A method for flotation separation of tungsten ore associated with sulfide ore
By using a combination of oxidizing agents and inhibitors in tungsten ore-associated sulfide ore, efficient separation of tungsten ore-associated sulfide ore is achieved, solving the problems of agent pollution and complex process, simplifying the process and improving the separation effect.
Patent Information
- Application Number
- CN202210873606.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-21
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-07-21
AI Technical Summary
In the recycling process of sulphide ore associated with tungsten ore, the prior art Chinese medicines are polluted, the process flow is complex, and the ore dressing indicators are poor. The depharmacy and inhibition processes are independent of each other, and there is a lack of unified methods for selective depharmacy and inhibition.
After grinding, oxidizer and foaming agent are added to flotation under different pH conditions, and the selective separation of polymetallic sulfide ore is achieved by combining inhibitors. The oxidizer is used to desorb the collector and combine it with high-efficiency inhibitors for surface inhibition, reducing the use of agents simplify the process flow.
It realizes efficient, stable and environmentally friendly separation of sulphide ore associated with tungsten ore, reduces the amount of agent used, simplifies the process flow, and improves the separation effect.
Smart Images

Figure BDA0003761538170000041
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ore dressing, in particular to a method for flotation separation of tungsten ore associated with sulfide ore. Background Art
[0002] Tungsten resources are my country's advantageous strategic mineral resource, and their reserves rank first in the world. However, there are few single tungsten metal deposits in my country, and a large number of valuable metals are often accompanied by tungsten ore. For example, the associated components in Tieshanlong Tungsten Ore in Jiangxi include Cu, Zn, Mo, Bi, Pb, Ag and other metals. The associated components of Dajishan Tungsten Ore in Jiangxi include Cu, Mo, Bi, S, Ag and other metals. The associated components in Xingluocangtten Ore in Ninghua, Fujian include Cu, Mo, Bi and other metals. Most of these associated metals exist in the form of sulfide minerals. The crude concentrate of sulfide ore formed by this type of associated resource after the main process of tungsten ore sand and tungsten fine mud is high in grade, rich in valuable components, and obvious comprehensive recycling value. In order to improve the recovery efficiency of sulphide ore associated with tungsten ore, ore dressers have conducted a lot of research. At present, most tungsten mines in my country mainly use flotation methods to recover associated sulfide ores. Common processes include "preferential flotation process", "partial mixed flotation process", "element-metallurgical joint process", etc.
[0003] Since the associated sulfide minerals adsorb the collector during the main process of reselecting and recycling of tungsten ore, the flotation performance is similar. No matter what process is used, the depharmaceutical pretreatment before the associated sulfide ore enters the sorting operation and the application of selective inhibitors during the sorting process are the key to achieving efficient separation of associated sulfide ore. The sodium sulfide depharmacy method is one of the most widely used methods in the flotation separation and pretreatment stage of tungsten ore associated sulfide minerals in industrial tungsten ore. During the de-drug process, controlling the degree of de-drug is the key. Incomplete de-drug will cause difficulties in inhibiting ganglite minerals in the subsequent process; complete de-drug requires sufficient or even excessive agents, and the de-drug time needs to be strictly controlled. Sulfide ore flotation inhibitors include two major categories: inorganic and organic. Inorganic agents have strong effects and are simple to prepare, but are harmful to the environment. Their applications in flotation of tungsten ore with sulfide ore are decreasing. The organic inhibitors are rich in types, wide sources, and environmentally friendly, but they are usually poor in water solubility and weak in inhibitory selectivity.
[0004] Whether it is the depharmaceutical pretreatment before sorting of tungsten ore-associated sulfide ore or the selection of inhibitors during sorting, a large number of scholars have conducted in-depth and systematic research on it, and many related achievements have also been applied to production practice. However, previous studies on the two processes of depharmacy and inhibition were mostly independent of each other, and the depharmacy of mixed crude concentrate and the selective inhibition of subsequent minerals in the production site were also carried out sequentially. Whether there is a method to unify the two processes of depharmacy and inhibition of a mineral, that is, to achieve selective inhibition of a mineral when selective depharmacy is performed on the mineral. Summary of the invention
[0005] The present invention provides a method for flotation separation of tungsten ore associated sulfide ore, which solves the problems of large reagent pollution, complex process flow, low mineral processing index, etc. in the comprehensive recovery process of tungsten ore associated polymetallic resources.
[0006] The method comprises the following steps:
[0007] (1) Grinding: Grind the polymetallic sulfide ore removed from the tungsten ore by flotation (the sulfide ore in the tungsten ore is the mixed ore first selected by flotation before the gravity separation of the tungsten ore, and the mixed ore is processed here). The fineness of the grinding operation is -0.074mm, accounting for 65%-70%;
[0008] (2) adding a pH adjuster to the pulp obtained by grinding in step (1) to adjust the pH of the pulp to 7-8, and sequentially adding an oxidant and a frother No. 2 oil to adjust the pulp, and then flotation is performed to obtain a molybdenum, copper, and sulfur mixed concentrate and a zinc concentrate;
[0009] (3) adding a pH adjuster to the molybdenum, copper and sulfur mixed concentrate obtained in step (2) to adjust the pH of the obtained pulp to 8-9, and sequentially adding an oxidant and a frother No. 2 oil to adjust the pulp, and then flotation is performed to obtain a molybdenum-sulfur mixed concentrate and a copper concentrate;
[0010] (4) adding an inhibitor and a frother No. 2 oil to the molybdenum-sulfur mixed concentrate obtained in step (3) for flotation to obtain a coarse concentrate 1 and a coarse tailing 1;
[0011] (5) The coarse concentrate 1 and the coarse tailings 1 obtained in step (4) are subjected to three concentrations and one scavenging, respectively, to obtain molybdenum concentrate and sulfur concentrate, and the concentrated middlings and scavenged middlings are returned in sequence.
[0012] In the above-mentioned step (1), the polymetallic sulfide ore separated from the tungsten ore by flotation contains molybdenum, copper, zinc and sulfur.
[0013] In step (2), the oxidant is one of hydrogen peroxide, potassium permanganate and sodium hypochlorite, and the amount of the oxidant is 1000-3000 g / t; the amount of No. 2 oil is 10-30 g / t.
[0014] In step (3), the oxidant is one of potassium permanganate and sodium hypochlorite, the amount of the oxidant is 500-1000 g / t, and the amount of No. 2 oil is 10-30 g / t.
[0015] In step (4), the inhibitor is 4-amino-6-hydroxy-2-mercaptopyrimidine, the amount of 4-amino-6-hydroxy-2-mercaptopyrimidine is 100-300 g / t, and the amount of No. 2 oil is 10-30 g / t.
[0016] In step (5), the inhibitor 4-amino-6-hydroxy-2-mercaptopyrimidine is added in the second concentration, and the inhibitor dosage is 50-150 g / t. No agent is added in the remaining two concentrations and scavenging.
[0017] The beneficial effects of the above technical solution of the present invention are as follows:
[0018] In the above scheme, an oxidant is used as an inhibitor. The oxidant can desorb the collectors adsorbed on the surface of sphalerite and chalcopyrite in sequence, but does not desorb the collectors adsorbed on the surface of pyrite and molybdenumite, thereby creating a selective inhibitory effect on sphalerite and chalcopyrite. Combined with the use of molybdenumite high-efficiency inhibitors, the flotation separation of tungsten ore-associated sulfide ore with the surface adsorbed on the surface is achieved. This method reduces the use of agents and shortens the process flow. It is a stable, efficient and environmentally friendly tungsten ore-associated sulfide ore ore ore ore dressing method. DETAILED DESCRIPTION
[0019] In order to make the technical problems to be solved, technical solutions and advantages of the present invention more clear, they are described in detail below in conjunction with specific embodiments.
[0020] The present invention aims at solving the existing problems and provides a method for flotation separation of tungsten ore associated with sulfide ore.
[0021] (1) Grinding: Grind the polymetallic sulfide ore removed from the tungsten ore by flotation, with the grinding fineness of -0.074mm accounting for 65%-70%;
[0022] (2) adding a pH adjuster to the pulp obtained by grinding in step (1) to adjust the pH of the pulp to 7-8, and sequentially adding an oxidant and a frother No. 2 oil to adjust the pulp, and then flotation is performed to obtain a molybdenum, copper, and sulfur mixed concentrate and a zinc concentrate;
[0023] (3) adding a pH adjuster to the molybdenum, copper and sulfur mixed concentrate obtained in step (2) to adjust the pH of the obtained pulp to 8-9, and sequentially adding an oxidant and a frother No. 2 oil to adjust the pulp, and then flotation is performed to obtain a molybdenum-sulfur mixed concentrate and a copper concentrate;
[0024] (4) adding an inhibitor and a frother No. 2 oil to the molybdenum-sulfur mixed concentrate obtained in step (3) for flotation to obtain a coarse concentrate 1 and a coarse tailing 1;
[0025] (5) The coarse concentrate 1 and the coarse tailings 1 obtained in step (4) are subjected to three concentrations and one scavenging, respectively, to obtain molybdenum concentrate and sulfur concentrate, and the concentrated middlings and scavenged middlings are returned in sequence.
[0026] This will be described below with reference to specific embodiments.
[0027] Example 1
[0028] The polymetallic sulfide ore flotation removed from a certain tungsten ore is finely ground to -0.074mm 65%. Add pH adjuster to the slurry obtained from the grinding to adjust the pH of the obtained slurry to 7. Add 3000g / t potassium permanganate and 30g / t No. 2 oil slurry to slurry to flotation, and then flotation is obtained to obtain molybdenum copper-sulfur mixed concentrate and zinc concentrate; add pH adjuster to the molybdenum copper-sulfur mixed concentrate to adjust the pH of the obtained slurry to 9, add 1000g / t potassium permanganate and 10g / t No. 2 oil slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to slurry to Flotation to obtain molybdenum-sulfur mixed concentrate and copper concentrate; 300g / t of 4-amino-6-hydroxy-2-mercaptopyrimidine and 20g / t of No. 2 oil were flotation to obtain coarse concentrate 1 and coarse tailings 1; 3 times of selection and one sweep of crude concentrate 1 and coarse tailings 1 were performed respectively to obtain molybdenum concentrate. The selected ore and the sweep and selected ore were returned in sequence. The 4-amino-6-hydroxy-2-mercaptopyrimidine of Selection 2 was 150g / t, Selection 1, Selection 3, Sweep and no medicine was added.
[0029] The results of the mineral processing tests are shown in the following table.
[0030] Flotation test index (wt.%)
[0031]
[0032] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for flotation separation of tungsten ore associated with sulfide ore, characterized in that: The steps include: (1) Grinding: Grind the polymetallic sulfide ore removed from the tungsten ore by flotation, with the grinding fineness of -0.074mm accounting for 65%-70%; (2) adding a pH adjuster to the pulp obtained by grinding in step (1) to adjust the pH of the pulp to 7-8, and sequentially adding an oxidant and a frother No. 2 oil to adjust the pulp, and then flotation is performed to obtain a molybdenum, copper, and sulfur mixed concentrate and a zinc concentrate; (3) adding a pH adjuster to the molybdenum, copper and sulfur mixed concentrate obtained in step (2) to adjust the pH of the obtained pulp to 8-9, and sequentially adding an oxidant and a frother No. 2 oil to adjust the pulp, and then flotation is performed to obtain a molybdenum-sulfur mixed concentrate and a copper concentrate; (4) adding an inhibitor and a frother No. 2 oil to the molybdenum-sulfur mixed concentrate obtained in step (3) for flotation to obtain a coarse concentrate 1 and a coarse tailing 1; (5) The coarse concentrate 1 and the coarse tailings 1 obtained in step (4) are subjected to three concentrations and one scavenging, respectively, to obtain molybdenum concentrate and sulfur concentrate, and the concentrated middlings and scavenged middlings are returned in sequence.
2. The method for flotation separation of tungsten ore associated with sulfide ore according to claim 1, characterized in that: The polymetallic sulfide ore separated from the tungsten ore by flotation in step (1) contains molybdenum, copper, zinc and sulfur.
3. The method for flotation separation of tungsten ore associated with sulfide ore according to claim 1, characterized in that: In the step (2), the oxidant is one of hydrogen peroxide, potassium permanganate and sodium hypochlorite, and the amount of the oxidant is 1000-3000 g / t; the amount of No. 2 oil is 10-30 g / t.
4. The method for flotation separation of tungsten ore associated with sulfide ore according to claim 1, characterized in that: In the step (3), the oxidant is one of potassium permanganate and sodium hypochlorite, the amount of the oxidant is 500-1000 g / t, and the amount of No. 2 oil is 10-30 g / t.
5. The method for flotation separation of tungsten ore associated with sulfide ore according to claim 1, characterized in that: In the step (4), the inhibitor is 4-amino-6-hydroxy-2-mercaptopyrimidine, the amount of 4-amino-6-hydroxy-2-mercaptopyrimidine is 100-300 g / t, and the amount of No. 2 oil is 10-30 g / t.
6. The method for flotation separation of tungsten ore associated with sulfide ore according to claim 1, characterized in that: In the step (5), the inhibitor 4-amino-6-hydroxy-2-mercaptopyrimidine is added in the second concentration, and the amount of the inhibitor is 50-150 g / t. No agent is added in the remaining two concentrations and scavenging.
Citation Information
Patent Citations
Mineral processing method for recycling scheelite / molybdenum oxide ores from molybdenum sulfide flotation tailings
CN102489407A
Beneficiation method for flotation and recovery of molybdenum from easy-floating gangue refractory molybdenum ore
CN102671769A
Method for recovering valuable metal from sulfide ore-contained tungsten rough concentrate
CN105498948A
Gravity separation and flotation separation combined process for treatment of complex tungsten-molybdenum-copper-lead-zinc polymetallic ores
CN107362899A
Comprehensive recovery and beneficiation process for wolframite and scheelite and associated valuable metals of wolframite and scheelite
CN112892853A