A basic carbon material catalyst and its preparation method and application

Through the alkaline carbon material catalyst based on industrial solid waste, the problem of heavy components and carbon analytical blockage in tar gas in low-order pulverized coal pyrolysis process is solved, and the in-situ quality improvement of high dust-containing tar gas is achieved The carbon excretion inhibits the tar yield and quality and extends the service life of the dust removal system.

CN115364840BActive Publication Date: 2024-11-05SHANXI GEMENG SINO US CLEAN ENERGY R & D CENT CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211079369.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-05
Publication Date
2024-11-05
Estimated Expiration
2042-09-05

AI Technical Summary

Technical Problem

The high content of dust and heavy tar in tar gas in the low-order pulverized coal pyrolysis process leads to clogging of dust collectors and carbon analysis problems. It is difficult for the existing technology to effectively regulate tar quality and dust removal efficiency.

Method used

Develop an alkaline carbon material catalyst based on industrial solid waste, prepared by mixing with coal crushing with high bond index, water vapor and ammonia activation, filtering materials for particulate bed dust collectors, modulating the volatile reaction path , inhibit carbon analysis and quality improvement tar.

Benefits of technology

It achieves in-situ quality improvement and carbon extraction inhibition of high dust-containing tar gas, extends the service life of the dust removal system, improves the tar yield and quality, and reduces the dust removal pressure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115364840B_ABST
    Figure CN115364840B_ABST
Patent Text Reader

Abstract

The invention relates to an alkaline carbon material catalyst, which is prepared by pyrolysis of industrial solid waste containing alkaline metal oxides and caking coal with a high caking index, and activation by water vapor and ammonia. The industrial solid waste is any one or more of carbide slag, red mud and magnesium slag, and the caking coal with a high caking index is fat coal and / or coking coal with a caking index of 95 to 110. The catalyst is used as a filter material for a particle bed dust collector, and the synergistic effect of in-situ catalytic quality improvement and carbon precipitation inhibition of high-dust pyrolysis tar gas is achieved while removing dust.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a carbon material catalyst, and in particular to an alkaline carbon material catalyst based on industrial solid waste. The alkaline carbon material catalyst of the present invention can be applied to the graded and quality-differentiated conversion and utilization of low-grade pulverized coal with pyrolysis technology as the core, and is mainly used for the quality control and carbon deposition inhibition of dust- and oil-containing high-temperature pyrolysis tar gas in the particle bed dust removal process. Background Art

[0002] Clean and efficient development and utilization of coal has become an important foothold and primary goal of my country's energy transformation and development. Pyrolysis technology is an effective way to achieve clean and efficient utilization of coal. Through pyrolysis technology, solid coal can be converted into valuable liquid tar, which can be converted into high-value-added clean fuels such as high-quality gasoline, kerosene, aviation fuel, diesel, and naphtha after deep processing.

[0003] Low-rank coal reserves are abundant worldwide and are mainly pulverized coal. In order to achieve large-scale graded and quality-based transformation and utilization of low-rank pulverized coal and the green and low-carbon development of the coal industry, various pyrolysis technologies using low-rank pulverized coal as raw materials have been developed successively at home and abroad. However, all of them have problems such as poor tar quality and high dust content, resulting in many pyrolysis processes still in the pilot or industrial demonstration stage.

[0004] This is mainly due to the high content of dust and heavy tar in the dusty tar gas and the complex reaction of volatiles, which leads to the re-reaction of volatiles during the dust separation process and the difficulty in controlling the tar quality.

[0005] Under low temperature conditions, heavy tar is very easy to condense and agglomerate with dust, forming a high-viscosity mixture that adheres to the wall of the container or pipe, causing blockage of dust collectors, pipes, valves and other process equipment; under high temperature conditions, volatiles themselves and the entrained particles will undergo cracking, condensation, coking and other reactions, causing light tar to be converted into heavy tar, resulting in carbon deposition and coking, causing heavy tar and carbon deposition to adhere to the solid particles and the surface of the dust collector, reducing the dust removal efficiency and ultimately leading to system blockage.

[0006] The dust removal and carbon deposition problems in tar gas make it impossible for the device to operate stably for a long period of time, which is a key problem that needs to be urgently solved in the existing low-grade pulverized coal pyrolysis process.

[0007] Granular bed dust collector is considered to be an effective method to control the dust content in tar by filtering materials, but the problem of re-reaction carbon deposition caused by the high activity of volatiles cannot be avoided. The heavy components and carbon deposition in tar are very easy to adhere to the solid particles, dust collector and pipeline surface, reducing the dust removal efficiency and eventually causing the dust removal system to be blocked. Therefore, it is necessary to reduce the formation of carbon deposition by adjusting the reaction behavior of volatiles, thereby alleviating the subsequent oil-dust separation pressure of high-temperature tar gas.

[0008] Wang et al. (Fuel, 2021, 285, 119156) used semi-coke particle bed for catalytic upgrading of volatiles to improve the quality of tar, significantly increasing the yield of light fractions and light tar in tar, but did not give the carbon deposition of tar under the catalytic action of semi-coke. Wang et al. (ACS Omega, 2021, 6, 3800-3808) prepared coke filter material for particle bed dust removal of coal pyrolysis volatiles. The results showed that coke effectively upgraded tar and inhibited carbon deposition.

[0009] The above research proves that using carbon-based catalysts as filter materials for granular bed dust collectors can achieve the synergistic effect of in-situ quality improvement of volatiles and carbon deposition inhibition while filtering dust.

[0010] However, the material and physicochemical properties of the filter material greatly affect the thermal reaction behavior of dusty tar gas during the dust removal process, thereby affecting the yield, quality and carbon content of tar. The acid-base properties of the catalyst also have an important influence on the quality of coal pyrolysis tar. Although solid acid catalysts can improve the quality of tar, they have strong catalytic cracking activity on tar due to the presence of strong acid sites. On the one hand, strong acid sites lead to the condensation of macromolecules to produce carbon deposits and catalyst deactivation (Fuel, 2022, 321, 124030); on the other hand, strong acid sites promote the conversion of tar to pyrolysis gas and carbon deposition, resulting in a significant decrease in tar yield and weakening the economic efficiency of the pyrolysis process (Journal of Fuel Chemistry, 2021, 49(03), 257-264). The solid base catalyst has a relatively weak cracking effect on tar, and can promote the dehydrogenation of hydrocarbon substances during the conversion of pyrolysis volatiles, thereby increasing the hydrogen-rich small molecules in the pyrolysis system and reducing the condensation reaction between macromolecules, which can effectively inhibit carbon deposition while ensuring the tar yield.

[0011] Therefore, developing alkaline carbon-based catalysts with moderate activity as granular bed filter materials can achieve in-situ quality improvement and carbon deposition inhibition of dust-containing pyrolysis tar gas while ensuring tar yield, ultimately providing theoretical and technical support for the development of granular bed dust removal technology for dust-containing pyrolysis tar gas.

[0012] Carbide slag is the solid waste discharged when carbide is hydrolyzed to produce acetylene gas; red mud is the solid waste discharged when the aluminum industry refines alumina; magnesium slag is the solid waste discharged by magnesium metal plants during the magnesium smelting process. The common characteristics of these solid wastes are fine particle size and alkalinity. The alkalinity is a huge challenge currently faced by the resource disposal and utilization of carbide slag, red mud, and magnesium slag. However, industrial solid wastes such as carbide slag, red mud, and magnesium slag contain alkaline active components such as CaO, Fe2O3, and MgO. These metal components can not only adjust the acidity and alkalinity of carbon-based catalysts, but also catalyze the cracking of heavy tar and activate small molecules in volatiles to provide hydrogen, thereby inhibiting carbon deposition and effectively improving the quality of tar.

[0013] Based on the above situation, by developing an alkaline carbon material catalyst based on industrial solid waste to adjust the volatile reaction pathway, the synergistic effect of in-situ quality improvement and carbon precipitation inhibition of high-dust tar gas can be achieved during the particle bed dust removal process. In addition, the preparation of alkaline carbon material catalysts by mixed pyrolysis also provides a new high-value-added resource disposal method for alkaline industrial solid wastes such as carbide slag, red mud, and magnesium slag. Summary of the invention

[0014] The purpose of the present invention is to provide an alkaline carbon material catalyst. In order to solve the problems of high heavy components in the dusty tar gas produced by pyrolysis of low-grade pulverized coal, and volatiles reacting and carbonizing to block pipelines, the catalyst is used as a granular bed filter material to simultaneously achieve the synergistic effects of in-situ quality improvement and carbonization inhibition of high-dust pyrolysis tar gas during the granular bed dust removal process.

[0015] The present invention firstly provides an economically feasible method for preparing an alkaline carbon material catalyst, which can realize the recycling of industrial solid waste and prepare a shaped alkaline carbon material catalyst with moderate activity for application in particle bed filtration and dust removal, while lightening tar and inhibiting carbon deposition.

[0016] The method for preparing alkaline carbon material catalyst using industrial solid wastes of the present invention comprises: mixing industrial solid wastes containing alkaline metal oxides with caking coal having a high caking index for pyrolysis, and preparing the alkaline carbon material catalyst through steam activation and ammonia activation.

[0017] Specifically, the present invention provides a detailed preparation method of the alkaline carbon material catalyst.

[0018] 1) After industrial solid waste containing alkaline metal oxides and caking coal with a high caking index are crushed, particles with a sieve size of less than 0.15 mm are selected, and the mixture is fully kneaded at a ratio of 1 to 20 wt % of the industrial solid waste to obtain a mixed material.

[0019] 2) After moistening the mixed materials with water, press them into shapes to obtain briquettes.

[0020] 3) In an air-tight environment, the coal briquette is pressurized and heated to 450-950°C for pyrolysis to prepare a shaped carbon material with interconnected pores.

[0021] 4) The shaped carbon material is heated to 850-950°C in an inert atmosphere, water vapor is introduced to activate the shaped carbon material to further create pores, ammonia is introduced to activate the shaped carbon material to give the shaped carbon material alkaline active groups, and after cooling, an alkaline carbon material catalyst containing both alkaline metal oxides and active groups is prepared.

[0022] In the raw materials for preparing the alkaline carbon material catalyst of the present invention, the industrial solid waste containing alkaline metal oxides may include but is not limited to any one or more of carbide slag, red mud and magnesium slag.

[0023] The caking coal with a high caking index specifically refers to fat coal and / or coking coal with a caking index of 95-110.

[0024] Specifically, the present invention preferably adds 10 to 15 wt % of water to the mixed material to wet the mixed material.

[0025] Specifically, the present invention preferably performs compression molding on the wetted mixed material at a pressure of 3 to 9 MPa.

[0026] Specifically, during the pyrolysis of the briquette, the briquette is subjected to a pressure of 700 to 1200 N / m 2 pressure.

[0027] More specifically, the present invention preferably heats the shaped coal to 450-950°C at a heating rate of 0.5-2.5°C / min and pyrolyzes it at a constant temperature of 1.5-2.5h to prepare a shaped carbon material.

[0028] Specifically, the present invention heats the shaped carbon material to 750-950°C at a heating rate of 5-10°C / min under an inert atmosphere, introduces water vapor to activate it for 1-2 hours, and then introduces ammonia to activate it for 1-2 hours to prepare an alkaline carbon material catalyst.

[0029] More specifically, the ammonia gas described in the present invention is a mixed gas with nitrogen as the balance gas and an ammonia content of 30-70% by volume.

[0030] There are many ways to mix the industrial solid waste containing alkaline metal oxides with the caking coal with a high caking index to obtain the mixed material. For example, it can include but is not limited to mixing 1-20wt% of industrial solid waste with 80-99wt% of fat coal or coking coal; mixing 1-20wt% of industrial solid waste, 30-50wt% of fat coal and 30-69wt% of coking coal, and so on.

[0031] The alkaline carbon material catalyst prepared by the above method of the present invention can effectively adjust the physical and chemical properties of the carbon material, and can effectively adjust the content of metal active components and acidity and alkalinity by adjusting the mass fraction of industrial solid waste; and can effectively adjust the pore structure of the carbon material catalyst by adjusting the proportion of caking coal and activation time.

[0032] Therefore, the alkaline carbon material catalyst described in the present invention can be used as a filter material for a granular bed dust collector, and can be used for filtering, removing dust and catalytically upgrading the quality of dusty tar gas from pyrolysis of low-grade pulverized coal.

[0033] In the particle bed filtration and dust removal process of dusty tar gas from pyrolysis of low-grade pulverized coal, the alkaline carbon material catalyst can crack the heavy tar in the tar gas, effectively activate small molecular gas compounds such as CH4, CO2, H2, C2H6 and C3H6 in the volatiles, promote the migration of hydrogen radicals and the collision with other free radicals, thereby stabilizing the large molecular free radical cracking fragments in the tar gas and avoiding the occurrence of polycondensation reaction and the formation of carbon deposition.

[0034] By using the alkaline carbon material catalyst of the present invention as the filter material of the granular bed dust collector, the synergistic effect of in-situ quality improvement of high-dust tar gas and carbon deposition inhibition is simultaneously achieved during the granular bed dust removal process, thereby solving the problem of high heavy components in the pyrolysis dust-containing tar gas and volatile matter re-reaction carbon deposition blocking the pipeline.

[0035] In addition, the alkaline carbon material catalyst prepared by the present invention is conducive to promoting the removal of N, S heterocyclic compounds and oxygen-containing compounds in tar, generating more monocyclic aromatic hydrocarbons, and effectively catalyzing the quality improvement of tar.

[0036] Furthermore, the alkaline carbon material catalyst described in the present invention can also be used to catalyze the tar catalytic reforming reaction in the process of biomass and coal gasification, promote the conversion of high carbon matrix components in tar to low carbon matrix components, effectively eliminate tar and inhibit carbon deposition, thereby extending the service life of the carbon material. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 These are SEM images of the alkaline carbon material catalysts prepared in Examples 1 to 3.

[0038] Figure 2 It is the XRD diagram of the alkaline carbon material catalyst prepared in Examples 1 to 3.

[0039] Figure 3 It is the tar yield of pyrolysis dust-containing tar gas after catalytic upgrading by alkaline carbon material catalyst.

[0040] Figure 4 It is a comparison of the relative contents of various chemical components in pyrolysis dust-containing tar gas after catalytic upgrading by alkaline carbon material catalyst.

[0041] Figure 5 It is a comparison of tar yields after catalytic reforming of biomass gasification tar gas over alkaline carbon material catalysts. DETAILED DESCRIPTION

[0042] The specific implementation of the present invention is further described in detail below in conjunction with the accompanying drawings and examples. The following examples are only used to more clearly illustrate the technical solution of the present invention so that those skilled in the art can well understand and utilize the present invention, rather than limiting the scope of protection of the present invention.

[0043] The names and abbreviations of the experimental methods, production processes, instruments and equipment involved in the embodiments and comparative examples of the present invention are conventional names in the field and are very clear and unambiguous in the relevant application fields. Those skilled in the art can understand the conventional process steps and apply the corresponding equipment based on the names and implement them according to conventional conditions or conditions recommended by the manufacturer.

[0044] The various raw materials or reagents used in the examples and comparative examples of the present invention are not particularly limited in terms of their sources, and are all conventional products that can be purchased commercially, or can be prepared according to conventional methods well known to those skilled in the art.

[0045] Example 1.

[0046] Industrial solid waste carbide slag and Liulin coking coal with adhesiveness were used as raw materials, which were crushed and sieved to a particle size less than 0.15 mm, respectively, and then mixed in a mass ratio of carbide slag to Liulin coking coal of 1:9 and fully kneaded to obtain a mixed sample.

[0047] The mixed sample was mixed with deionized water at a mass ratio of 10:1, stirred thoroughly and evenly, placed in a metal mold, and molded on a pressure molding machine at a pressure of 7 MPa to obtain coal briquettes.

[0048] The briquette is placed in a corundum crucible and a 1200N / m 2 The carbon material was prepared by heating the sample to 500°C at a rate of 1°C / min from room temperature and then cooling the muffle furnace to room temperature to obtain a shaped carbon material.

[0049] The shaped carbon material was placed in a tubular furnace and heated from room temperature to 750°C at a heating rate of 10°C / min under an inert atmosphere. 0.042 mL / (min·g) of water vapor was introduced for activation for 2 h, and then a 50% ammonia mixed gas (nitrogen as the balance gas) was introduced for activation for 1 h. After cooling to room temperature, an alkaline carbon material catalyst was obtained, which was named CM-1.

[0050] Example 2.

[0051] Industrial solid waste carbide slag and Liulin coking coal with adhesiveness were used as raw materials, which were crushed and sieved to a particle size less than 0.15 mm, mixed in a mass ratio of carbide slag to Liulin coking coal of 3:17, and fully kneaded to obtain a mixed sample.

[0052] The mixed sample was mixed with deionized water at a mass ratio of 10:1, stirred thoroughly and evenly, placed in a metal mold, and molded on a pressure molding machine at a pressure of 6.5 MPa to obtain coal briquettes.

[0053] The briquette is placed in a corundum crucible and a 1200N / m 2 The carbon material was prepared by heating the sample in a muffle furnace at a heating rate of 1°C / min from room temperature to 850°C and maintaining the temperature for 2 hours. The muffle furnace was then cooled to room temperature to obtain a shaped carbon material.

[0054] The shaped carbon material was placed in a tubular furnace and heated from room temperature to 850°C at a heating rate of 10°C / min under an inert atmosphere. 0.042 mL / (min·g) of water vapor was introduced for activation for 2 h, and then a 45% ammonia mixed gas (nitrogen as the balance gas) was introduced for activation for 1 h. After cooling to room temperature, an alkaline carbon material catalyst was obtained, which was named CM-2.

[0055] Example 3.

[0056] Industrial solid waste carbide slag and Liulin coking coal with adhesiveness were used as raw materials, which were crushed and sieved to a particle size less than 0.15 mm, mixed in a mass ratio of 1:4 between carbide slag and Liulin coking coal, and fully kneaded to obtain a mixed sample.

[0057] The mixed sample was mixed with deionized water at a mass ratio of 10:1, stirred thoroughly and evenly, placed in a metal mold, and molded on a pressure molding machine at a pressure of 7 MPa to obtain coal briquettes.

[0058] The briquette is placed in a corundum crucible and a 1200N / m 2 The carbon material was prepared by heating the sample to 900°C at a heating rate of 1.5°C / min from room temperature and then cooling the muffle furnace to room temperature to obtain a shaped carbon material.

[0059] The shaped carbon material was placed in a tubular furnace and heated from room temperature to 900°C at a heating rate of 10°C / min under an inert atmosphere. 0.042 mL / (min·g) of water vapor was introduced for activation for 1.5 h, and then a 60% ammonia mixed gas (nitrogen as the balance gas) was introduced for activation for 2 h. After cooling to room temperature, an alkaline carbon material catalyst was obtained, which was named CM-3.

[0060] Example 4.

[0061] Industrial solid waste red mud and Liulin coking coal with adhesiveness were used as raw materials, which were crushed and sieved to a particle size of less than 0.15 mm, respectively, and then mixed in a mass ratio of red mud to Liulin coking coal of 1:9 and fully kneaded to obtain a mixed sample.

[0062] The mixed sample was mixed with deionized water at a mass ratio of 10:1, stirred thoroughly and evenly, placed in a metal mold, and molded on a pressure molding machine at a pressure of 7 MPa to obtain coal briquettes.

[0063] The briquette is placed in a corundum crucible and a force of 800 N / m is applied to the surface. 2 The carbon material was prepared by heating the mixture in a muffle furnace at a heating rate of 1°C / min from room temperature to 750°C and maintaining the temperature for 2 hours. The muffle furnace was then cooled to room temperature to obtain a shaped carbon material.

[0064] The shaped carbon material was placed in a tubular furnace and heated from room temperature to 950°C at a heating rate of 10°C / min under an inert atmosphere. 0.042 mL / (min·g) of water vapor was introduced for activation for 2 h, and then a 50% ammonia mixed gas (nitrogen as the balance gas) was introduced for activation for 1 h. After cooling to room temperature, an alkaline carbon material catalyst was obtained, which was named CM-4.

[0065] Example 5.

[0066] Industrial solid waste magnesium slag and Malan fat coal with adhesiveness were used as raw materials, which were crushed and sieved to a particle size of less than 0.15 mm, respectively, and then mixed in a mass ratio of magnesium slag to Malan fat coal of 1:4 and fully kneaded to obtain a mixed sample.

[0067] The mixed sample was mixed with deionized water at a mass ratio of 10:1, stirred thoroughly and evenly, placed in a metal mold, and molded on a pressure molding machine at a pressure of 7 MPa to obtain coal briquettes.

[0068] The briquette is placed in a corundum crucible and a 1200N / m 2 The carbon material was prepared by heating the sample to 950°C at a heating rate of 1.5°C / min from room temperature and then cooling the muffle furnace to room temperature to obtain a shaped carbon material.

[0069] The shaped carbon material was placed in a tubular furnace and heated from room temperature to 900°C at a heating rate of 5°C / min under an inert atmosphere. 0.042 mL / (min·g) of water vapor was introduced for activation for 1.5 h, and then a 50% ammonia mixed gas (nitrogen as the balance gas) was introduced for activation for 1 h. After cooling to room temperature, an alkaline carbon material catalyst was obtained, which was named CM-5.

[0070] Figure 1The SEM images of the alkaline carbon material catalysts are shown, with CM-1 (a), CM-2 (b) and CM-3 (c) as representatives. Figure 1 It can be seen that the pore structures of various alkaline carbon material catalysts are rich and the pores are evenly distributed.

[0071] The alkaline carbon material catalyst is a material with interconnected or closed pores forming a network structure, which promotes the diffusion and mass transfer of macromolecular compounds in dusty tar gas, inhibits the polycondensation reaction between macromolecular compounds to a certain extent, and inhibits the formation of carbon deposition. In addition, its interconnected pore structure can increase the dust holding capacity of the particle bed and reduce the bed pressure drop, which helps to extend the service life of the particle bed.

[0072] Figure 2 The XRD patterns of CM-1, CM-2 and CM-3 are further given. The alkali metal calcium in the alkaline carbon material catalyst prepared from carbide slag mainly exists in the form of Ca(OH)2, CaO and CaS. The presence of metal active components can promote the cracking of heavy tar and the activation of small molecular gas compounds, thereby effectively improving the quality of tar.

[0073] Application example 1.

[0074] Long flame coal from Xinjiang with a particle size of 0.25 to 0.43 mm was selected as the research object, and a fixed bed reaction device was used as a particle bed dust collector. The effect of the alkaline carbon material catalyst prepared in the above Examples 1 to 5 as the filter material of the particle bed dust collector on the thermal conversion behavior of pyrolysis dust-containing tar gas and its catalytic quality improvement performance were investigated and verified.

[0075] Long flame coal and the alkaline carbon material catalyst prepared in Examples 1 to 5 are respectively filled into a two-stage quartz tube reactor in a mass ratio of 2:1, wherein the long flame coal is heated to 600°C in a nitrogen atmosphere for rapid pyrolysis, and the generated dusty pyrolysis tar gas is passed through an alkaline carbon material catalyst filter material heated to 500°C to perform in-situ catalytic upgrading of the tar gas.

[0076] The tar after catalytic upgrading was collected through a condensation system, the tar yield was calculated, and the chemical composition of the tar was analyzed using GC×GC-MS.

[0077] Since the residence time of dusty tar gas will affect the reaction behavior of volatiles in the particle bed dust collector, and the solid acid catalyst γ-Al2O3 also has a catalytic effect on the pyrolysis of dusty tar gas, control experiments of inert material quartz sand (QB) and solid acid catalyst γ-Al2O3 were carried out according to the above method.

[0078] according to Figure 3It can be seen from the tar yield that QB has no catalytic cracking effect on pyrolysis dusty tar gas due to its relative inertness, so the tar yield under the action of QB is the highest. After the pyrolysis dusty tar gas is catalytically upgraded by the granular bed filter material (CM-1 to CM-5), the tar yield is relatively high, which is higher than the tar yield under the action of γ-Al2O3. This is mainly because γ-Al2O3 has a strong cracking ability for tar due to its strong acid sites, resulting in the conversion of tar to carbon deposition and pyrolysis gas, and the tar yield is greatly reduced.

[0079] In contrast, CM-1 to CM-5, based on their interconnected pore structures and alkalinity, promote the mass transfer of macromolecular compounds, while promoting the dehydrogenation of hydrocarbon substances to produce hydrogen-rich small molecules, inhibiting the polycondensation of macromolecular substances, and significantly reducing the carbonization yield. Therefore, the alkaline carbon material catalyst guarantees the tar yield to a certain extent, inhibits the conversion of tar to carbonization and pyrolysis gas, and improves the economic efficiency of the pyrolysis process.

[0080] Furthermore, according to Figure 4 The relative content of chemical composition in the tar shows that compared with QB, under the action of γ-Al2O3 and alkaline carbon material catalysts, the relative content of oxygen-containing compounds and heterocyclic compounds containing N and S in the tar is reduced, and the relative content of monocyclic aromatic hydrocarbons is increased. The alkaline carbon material catalyst and γ-Al2O3 have effectively improved the quality of tar and changed the chemical composition of tar. When the chemical composition of the tars of the two are similar and the relative content is equivalent, the tar yield under the action of the alkaline carbon material catalyst is higher, which proves that the alkaline carbon material catalyst is more advantageous as a granular bed filter material.

[0081] Application example 2.

[0082] A corn cob biomass with a particle size of 0.25-0.43 mm was selected as the research object, and a fixed bed reaction apparatus was used to investigate and verify the effects of the alkaline carbon material catalysts prepared in Examples 1-5 above on the catalytic reforming reaction of tar during biomass gasification.

[0083] Corn cob biomass and the alkaline carbon material catalyst prepared in Examples 1 to 5 were respectively filled in a two-stage quartz tube reactor in a mass ratio of 2:1, and the corn cob biomass was heated to 950°C for gasification in an atmosphere of 50% water vapor (N2 as the balance gas). The generated biomass tar gas was passed through an alkaline carbon material catalyst heated to 750°C for in-situ catalytic reforming, and the tar was collected and the tar yield was calculated.

[0084] Since the residence time of dusty tar gas will affect the reaction behavior of volatiles in the particle bed dust collector, and the solid acid catalyst γ-Al2O3 also has a catalytic effect on the pyrolysis of dusty tar gas, control experiments of inert material quartz sand (QB) and solid acid catalyst γ-Al2O3 were carried out according to the above method.

[0085] Since the solid acid catalyst γ-Al2O3 also has a catalytic reforming effect on biomass tar gas, a control experiment using a commercial γ-Al2O3 catalyst was carried out according to the above method.

[0086] In addition, multiple in-situ catalytic reforming experiments were carried out on the same γ-Al2O3 and alkaline carbon material catalyst to measure its cycle life.

[0087] from Figure 5 It can be seen from the tar yield that the alkaline carbon material catalyst can promote the catalytic reforming reaction of tar and water vapor and improve the tar elimination efficiency, and its effect is equivalent to that of the γ-Al2O3 catalyst.

[0088] However, the results of the cycle life test showed that the γ-Al2O3 catalyst was deactivated due to carbon deposition after one use, while the alkaline carbon material catalyst could be recycled many times and had a longer life than γ-Al2O3.

[0089] It can be seen that the alkaline carbon material catalyst has better anti-coking performance than the solid acid catalyst and is more suitable as a catalyst for catalytic reforming of biomass gasification tar.

[0090] The above embodiments of the present invention do not describe all the details in detail, nor limit the present invention to the above embodiments. Various changes, modifications, substitutions and variations made by ordinary technicians in this field without departing from the principles and purpose of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing an alkaline carbon material catalyst comprises the following steps: mixing industrial solid waste containing alkaline metal oxides with caking coal having a high caking index, pyrolyzing the mixture, and activating the mixture with steam and ammonia to prepare the alkaline carbon material catalyst. 1) crushing industrial solid waste containing alkaline metal oxides and caking coal with a high caking index, selecting particles with a size of less than 0.15 mm by screening, and fully kneading them in a ratio of 1 to 20 wt % of the industrial solid waste to obtain a mixed material; 2) Wetting the mixed material with water and pressing it into shape to obtain briquettes; 3) Pressurizing and heating the briquette to 450-950°C in an air-tight condition to pyrolyze the briquette to prepare a shaped carbon material; 4) The shaped carbon material is heated to 850-950°C in an inert atmosphere, firstly steam is introduced to activate it, then ammonia is introduced to activate it, and after cooling, an alkaline carbon material catalyst is prepared; Among them, the industrial solid waste containing alkaline metal oxides is any one or more of carbide slag, red mud and magnesium slag, and the caking coal with a high caking index is fat coal and / or coking coal with a caking index of 95-110.

2. The method for preparing the basic carbon material catalyst according to claim 1, characterized in that Add 10-15wt% water to the mixed material.

3. The method for preparing the basic carbon material catalyst according to claim 1, characterized in that The moistened mixture is pressed into shape at a pressure of 3 to 9 MPa.

4. The method for preparing the basic carbon material catalyst according to claim 1, characterized in that Apply 700~1200N / m to the briquette 2 The pyrolysis is carried out at a pressure of 5. The method for preparing the basic carbon material catalyst according to claim 1, characterized in that The briquette is heated to 450-950°C at a heating rate of 0.5-2.5°C / min and pyrolyzed at a constant temperature of 1.5-2.5h.

6. The method for preparing an alkaline carbon material catalyst according to claim 1 is characterized in that the shaped carbon material is heated to 750-950°C at a heating rate of 5-10°C / min under an inert atmosphere, water vapor is introduced for activation for 1-2 hours, and then ammonia is introduced for activation for 1-2 hours.

7. The alkaline carbon material catalyst prepared by the preparation method according to claim 1.

8. The alkaline carbon material catalyst according to claim 7 is used as a filter material for a granular bed dust collector in filtering and removing dust and catalytically upgrading dusty tar gas from pyrolysis of low-grade pulverized coal.

9. Use of the alkaline carbon material catalyst according to claim 7 in catalytic reforming reaction of tar in the process of catalytic biomass and coal gasification.