A polystyrene material with high gloss and high toughness and its preparation method and application

By adding specific toughening agents and polyethylene resins to HIPS materials and performing extrusion and granulation treatment, the problems of low gloss and poor toughness of the material are solved, and a high gloss, high toughness and high strength polystyrene material is achieved , expanding its applications in the fields of home appliances, electronics and automotive.

CN115368699BActive Publication Date: 2024-11-26KINGFA SCI & TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211207344.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-30
Publication Date
2024-11-26
Estimated Expiration
2042-09-30

AI Technical Summary

Technical Problem

The existing high-impact polystyrene (HIPS) materials have low gloss and poor toughness, making them difficult to meet the strength requirements of parts, limiting their applications in home appliances, electronics and automotive fields.

Method used

Simultaneously add styrene-butadiene-styrene block copolymer (toughening agent a), random styrene-butadiene copolymer (toughening agent b), and polyethylene resin and mix at high speed Extrusion granulation is carried out in the material equipment to improve the fluidity and compatibility of the material, thereby improving gloss and toughness.

Benefits of technology

The high glossiness of the material (more than 86%), the impact strength of the cantilever beam notched (more than 15kJ/m2) and the bending modulus (more than 2000MPa) are achieved, and the high strength and aesthetic requirements of the parts are met.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003874558380000041
    Figure BDA0003874558380000041
  • Figure BDA0003874558380000051
    Figure BDA0003874558380000051
  • Figure BDA0003874558380000061
    Figure BDA0003874558380000061
Patent Text Reader

Abstract

The present invention discloses a polystyrene material with high gloss and high toughness, and its preparation method and application, and relates to the field of polymer materials. The polystyrene material includes polystyrene resin, toughener a, toughener b, polyethylene resin, and lubricant; the melt flow index of the polystyrene resin is tested at 200°C and 5kg conditions to be ≥5g / 10min; toughener a is styrene-ethylene-butadiene-styrene block copolymer, and its number average molecular weight is 9-300,000 g / mol; toughener b is random styrene-butadiene copolymer, and its melt flow index is tested at 200°C and 5kg conditions to be 8-20g / 10min. The present application improves the fluidity of the matrix as a whole by adding toughener a, toughener b and polyethylene resin simultaneously, so that the material has the ability to more easily replicate high-gloss molds, the glossiness is improved, and the rigidity and toughness of the material meet the requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer materials, and in particular to a polystyrene material with high gloss and high toughness, and a preparation method and application thereof. Background Art

[0002] High-impact polystyrene (HIPS) consists of a rubber phase and a continuous polystyrene phase. By grafting a small amount of polybutadiene onto the polystyrene matrix, an "island structure" is formed, which gives it good impact strength, rigidity, processing performance and colorability. It can be used as a cost-effective solution to replace ABS in the fields of home appliances, electronic appliances, OA and automobiles. However, in the current technology, the addition of rubber makes the gloss of HIPS very poor, which seriously affects the appearance and texture when used in the shell.

[0003] The prior art balances high gloss and high toughness by controlling the weight ratio of polybutadiene rubber phase 1 (particle size 0.5-1.0 μm) to polybutadiene rubber phase 2 (particle size 1.5-5.0 μm) between 1:5-1:15. Alternatively, capsule particles (particle size 0.8 μm-1.0 μm) are compounded with microporous particles (particle size 1.2 μm-4.4 μm) to prepare high gloss and high impact polystyrene materials. The gloss of the material is improved, but the impact strength is still lower than that of ABS, and it is difficult to meet the strength requirements of the parts.

[0004] Therefore, it is urgent to develop technologies that can simultaneously solve the defects of HIPS materials such as low gloss and poor toughness in order to expand the application areas of HIPS. Summary of the invention

[0005] The present invention provides a polystyrene material with high gloss and high toughness, and a preparation method and application thereof, so as to prepare a polystyrene material with high gloss, high rigidity and high toughness, which can completely replace ABS in terms of performance and be applied to the fields of home appliances, electronic appliances, OA and automobiles, thereby expanding the application of HIPS.

[0006] In order to solve the above technical problems, one of the purposes of the present invention is to provide a polystyrene material with high gloss and high toughness, comprising the following components in parts by weight:

[0007] Polystyrene resin: 100 parts;

[0008] Toughener a: 15-30 parts;

[0009] Toughener b: 5-20 parts;

[0010] Polyethylene resin: 1-15 parts;

[0011] Lubricant: 0.2-5 parts;

[0012] The melt flow index of the polystyrene resin is ≥5g / 10min when tested at 200°C and 5kg; the toughening agent a is a styrene-ethylene-butadiene-styrene block copolymer, and its number average molecular weight is 90,000-300,000 g / mol; the toughening agent b is a random styrene-butadiene copolymer, and its melt flow index is 8-20g / 10min when tested at 200°C and 5kg.

[0013] By adopting the above scheme, the present application simultaneously adds toughening agent a, toughening agent b and polyethylene resin, thereby improving the overall fluidity of the matrix, making the material more easily capable of replicating high-gloss molds and improving the smoothness of the surface of the workpiece. At the same time, the polyethylene resin easily flows to the surface of the material to cover the rubber molecules, thereby improving the overall gloss of the material; in addition, toughening agent a uses toughening agent b to improve its compatibility with polystyrene resin, giving the material higher overall rigidity and toughness.

[0014] As a preferred embodiment, the melt flow index of the polyethylene resin is 10-30 g / 10 min when measured at 190° C. and 2.16 kg.

[0015] As a preferred solution, the melt flow index of the polystyrene resin is 10-15 g / 10 min when tested under the conditions of 200° C. and 5 kg.

[0016] As a preferred embodiment, the butadiene content of the random styrene-butadiene copolymer is less than 40%.

[0017] As a preferred embodiment, the butadiene content of the random styrene-butadiene copolymer is 10%-30%.

[0018] As a preferred embodiment, the weight proportion of the polyethylene resin is 5 to 10 parts.

[0019] As a preferred embodiment, the mass ratio of the toughening agent a to the toughening agent b is (4-5):1.

[0020] By adopting the above scheme, the addition ratio of toughener a and toughener b is limited, which greatly improves the rigidity and toughness of the material while ensuring that the gloss and fluidity of the material are not affected.

[0021] As a preferred embodiment, the lubricant includes one or more of stearic acid amide, stearic acid metal salt and ethylene wax lubricants.

[0022] As a preferred embodiment, the lubricant is a stearic acid amide lubricant.

[0023] As a preferred embodiment, the lubricant is ethylene bisstearamide.

[0024] As a preferred embodiment, the polyethylene resin is a low-density linear polyethylene resin and / or a high-density polyethylene resin.

[0025] As a preferred embodiment, the number average molecular weight of the styrene-ethylene-butadiene-styrene block copolymer is 100,000-200,000 g / mol.

[0026] In order to solve the above technical problems, the second purpose of the present invention provides a method for preparing a polystyrene material with high gloss and high toughness, comprising the following steps: putting polystyrene resin, toughening agent a, toughening agent b, polyethylene resin and lubricant into a high-speed mixing device and mixing them evenly, and then extruding and granulating them through an extrusion device to obtain a polystyrene material with high gloss and high toughness.

[0027] As a preferred embodiment, in the extrusion equipment, the screw speed is 300-500rpm, and the screw temperatures of each section of the extrusion equipment from the feeding port to the die are set to zone 1 temperature 80-100°C, zone 2 temperature 160-180°C, zone 3 temperature 190-210°C, zone 4 temperature 190-210°C, zone 5 temperature 190-210°C, zone 6 temperature 180-200°C, zone 7 temperature 180-200°C, zone 8 temperature 190-210°C, zone 9 temperature 190-210°C, and die head temperature 200-220°C.

[0028] In order to solve the above technical problems, the third object of the present invention provides a polystyrene material with high gloss and high toughness for use in the fields of home appliances, electronic appliances, OA or automobiles, especially in the application of product shells.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] The present application simultaneously adds toughening agent a, toughening agent b and polyethylene resin, thereby improving the fluidity of the matrix as a whole, making the material more capable of replicating high-gloss molds, thereby improving the flatness and smoothness of the surface of the product. At the same time, the polyethylene resin is easy to flow to the surface of the material to cover the rubber molecules, thereby further improving the glossiness. In addition, toughening agent a uses toughening agent b to improve its compatibility with polystyrene resin, giving the material higher rigidity and toughness as a whole, and finally making the glossiness of the product reach more than 86%, and the cantilever beam notched impact strength reaches 15kJ / m 2 The flexural modulus is above 2000 MPa. DETAILED DESCRIPTION

[0031] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] The following Table 1 shows the sources of raw materials in the examples and comparative examples of the present application. Unless otherwise specified, the lubricants were commercially available, and the same lubricants were used in parallel experiments.

[0033] Table 1 - Sources and properties of raw materials in Examples and Comparative Examples

[0034]

[0035]

[0036] Examples 1-10 and Comparative Examples 1-10

[0037] A polystyrene material with high gloss and high toughness, wherein the contents of the components are shown in Table 2, including a polystyrene resin, a toughening agent a1, a toughening agent b, a polyethylene resin and a lubricant; the polyethylene resin is a low-density linear polyethylene resin or a high-density linear polyethylene resin; the toughening agent a1 is a styrene-ethylene-butadiene-styrene block copolymer (SEBS); the toughening agent b is a random styrene-butadiene copolymer; and the lubricant is ethylene bisstearamide.

[0038] The preparation method of the polystyrene material with high gloss and high toughness comprises the following steps: weighing each component according to the ratio, putting the polystyrene resin, toughening agent a, toughening agent b, polyethylene resin and lubricant into a high-speed mixer and mixing them evenly, and then extruding and granulating them through an extruder, the screw speed is 400 rpm, and the screw temperatures of each section of the extruder from the feed port to the die are set to 90°C for zone one, 170°C for zone two, 200°C for zone three, 200°C for zone four, 200°C for zone five, 190°C for zone six, 190°C for zone seven, 200°C for zone eight, 200°C for zone nine, and 210°C for die head, so as to obtain a polystyrene material with high gloss and high toughness.

[0039] Table 2 - Content of each component in the polystyrene material of Examples 1-10 and Comparative Examples 1-10

[0040]

[0041]

[0042] Performance testing

[0043] 1. Surface gloss: The materials of Examples 1-10 and Comparative Examples 1-10 were injection molded into square plates using a high-gloss mold, and then the gloss was tested at an angle of 60° using a surface gloss instrument according to "GB / T 8807-1988 Plastic Mirror Gloss Test Method". The test results are shown in Table 3. The surface gloss of the present application is above 86%, which meets the requirements.

[0044] 2. Izod notch impact strength: According to GB / T 1843-1996 "Plastic Izod Impact Test Method" standard, the materials of Examples 1-10 and Comparative Examples 1-10 were tested, with a pendulum energy of 2.75 J, A-type notch, and room temperature test. The test results are shown in Table 3. The Izod notch impact strength of the present application is 15 kJ / m 2 The above requirements are met.

[0045] 3. Flexural modulus: The materials of Examples 1-10 and Comparative Examples 1-10 were tested according to GB / T 9341-2008 "Determination of Flexural Properties of Plastics" at a test speed of 2 mm / min. The test results are shown in Table 3. The flexural modulus of the present application is above 2000 MPa, which meets the requirements.

[0046] Table 3 - Performance test results of Examples 1-10 and Comparative Examples 1-10

[0047]

[0048]

[0049] Combining the performance test results of Example 1 and Comparative Example 1 in Table 3, it can be seen that the melt flow index of the polystyrene resin is low, which will cause the fluidity of the matrix to be too low, thereby affecting the mold replication ability and ultimately causing the gloss of the product to be reduced. The present application adopts a melt flow index of more than 5g / 10min, which can increase the flow rate of the matrix and ensure that the gloss of the product is not affected.

[0050] Combining the performance test results of Example 1 and Comparative Examples 2-3, 6-7 in Table 3, it can be seen that compared with SBS, the toughening agent a uses SEBS and when its number average molecular weight is 90,000-300,000 g / mol, it can be distributed in the GPPS resin with a larger rubber particle size, which helps to improve the notched impact strength of the product and improve the toughness. At the same time, because the SEBS rubber contains vinyl groups, it is difficult to plasticize itself. When the molecular weight is large, it is basically distributed in the GPPS matrix resin in a large particle size. The toughening agent a is dispersed in the GPPS resin with a larger rubber size. When the amount added is too much, the surface gloss will be significantly reduced, the surface roughness will be greater, and the gloss reduction will be more obvious.

[0051] Combining the performance test results of Examples 1 and 9 and Comparative Examples 4-5 and 8 in Table 3, it can be seen that the addition of toughener b not only has a toughening effect on the substrate itself, but also helps to improve the compatibility of toughener a and polystyrene resin, helps to improve the combination of toughener a and polystyrene resin, thereby improving the toughening efficiency of toughener a, greatly improving the toughness of the system, and at the same time, it itself has a high melt flow rate, which helps to improve the overall fluidity of the matrix, making the material easier to replicate high-gloss molds, thereby making the surface of the product material smooth and smooth, and the glossiness is improved, and the toughener b has little effect on the glossiness of the material.

[0052] Combining the performance test results of Examples 1 and 10 and Comparative Examples 9-10 in Table 3, it can be seen that by adding polyethylene resin with a high melt flow index, the polyethylene resin molecules are more likely to migrate to the surface of the material to cover the surface rubber, thereby improving the gloss. If the content is too little, it cannot achieve the effect of complete coverage, and if the content is too much, the rigidity and toughness of the material will decrease.

[0053] Combining the performance test results of Examples 1 and 4-8 in Table 3, it can be seen that the addition of polyethylene resin can improve the gloss of the material. By limiting the addition ratio of toughening agent a and toughening agent b to (4-5): 1, the rigidity and toughness of the material can be greatly improved while ensuring that the gloss of the material is not affected, and the overall performance is better.

[0054] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present invention. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. It is particularly pointed out that for those skilled in the art, any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention should be included in the scope of protection of the present invention.

Claims

1. A polystyrene material with high gloss and high toughness, characterized in that: It includes the following components by weight: Polystyrene resin: 100 parts; Toughener a: 15-30 parts; Toughener b: 5-20 parts; Polyethylene resin: 1-15 parts; Lubricant: 0.2-5 parts; The melt flow index of the polystyrene resin is ≥5g / 10min when tested at 200°C and 5kg; the toughening agent a is a styrene-ethylene-butadiene-styrene block copolymer, and its number average molecular weight is 90,000-300,000 g / mol; the toughening agent b is a random styrene-butadiene copolymer, and its melt flow index is 8-20g / 10min when tested at 200°C and 5kg.

2. A polystyrene material with high gloss and high toughness as claimed in claim 1, characterized in that: The melt flow index of the polyethylene resin is measured at 190° C. and 2.16 kg and is in the range of 10-30 g / 10 min.

3. A polystyrene material with high gloss and high toughness as claimed in claim 1, characterized in that: The butadiene mass content of the random styrene-butadiene copolymer is less than 40%.

4. A polystyrene material with high gloss and high toughness as claimed in claim 1, characterized in that: The weight portion of the polyethylene resin is 5 parts to 10 parts.

5. A polystyrene material with high gloss and high toughness as claimed in claim 4, characterized in that: The mass ratio of the toughening agent a to the toughening agent b is (4-5):

1.

6. A polystyrene material with high gloss and high toughness as claimed in claim 1, characterized in that: The lubricant includes one or more of stearic acid amide, stearic acid metal salt and ethylene wax lubricants.

7. The polystyrene material with high gloss and high toughness as claimed in claim 1, characterized in that: The polyethylene resin is a low-density linear polyethylene resin and / or a high-density polyethylene resin.

8. A method for preparing a polystyrene material with high gloss and high toughness as claimed in any one of claims 1 to 7, characterized in that: The following steps are involved: The polystyrene resin, toughening agent a, toughening agent b, polyethylene resin and lubricant are put into a high-speed mixing device and mixed evenly, and then extruded and granulated through an extrusion device to obtain a polystyrene material with high gloss and high toughness.

9. The method for preparing a polystyrene material with high gloss and high toughness as claimed in claim 8, characterized in that: In the extrusion equipment, the screw speed is 300-500rpm, and the screw temperatures of each section of the extrusion equipment from the feeding port to the die are set to zone 1 temperature 80-100°C, zone 2 temperature 160-180°C, zone 3 temperature 190-210°C, zone 4 temperature 190-210°C, zone 5 temperature 190-210°C, zone 6 temperature 180-200°C, zone 7 temperature 180-200°C, zone 8 temperature 190-210°C, zone 9 temperature 190-210°C, and die head temperature 200-220°C.

10. Use of the high-gloss and high-toughness polystyrene material according to any one of claims 1 to 7 in the fields of household appliances, electronic appliances, OA or automobiles.