 to obtain a test piece. Then, the test piece is placed in a hot press and heated at 150° C. for 8 minutes with a pressing load of 500 kgf to cure the foamable adhesive sheet 10.
[0303] The remaining portion was fixed with a jig to obtain a test piece. The test piece was then placed in a hot oven and heated at 180° C. for 30 minutes to cure the foamable adhesive sheet 10 .
[0304] The heated test piece was measured for shear strength (adhesive strength) using a tensile tester Tensilon RTF1350 (manufactured by A&D Co.) in accordance with JIS K6850 corresponding to ISO 4587. The measurement conditions were a tensile speed of 10 mm / min and a temperature of 200°C.
[0305] [Table 3]
[0306]
[0307] As shown in Table 3, in Examples 10 to 23, since an intermediate layer is disposed between the substrate and the adhesive layer, the adhesion based on the L-shaped bending test and the adhesion based on the cross bending test are both good, and the adhesion based on the cutter cutting test is also good. It should be noted that the test results of the surface side of the first adhesive layer of the foamable adhesive sheet are the same as the test results of the surface side of the second adhesive layer.
[0308] In addition, as shown in Table 3, the larger the average particle size of the foaming agent, the smaller the static friction coefficient and the dynamic friction coefficient, and the higher the pencil hardness. In addition, in Example 15, compared with Examples 10 and 12, the average particle size of the foaming agent is large, the static friction coefficient and the dynamic friction coefficient are small, the pencil hardness becomes higher, and the insertion weight becomes smaller. In addition, in Example 15, compared with the reference example, the static friction coefficient and the dynamic friction coefficient are small, the pencil hardness is high, and therefore the insertion weight becomes smaller. Thus, it is suggested that when the average particle size of the foaming agent is above a specified value, the sliding property and the insertion property become good. In addition, it is suggested that the friction coefficient and hardness of the surface of the adhesive layer side of the foaming adhesive sheet contribute to the insertion property. It should be noted that the evaluation results of the surface side of the first adhesive layer of the foaming adhesive sheet are shown in Table 3, and the evaluation results of the surface side of the first adhesive layer of the foaming adhesive sheet are roughly the same as the evaluation results of the second adhesive layer.
[0309] In addition, as shown in Table 3, in Examples 10 to 11 in which the average particle size of the foaming agent is 7 μm, the bonding strength when the gap is about 280 μm exceeds 0.51 MPa, which is good, but the bonding strength when the gap is about 350 μm decreases. On the other hand, in Examples 12 to 20 in which the average particle size of the foaming agent is 13 μm to 21 μm, the bonding strength when the gap is about 280 μm and when the gap is about 350 μm both exceed 0.51 MPa, which is good. In addition, in Examples 21 to 23 in which the average particle size of the foaming agent is 25 μm to 41 μm, the bonding strength when the gap is about 280 μm decreases. Thus, it is suggested that when the average particle size of the foaming agent is within a specified range, both the bonding property when the gap between components is relatively narrow and the bonding property when the gap between components is relatively wide become good.
[0310] Description of Reference Numerals
[0311] 1…adhesive layer;
[0312] 2…substrate;
[0313] 3…middle layer;
[0314] 10…Foaming adhesive sheet;
[0315] 11…adhesive sheet after foaming and curing;
[0316] 20a ... a first member;
[0317] 20b ... a second member;
[0318] 100…items.
Claims
1. A foamable adhesive sheet comprising a substrate and an adhesive layer disposed on at least one surface side of the substrate, The adhesive layer contains a curable adhesive and a foaming agent. The curable adhesive contains an epoxy resin and a curing agent. An intermediate layer is arranged between the substrate and the adhesive layer, The substrate is a resin substrate containing a resin having a glass transition temperature of 80° C. or higher, the intermediate layer contains a cross-linked polyester resin, and the average thickness of the intermediate layer is 0.5 μm or more and 4 μm or less, The peeling force of the surface on which the adhesive layer is disposed measured by the SAICAS method, that is, the surface and interface cutting analysis system method, is 2.0 N or more.
2. The foamable adhesive sheet according to claim 1, in, The adhesive force of the adhesive layer is 0 N / 25 mm or more and 0.1 N / 25 mm or less, The adhesive layer is disposed on the outermost surface.
3. The foamable adhesive sheet according to claim 1, in, The pencil hardness of the surface of the foamable adhesive sheet on the adhesive layer side is F or higher.
4. The foamable adhesive sheet according to claim 1, in, The static friction coefficient of the surface of the foamable adhesive sheet on the adhesive layer side is 0.30 or less.
5. The foamable adhesive sheet according to claim 1, in, The average particle size of the foaming agent is 10 μm or more and 24 μm or less.
6. The foamable adhesive sheet according to claim 5, in, The average thickness of the adhesive layer is equal to or greater than the average particle size of the foaming agent.
7. The foamable adhesive sheet according to claim 6, in, The average thickness of the adhesive layer is 10 μm or more and 200 μm or less.
8. The foamable adhesive sheet according to claim 5, in, When the resin component contained in the adhesive layer is 100 parts by mass, the content of the foaming agent is 3 parts by mass or more and 25 parts by mass or less.
9. The foamable adhesive sheet according to claim 5, in, The adhesive layer can be foamed at a foaming ratio of 3.5 times or more and 9 times or less.
10. The foamable adhesive sheet according to claim 1, in, The bending moment of the foamable adhesive sheet is greater than or equal to 3 gf·cm and less than 40 gf·cm.
11. A method for manufacturing an article, comprising: a disposing step of disposing the foamable adhesive sheet according to claim 1 between the first member and the second member; and The bonding step is to foam and cure the foamable adhesive sheet to bond the first member and the second member.
Citation Information
Patent Citations
Tacky adhesive layer and tacky adhesive sheet
JP2014065889A
Adhesive sheet
JP2019203062A
Adhesive sheet
WO2016163514A1
Substrate-less double-sided pressure-sensitive adhesive sheet
CN103857761A
Binder for electrochemical cells, paste for electrochemical cells, and method for producing electrode for electrochemical cells
CN105794029A
Cited By
Preparation method of expansion insulating sheet
CN120623950A