Repair method of lithium iron phosphate positive electrode material, positive electrode material and application

By using multi-functional solvents of ethanol, lithium acetate and polyvinylpyrrolidone to perform solvothermal treatment and calcination of lithium iron phosphate cathode materials, the problem of short cycle life of lithium iron phosphate cathode materials is solved, and efficient material repair and cycle life extension are achieved. Suitable for large-scale recycling.

CN115417396BActive Publication Date: 2024-10-29TSINGHUA SHENZHEN INTERNATIONAL GRADUATE SCHOOL

Patent Information

Application Number
CN202211261376.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-14
Publication Date
2024-10-29
Estimated Expiration
2042-10-14

AI Technical Summary

Technical Problem

The existing recycling technology of lithium iron phosphate cathode materials has problems such as short cycle life, high energy consumption, poor environmental protection and unclear economic benefits, especially in the repair process of discarded lithium iron phosphate cathode materials.

Method used

The lithium iron phosphate cathode material is solvothermal treated using a multifunctional solvent mixed with ethanol, lithium acetate and polyvinylpyrrolidone. After vacuum drying and calcination, the repaired material is doped and carbon-coated in an argon and hydrogen environment. Extend its cycle life.

Benefits of technology

It effectively repairs the cycle life of the lithium iron phosphate cathode material, with a capacity retention rate of 76.6%, excellent performance, and the solvent used is cheap, environmentally friendly, and suitable for large-scale recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115417396B_ABST
    Figure CN115417396B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for repairing a lithium iron phosphate positive electrode material, comprising the following steps: S1, mixing the lithium iron phosphate positive electrode material with a multifunctional solvent, and performing a solvent thermal treatment; the multifunctional solvent is prepared by mixing ethanol, lithium acetate and polyvinyl pyrrolidone; S2, vacuum drying the precipitate obtained after the solvent thermal treatment; S3, calcining the solid powder obtained by vacuum drying to obtain the repaired lithium iron phosphate positive electrode material. The present invention uses a multifunctional solvent composed of ethanol, polyvinyl pyrrolidone and lithium acetate to firstly activate the surface of the lithium iron phosphate positive electrode material. The surface of the lithium iron phosphate positive electrode material after the activation treatment can effectively combine with lithium ions during the solvent thermal treatment process, and the anti-site defects in the lithium iron phosphate are repaired by using the reducing property of ethanol. In the subsequent calcination process, it is not necessary to add lithium salt to supplement lithium ions, which is conducive to effectively repairing the lithium iron phosphate positive electrode material during calcination.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of recycling lithium iron phosphate positive electrode materials, and in particular to a repair method, positive electrode material and application of lithium iron phosphate positive electrode materials. Background Art

[0002] Since the excellent energy storage technology of lithium-ion batteries has been used in all aspects of life, especially with the popularization of new energy vehicles, the use of lithium-ion batteries has shown a sharp increase. Compared with other types of lithium-ion batteries, lithium iron phosphate positive electrode material lithium-ion batteries have been widely used because of their excellent cycle stability and low price. It is estimated that by 2025, the global shipment of lithium iron phosphate positive electrode material batteries will reach 480.1GWh. Since the life of lithium iron phosphate positive electrode material lithium-ion batteries is about 5-8 years, this means that a large number of discarded lithium-ion batteries will be generated in the future. Discarded lithium iron phosphate positive electrode material batteries will cause great pollution to water resources, soil, etc., and more importantly, the discarded lithium iron phosphate positive electrode material battery positive electrode material contains lithium resources. Therefore, the recycling of lithium-ion batteries has become particularly important.

[0003] The traditional recycling technologies for positive electrode materials of lithium-ion batteries include wet recycling technology and pyrometallurgical recycling technology. The wet recycling technology destroys the structure of the positive electrode material through acid or alkaline solution, precipitates the precious metal ions in the positive electrode material, and separates and recycles them. This method has a complicated recycling process and will cause secondary pollution to the environment during the recycling process. For pyrometallurgical recycling, the metal elements in the positive electrode material are reduced at high temperature to achieve alloying, and finally the various elements are separated and calcined to become lithium-ion batteries. The temperature required for the high-temperature reduction of transition metal ions is generally 1000°C or above. The recycling of lithium elements by pyrometallurgical recycling is very limited. Overall, the disadvantages of pyrometallurgical recycling are high energy consumption, environmental protection, cumbersome recycling process steps, and obvious disadvantages for the recycling of expensive lithium elements. Since the discarded lithium iron phosphate positive electrode material battery does not contain precious metals such as cobalt and nickel, the economic benefits of recycling lithium iron phosphate positive electrode materials by the above method are not obvious.

[0004] Recently, people have discovered that discarded lithium-ion batteries can be effectively recycled through direct repair, thus avoiding the shortcomings of wet and pyrometallurgical recycling. Although lithium iron phosphate cathode materials can be repaired through direct repair, the cycle life of the repaired lithium iron phosphate cathode materials is too short. Most of the repaired lithium iron phosphate cathode materials can only be cycled 100-300 times, so it is difficult to actually apply them to actual production and life. Therefore, the urgent problem for the repaired lithium iron phosphate cathode material battery is how to achieve a longer cycle life for the repaired lithium iron phosphate cathode material. Another problem is that the reducing agent used in direct recycling is toxic or expensive. The above factors have caused certain obstacles to the large-scale recycling of discarded lithium iron phosphate cathode materials. Summary of the invention

[0005] The purpose of the present invention is to solve the technical problem that the cycle life of the repaired lithium iron phosphate positive electrode material is short, and to provide a repair method, positive electrode material and application of the lithium iron phosphate positive electrode material.

[0006] The technical problem of the present invention is solved by the following technical solutions:

[0007] A method for repairing a lithium iron phosphate positive electrode material comprises the following steps:

[0008] S1. Mixing a lithium iron phosphate positive electrode material with a multifunctional solvent and performing a solvent thermal treatment; the multifunctional solvent is prepared by mixing ethanol, lithium acetate and polyvinyl pyrrolidone;

[0009] S2, vacuum drying the precipitate obtained after the solvent thermal treatment;

[0010] S3. calcining the solid powder obtained by vacuum drying to obtain a repaired lithium iron phosphate positive electrode material.

[0011] In some embodiments, the following technical features are also included:

[0012] In step S1, the amount of ethanol is 10-20% of the mass of the lithium iron phosphate positive electrode material, the amount of lithium acetate is 10-20% of the mass of the lithium iron phosphate positive electrode material, and the amount of polyvinyl pyrrolidone is 0.5%-1% of the mass of the lithium iron phosphate positive electrode material.

[0013] In step S1, mixing the lithium iron phosphate positive electrode material with the multifunctional solvent comprises: dissolving polyvinyl pyrrolidone and the lithium iron phosphate positive electrode material in ethanol, stirring for 5h-12h, then pouring lithium acetate and stirring for 2h-5h.

[0014] In step S1, the solvent thermal treatment process is assisted by any one of ultrasound, hydrothermal, and heating and pressurization.

[0015] In step S1, the temperature of the solvent thermal treatment is 150-180° C., and the time of the solvent thermal treatment is 5-12 hours.

[0016] In step S2, the vacuum drying temperature is 60-120°C, and the drying time is 12-24 hours.

[0017] Step S3 includes: calcining the solid powder obtained by vacuum drying at 600-750° C. in an argon-hydrogen environment for 2 h to 10 h to obtain a repaired, doped, carbon-coated lithium iron phosphate positive electrode material.

[0018] The present invention also adopts the following technical solution:

[0019] A lithium iron phosphate positive electrode material is prepared by the above-mentioned lithium iron phosphate positive electrode material repair method.

[0020] A positive electrode sheet comprises a current collector and a positive electrode material layer arranged on the surface of the current collector, wherein the material of the positive electrode material layer comprises the above-mentioned lithium iron phosphate positive electrode material.

[0021] A battery comprises the above-mentioned positive electrode sheet.

[0022] The beneficial effects of the present invention compared with the prior art include:

[0023] The repair method of the lithium iron phosphate positive electrode material proposed by the present invention first uses a multifunctional solvent mixed with ethanol, lithium acetate and polyvinyl pyrrolidone to activate the surface of the lithium iron phosphate positive electrode material. The surface of the lithium iron phosphate positive electrode material after the activation treatment can effectively combine with lithium ions during the solvent heat treatment process, and the anti-site defects in the lithium iron phosphate are repaired by using the reducing property of ethanol, and no lithium salt needs to be added to supplement lithium ions during the subsequent calcination process, which is conducive to more effective repair of the lithium iron phosphate positive electrode material during calcination. Moreover, due to the coating of the waste lithium iron phosphate by polyvinyl pyrrolidone in the multifunctional solvent, the surface of the lithium iron phosphate positive electrode material can be nitrogen doped and carbon coated during the heat treatment and calcination process, and the element doping and carbon coating can achieve a long life cycle of the repaired lithium iron phosphate positive electrode material. At the same time, the multifunctional solvent used in the present invention is low-priced, environmentally friendly, and has simple steps, which is suitable for large-scale repair of lithium iron phosphate positive electrode materials. The multifunctional solvent of the present invention can utilize the reducing property of ethanol to effectively repair the lithium iron anti-site defects in the lithium iron phosphate positive electrode material during the treatment of lithium iron phosphate. Specifically, the reducing agent ethanol can reduce the Fe at the Li position in the waste lithium iron phosphate. 3+ Reduction to Fe 2+And reduce the diffusion barrier of Fe migrating to the original Fe position and return it to the original Fe position, thereby effectively reducing the diffusion barrier of lithium ions entering the lithium iron phosphate positive electrode material during the repair process.

[0024] Other beneficial effects of the embodiments of the present invention will be further described below. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is a performance diagram of repairing lithium iron phosphide under different repair conditions in an embodiment of the present invention;

[0026] Figure 2 is a comparison diagram of X-ray diffraction of lithium iron phosphate positive electrode material and lithium iron phosphate after repair under optimal conditions in an embodiment of the present invention;

[0027] Figure 3 This is an X-ray photoelectron spectrum analysis diagram of the lithium iron phosphate positive electrode material after repair under optimal conditions in an embodiment of the present invention;

[0028] Figure 4 It is a comparison chart of the discharge specific capacity and coulomb efficiency of the lithium iron phosphate positive electrode material after the optimal condition repair in the embodiment of the present invention, the lithium iron phosphate positive electrode material before the repair and the button battery made of commercial lithium iron phosphate;

[0029] Figure 5 It is a comparison chart of the discharge specific capacity and coulomb efficiency of the soft-pack battery made of the lithium iron phosphate positive electrode material after the optimal condition repair in the embodiment of the present invention and the lithium iron phosphate positive electrode material before the repair in the electrochemical test;

[0030] Figure 6a is a graph showing changes in polarization voltage of waste lithium iron phosphate cathode material during cycling in an embodiment of the present invention;

[0031] Figure 6b is a graph showing changes in polarization voltage of the repaired lithium iron phosphate cathode material during cycling in an embodiment of the present invention;

[0032] Figure 7 This is the refined XRD spectrum of the lithium iron phosphate cathode material before repair;

[0033] Figure 8 This is the refined XRD spectrum of the repaired lithium iron phosphate cathode material;

[0034] Fig. 9 This is a flow chart of a method for repairing a lithium iron phosphate positive electrode material according to an embodiment of the present invention. DETAILED DESCRIPTION

[0035] Before introducing the specific implementation mode of the present invention, the idea of ​​the present invention is first introduced as follows:

[0036] The present invention provides a multifunctional solvent for directly repairing, doping and carbonizing lithium iron phosphate positive electrode materials. The components of the solvent include a reducing solvent ethanol medium, lithium acetate and a doped modified polyvinyl pyrrolidone additive, which together constitute the multifunctional solvent. The method of the present invention directly repairs, dopes and carbonizes lithium iron phosphate by using the multifunctional solvent. The process is as follows: the waste lithium iron phosphate positive electrode material is treated with the multifunctional solvent, the product after the solvent heat treatment is vacuum dried, and finally calcined under an atmosphere of argon and hydrogen, so that the capacity of the repaired lithium iron phosphate positive electrode material is restored from 100 mAh / g before the repair to 140 mAh / g, and the capacity retention rate after 1000 cycles is 76.6%. The repaired positive electrode material has a uniform and complete particle structure and excellent performance, and can be reused to assemble a new lithium iron phosphate positive electrode material battery. The multifunctional solvent used in the method is low in price and environmentally friendly. The multifunctional solvent used can effectively combine the lithium iron phosphate positive electrode material with lithium ions and is conducive to improving the lithium replenishment efficiency in the subsequent process. The multifunctional solvent used utilizes the reducing property of the reducing solvent ethanol to repair the anti-site defects in the lithium iron phosphate cathode material, without the need to add expensive or toxic reducing agents, thus achieving the maximum utilization efficiency of the solvent. At the same time, the multifunctional solvent doped the lithium iron phosphate cathode material with elements and coated it with carbon during the repair process, so that the repaired lithium iron phosphate cathode material has a longer cycle life, which is better than the cycle life of commercial lithium iron phosphate cathode materials.

[0037] The present invention is further described below with reference to the accompanying drawings and in combination with preferred embodiments. It should be noted that the embodiments and features in the embodiments of the present application can be combined with each other without conflict.

[0038] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the embodiments of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0039] Reference Fig. 9 The embodiment of the present invention provides a method for repairing a lithium iron phosphate positive electrode material, comprising the following steps:

[0040] S1. Mixing the lithium iron phosphate positive electrode material with a multifunctional solvent and performing solvent thermal treatment.

[0041] Wherein, the multifunctional solvent in step S1 is prepared by mixing raw materials including a reducing solvent, a lithium salt and a doping agent; the reducing solvent is selected from ethanol; the lithium salt is selected from lithium acetate; and the doping agent is selected from polyvinyl pyrrolidone. The amount of ethanol is 10-20% of the mass of the lithium iron phosphate positive electrode material, the amount of lithium acetate is 10-20% of the mass of the lithium iron phosphate positive electrode material, and the amount of polyvinyl pyrrolidone is 0.5%-1% of the mass of the lithium iron phosphate positive electrode material. For example, if the lithium iron phosphate positive electrode material is 100mg, the amount of ethanol in the multifunctional solvent is 10mg-20mg, the amount of lithium acetate is 10-20mg, and the amount of polyvinyl pyrrolidone is 5-10mg. The mixing of the lithium iron phosphate positive electrode material and the multifunctional solvent includes: dissolving the doping agent polyvinyl pyrrolidone and the lithium iron phosphate positive electrode material in a reducing solvent, stirring for 5h-12h, within this stirring time range, polyvinyl pyrrolidone can well nucleate on the surface of the lithium iron phosphate positive electrode material and wrap the lithium iron phosphate particles to form a lithium-philic interface, which is beneficial to the subsequent lithium replenishment process, and then pouring lithium salt and stirring for 2h-5h, within this stirring time range, the lithium ions in the lithium salt can be well coupled with the lithium-philic interface of the lithium iron phosphate, forming a suitable lithium-rich layer on the surface of the lithium iron phosphate particles, which can provide the required lithium source during the calcination process. The solvent thermal treatment process is assisted by any one of ultrasound, hydrothermal, heating and pressurization. The temperature of the solvent thermal treatment is 150-180°C, and the time of the solvent thermal treatment is 5-12h.

[0042] S2. vacuum drying the precipitate obtained after the solvent thermal treatment.

[0043] Specifically, the vacuum drying temperature in step S2 is 60-120° C., and the drying time is 12 h-24 h. Within this drying temperature and time range, the residual trace moisture from the air and the reducing solvent ethanol used are dried.

[0044] S3. calcining the solid powder obtained by vacuum drying to obtain a repaired lithium iron phosphate positive electrode material.

[0045] Specifically, step S3 is operated as follows: the solid powder obtained by vacuum drying is calcined at 600-750°C in an argon and hydrogen environment for 2h-10h to obtain a repaired, doped, and carbon-coated lithium iron phosphate positive electrode material. Within this temperature and time range, lithium ions can be embedded into the lithium iron phosphate particles at this temperature to repair the lithium vacancies of the lithium iron phosphate. Maintaining it for a period of time allows the lithium ions to fully enter the interior, so that the repair process can continue. A more effective repair of lithium iron phosphate is achieved.

[0046] In a preferred embodiment, the present invention provides a lithium iron phosphate positive electrode material, which is prepared by the above-mentioned lithium iron phosphate positive electrode material repair method.

[0047] In a preferred embodiment, the present invention further provides a positive electrode sheet, comprising a current collector and a positive electrode material layer disposed on the surface of the current collector, wherein the material of the positive electrode material layer comprises the above-mentioned lithium iron phosphate positive electrode material.

[0048] In other preferred embodiments, the present invention provides a battery comprising the above-mentioned positive electrode sheet.

[0049] Example 1

[0050] An embodiment of the present invention provides a method for repairing a lithium iron phosphate positive electrode material, comprising the following steps: dissolving 10 mg of a surfactant polyvinyl pyrrolidone and waste lithium iron phosphate positive electrode material powder (100 mg) in an ethanol solution (15 mg), stirring for 5 hours, and then pouring lithium acetate (15 mg) into the above solution and stirring for 2 hours.

[0051] After being stirred for 2 h, the mixed solution was poured into a reactor for solvent thermal treatment at 180° C. for 5 h.

[0052] The precipitate obtained after the solvothermal reaction was vacuum dried at 120°C for 12 h.

[0053] The solid powder obtained by vacuum drying was calcined at 600°C for 5 hours in an argon and hydrogen environment to finally obtain a repaired lithium iron phosphate positive electrode material.

[0054] Embodiment 2:

[0055] An embodiment of the present invention provides a method for repairing a lithium iron phosphate positive electrode material, comprising the following steps: dissolving 10 mg of a surfactant polyvinyl pyrrolidone and waste lithium iron phosphate positive electrode material powder (100 mg) in an ethanol solution (15 mg), stirring for 5 hours, and then pouring lithium acetate (15 mg) into the above solution and stirring for 2 hours.

[0056] After being stirred for 2 h, the mixed solution was poured into a reactor for solvent thermal treatment at 180° C. for 5 h.

[0057] The precipitate obtained after the solvothermal reaction was vacuum dried at 120°C for 12 h.

[0058] The solid powder obtained by vacuum drying was calcined at 600°C for 10 hours in an argon and hydrogen environment to finally obtain a repaired lithium iron phosphate positive electrode material.

[0059] Embodiment 3:

[0060] An embodiment of the present invention provides a method for repairing a lithium iron phosphate positive electrode material, comprising the following steps: dissolving 10 mg of a surfactant polyvinyl pyrrolidone and waste lithium iron phosphate positive electrode material powder (100 mg) in an ethanol solution (15 mg), stirring for 5 hours, and then pouring lithium acetate (15 mg) into the above solution and stirring for 2 hours.

[0061] After being stirred for 2 h, the mixed solution was poured into a reactor for solvent thermal treatment at 180° C. for 5 h.

[0062] The precipitate obtained after the solvothermal reaction was vacuum dried at 120°C for 12 h.

[0063] The solid powder obtained by vacuum drying was calcined at 700°C for 2 hours in an argon and hydrogen environment to finally obtain a repaired lithium iron phosphate positive electrode material.

[0064] Example 4

[0065] An embodiment of the present invention provides a method for repairing a lithium iron phosphate positive electrode material, comprising the following steps: dissolving 10 mg of a surfactant polyvinyl pyrrolidone and waste lithium iron phosphate positive electrode material powder (100 mg) in an ethanol solution (15 mg), stirring for 5 hours, and then pouring lithium acetate (15 mg) into the above solution and stirring for 2 hours.

[0066] After being stirred for 2 h, the mixed solution was poured into a reactor for solvent thermal treatment at 180° C. for 5 h.

[0067] The precipitate obtained after the solvothermal reaction was vacuum dried at 120°C for 12 h.

[0068] The solid powder obtained by vacuum drying was calcined at 700°C for 5 hours in an argon and hydrogen environment to finally obtain a repaired lithium iron phosphate positive electrode material.

[0069] Example 5

[0070] An embodiment of the present invention provides a method for repairing a lithium iron phosphate positive electrode material, comprising the following steps: dissolving 10 mg of a surfactant polyvinyl pyrrolidone and waste lithium iron phosphate positive electrode material powder (100 mg) in an ethanol solution (15 mg), stirring for 5 hours, and then pouring lithium acetate (15 mg) into the above solution and stirring for 2 hours.

[0071] After being stirred for 2 h, the mixed solution was poured into a reactor for solvent thermal treatment at 180° C. for 5 h.

[0072] The precipitate obtained after the solvothermal reaction was vacuum dried at 120°C for 12 h.

[0073] The solid powder obtained by vacuum drying was calcined at 750°C for 2 hours in an argon and hydrogen environment to finally obtain a repaired lithium iron phosphate positive electrode material.

[0074] Experimental testing and analysis

[0075] The above amount of lithium acetate is related to the amount of lithium ions measured by the inductively coupled plasma spectrometer of the waste lithium-ion battery. The amount of lithium acetate added is more than the amount of lithium ions missing from the waste lithium ions. Because the amount of lithium ions consumed during the regeneration process is lost, experiments have confirmed that it is generally 10%-20% of the mass of the waste lithium iron phosphate. If the amount is too much, there will be too many lithium ions remaining. Lithium ions will form compounds such as lithium carbonate or lithium hydroxide, which will produce gas during the long cycle of the battery, and most of the compounds formed are non-conductive, thus affecting the cycle performance of lithium iron phosphate. If the amount is too little, the waste lithium iron phosphate cannot be effectively repaired and cannot be restored to the ideal capacity. Polyvinyl pyrrolidone is used to coat the surface of lithium iron phosphate particles. According to the experiment, the optimal amount is 0.5-1% of the mass of the waste lithium iron phosphate. Because too much will be too thick to be coated, which is not conducive to lithium ion transmission during the repair process, and too thin to form an active surface, which is not conducive to the combination of lithium ions and the surface of phosphate particles during the hydrothermal process. The function of ethanol is to dissolve polyvinyl pyrrolidone and lithium acetate and allow the waste lithium iron phosphate to be fully mixed with them, so the selected mass can be 10%-20% of the waste lithium iron phosphate.

[0076] The performance of the lithium iron phosphate positive electrode materials obtained in the above examples was tested and analyzed respectively.

[0077] Structural analysis:

[0078] Figure 1The experimental data of the above five embodiments can be obtained from the data in the figure. The change of temperature and the change of holding time will affect the repair of lithium iron phosphate. As the temperature changes from 600 degrees Celsius for 5 hours to 600 degrees Celsius for 10 hours, it can be seen that the performance of repairing lithium iron phosphate decreases. This is due to the extension of time. At this temperature, the phosphoric acid particles may become larger, so the heating temperature time cannot be too long. Therefore, in order to obtain better repair conditions, we raise the temperature to 700 degrees Celsius, and heat for 2 hours and 5 hours at 700 degrees Celsius. The performance at 700 degrees Celsius is significantly higher than that at 600 degrees Celsius. We found that heating at 700 degrees Celsius for 5 hours is better than that at 2 hours. This is because a slightly longer temperature can be more conducive to lithium ions entering the interior of lithium iron phosphate for effective repair. If the temperature is too short, lithium ions cannot be completely embedded in the interior of lithium iron phosphate. However, when the temperature is raised to 750 degrees Celsius and kept for two hours, it is found that the performance has decreased significantly. The possible reason is that the grains of lithium iron phosphate may become larger and coarser at high temperatures, so the performance deteriorates. Therefore, based on the above data, we selected 700 degrees Celsius for 5 hours as the best condition for repairing lithium iron phosphate. The following data are all obtained under the best repair conditions.

[0079] See also Figure 2 , where the horizontal axis is 2-theta (degree) (the incident angle of the X-ray). An X-ray diffractometer is used to compare the XRD (Diffraction of x-rays) of the waste lithium iron phosphate positive electrode material and the regenerated positive electrode material collected in the embodiment of the present invention. It can be observed that after the repair, the diffraction peak corresponding to FePO4 in the waste lithium iron phosphate positive electrode material completely disappears, and the regenerated positive electrode material shows the same diffraction peak as the pure phase of the commercial lithium iron phosphate positive electrode material, and has a high degree of crystallinity. The waste lithium iron phosphate positive electrode material is completely converted into a usable lithium iron phosphate positive electrode material. See Figure 3 X-ray photoelectron spectroscopy (XPS) was used to perform in-depth analysis on the repaired cathode material collected in the embodiment of the present invention. The horizontal axis is the binding energy (eV). Specifically, Ar ion etching was performed for 5 minutes, and an XPS spectrum line was collected once. Four consecutive etchings were performed and five spectra were collected. The first spectrum was the surface information of the sample. As the number of etchings increased, the spectrum information was the bulk phase information. This shows that the lithium iron phosphate was effectively doped with N element through the proposed repair method.

[0080] Electrochemical performance analysis:

[0081] Preparation of battery pole pieces: The waste or regenerated positive electrode material according to the embodiment of the present invention, carbon black and polyvinylidene fluoride binder are fully mixed and ground in a mass ratio of 8:1:1, and N-methylpyrrolidone solvent is added to prepare positive electrode slurry, which is coated on aluminum foil. After vacuum drying at 120°C for 24 hours, it is made into a pole piece with a regular shape, and the pole piece quality is recorded.

[0082] Electrochemical performance test: The obtained electrode was assembled with lithium sheet, spring, gasket and Celgard diaphragm in a glove box to obtain button battery. The assembled battery was electrochemically tested using Wuhan Blue Electric Battery Test System. The results are as follows: Figure 4 As shown, the horizontal axis is the number of cycles, the vertical axis on the left is the discharge capacity (mAh / g), the vertical axis on the right is the coulomb efficiency, the voltage window is 2.5-4.3V, and at a current density of 1C, the first discharge capacity of the button cell made of waste lithium iron phosphate positive electrode material is only 104mAh / g; the first discharge capacity of the button cell assembled with the regenerated lithium iron phosphate positive electrode material prepared in the embodiment of the present invention is increased to 139mAh / g, and the capacity retention rate after 1000 cycles is close to 80%, indicating that the regeneration method provided by the present invention significantly improves the electrochemical performance of the positive electrode of the waste lithium iron phosphate positive electrode material. The capacity retention rate of the repaired lithium iron phosphate positive electrode material after 1000 cycles (76.6%) is higher than the capacity retention rate of the commercial lithium iron phosphate positive electrode material after 1000 cycles (35.5%).

[0083] Preparation of soft-pack battery pole piece: The same mass of discarded or regenerated positive electrode materials, carbon black and polyvinylidene fluoride binder according to the embodiment of the present invention are fully mixed and ground in a mass ratio of 9:0.5:0.5, and N-methylpyrrolidone solvent is added to prepare positive electrode slurry, which is applied on aluminum foil and vacuum dried at 120°C for 24 hours to form a pole piece with a regular shape. Commercial graphite, carbon black and polyvinylidene fluoride binder are fully mixed and ground in a mass ratio of 9:0.5:0.5, and N-methylpyrrolidone solvent is added to prepare negative electrode slurry, which is applied on copper foil and vacuum dried at 120°C for 24 hours to form a negative electrode pole piece with a regular shape.

[0084] Electrochemical performance test: The obtained positive and negative electrodes and Celgard separators were assembled into battery cells, vacuum dried at 60°C for 12 hours, and then injected with electrolyte to encapsulate and make soft-pack batteries. The assembled soft-pack batteries were electrochemically tested using the Wuhan Blue Electric Battery Test System. The results are as follows: Figure 5As shown, the horizontal axis is the number of cycles, the vertical axis on the left is the discharge capacity (mAh), the vertical axis on the right is the coulomb efficiency, the voltage window is 2.9-4.2V, and at a current density of 0.3C, the discharge specific capacity of the soft-pack battery made of waste lithium iron phosphate positive electrode material is only about 170mAh; the discharge capacity of the soft-pack battery assembled with the repaired lithium iron phosphate positive electrode material prepared in the embodiment of the present invention is about 270mAh, and the capacity retention rate after 300 cycles is close to 99%. The electrochemical properties of discharge capacity and capacity retention rate are much higher than those of the waste lithium iron phosphate positive electrode material, which shows that the regeneration method provided by the present invention significantly improves the electrochemical performance of the positive electrode of the waste lithium iron phosphate positive electrode material.

[0085] Preparation of battery pole pieces: The waste or regenerated positive electrode material according to the embodiment of the present invention, carbon black and polyvinylidene fluoride binder are fully mixed and ground in a mass ratio of 8:1:1, and N-methylpyrrolidone solvent is added to prepare positive electrode slurry, which is coated on aluminum foil. After vacuum drying at 120°C for 24 hours, it is made into a pole piece with a regular shape, and the pole piece mass is recorded.

[0086] Electrochemical performance test: The obtained electrode was assembled with lithium sheet, spring, gasket and Celgard diaphragm in a glove box to obtain button battery. The assembled battery was electrochemically tested using Wuhan Blue Electric Battery Test System. The results are as follows: Figure 6a and 6b As shown, Figure 6a This is the polarization voltage change diagram of waste lithium iron phosphate positive electrode material during the cycle process; Figure 6b This is the polarization voltage change diagram of the repaired lithium iron phosphate positive electrode material during the cycle process. Figure 6a and 6b The horizontal axis is the discharge capacity (mAh / g), and the vertical axis is the voltage (V). The voltage window is 2.5-4.3V. At a current density of 1C, the polarization voltage of the button cell made of waste lithium iron phosphate positive electrode material increases continuously during the electrochemical cycle, and the polarization voltage is 203mV after 500 cycles. The polarization voltage of the repaired lithium iron phosphate positive electrode material remains basically unchanged during the cycle, and the polarization voltage is 58.9mV after 500 cycles. On the other hand, the discharge capacity of the repaired lithium iron phosphate positive electrode material is about 140mAh / g, which is much higher than the discharge capacity of the discarded lithium iron phosphate positive electrode material of 100mAh / g. This means that the discarded lithium iron phosphate positive electrode material can be effectively repaired by the method of the embodiment of the present invention, and a longer cycle life can be obtained.

[0087] Figure 7 This is the refined XRD spectrum of the lithium iron phosphate cathode material before repair. Figure 8This is a refined XRD spectrum of the repaired lithium iron phosphate cathode material. From the refined results, it can be seen that after the repair, the anti-site defects of the lithium iron phosphate cathode material are reduced from the original 4.28% to 1.46%, which also proves that the anti-site defects are effectively repaired by the method of the embodiment of the present invention.

[0088] A multifunctional solvent for repairing, doping and carbon coating of lithium iron phosphate provided by an embodiment of the present invention has at least the following beneficial effects: the repair uses a multifunctional solvent to first activate the surface of the lithium iron phosphate positive electrode material, and the surface of the lithium iron phosphate positive electrode material after the activation treatment can effectively combine with lithium ions during the solvent thermal process, and no lithium salt needs to be added to supplement lithium ions during the subsequent calcination process, which is conducive to more effective repair of the lithium iron phosphate positive electrode material during calcination. Another point is that the multifunctional solvent can effectively repair the lithium iron anti-site defects in the lithium iron phosphate positive electrode material by using the reducing property of alcohols in the process of treating lithium iron phosphate, thereby repairing the anti-site defects, which plays a vital role in the lithium supplementation process of the lithium iron phosphate positive electrode material in the subsequent calcination process, and effectively reduces the diffusion barrier of lithium ions entering the lithium iron phosphate positive electrode material. More importantly, the multifunctional solvent can perform element doping and carbon coating on the surface of the lithium iron phosphate positive electrode material during the treatment and subsequent calcination process. And this element doping and carbon coating can achieve a long life cycle of the repaired lithium iron phosphate positive electrode material. Combining the advantages of the above multifunctional solvents, the capacity retention rate of the repaired lithium iron phosphate cathode material is close to 80% after 1000 cycles. The multifunctional solvent used in the method is low-cost, environmentally friendly, and has simple steps, which is suitable for large-scale repair of lithium iron phosphate cathode materials.

[0089] The above content is a further detailed description of the present invention in combination with specific / preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, without departing from the concept of the present invention, they can also make several substitutions or modifications to these described embodiments, and these substitutions or modifications should be regarded as belonging to the protection scope of the present invention. In the description of this specification, the description of the reference terms "an embodiment", "some embodiments", "preferred embodiments", "examples", "specific examples" or "some examples" means that the specific features, structures, materials or characteristics described in combination with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily target the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in a suitable manner in any one or more embodiments or examples. In the absence of mutual contradiction, those skilled in the art can combine and combine the different embodiments or examples described in this specification and the features of different embodiments or examples. Although the embodiments of the present invention and their advantages have been described in detail, it should be understood that various changes, substitutions and modifications can be made herein without departing from the scope of protection of the patent application.

Claims

1. A method for repairing a lithium iron phosphate positive electrode material, characterized in that: The following steps are involved: S1. Mixing the lithium iron phosphate positive electrode material with a multifunctional solvent and performing a solvent thermal treatment; the multifunctional solvent is prepared by mixing ethanol, lithium acetate and polyvinyl pyrrolidone; wherein the mixing of the lithium iron phosphate positive electrode material with the multifunctional solvent comprises: dissolving polyvinyl pyrrolidone and the lithium iron phosphate positive electrode material in ethanol, stirring for 5h-12h, then pouring lithium acetate and stirring for 2h-5h; wherein the amount of the ethanol is 10-20% of the mass of the lithium iron phosphate positive electrode material, the amount of the lithium acetate is 10-20% of the mass of the lithium iron phosphate positive electrode material, and the amount of the polyvinyl pyrrolidone is 0.5%-1% of the mass of the lithium iron phosphate positive electrode material; wherein the temperature of the solvent thermal treatment is 150-180°C, and the time of the solvent thermal treatment is 5-12h; S2, vacuum drying the precipitate obtained after the solvent thermal treatment; S3, calcining the solid powder obtained by vacuum drying to obtain a repaired lithium iron phosphate positive electrode material; The solid powder obtained by vacuum drying is calcined at 700°C in an argon and hydrogen environment for 5 hours to obtain a repaired, doped and carbon-coated lithium iron phosphate positive electrode material; the lithium iron phosphate is coated with polyvinyl pyrrolidone in the multifunctional solvent, so that the surface of the lithium iron phosphate positive electrode material is doped with nitrogen during the heat treatment and calcination process, and the long life cycle of the repaired lithium iron phosphate positive electrode material is achieved by nitrogen doping and carbon coating.

2. The method for repairing lithium iron phosphate positive electrode material according to claim 1, characterized in that: In step S1, the solvent thermal treatment process is assisted by any one of ultrasound, hydrothermal, and heating and pressurization.

3. The method for repairing lithium iron phosphate positive electrode material according to claim 1, characterized in that: In step S2, the vacuum drying temperature is 60-120°C, and the drying time is 12h-24h.

4. A lithium iron phosphate positive electrode material, characterized in that: The lithium iron phosphate positive electrode material is prepared by the repairing method of any one of claims 1 to 3.

5. A positive electrode sheet, characterized in that: It comprises a current collector and a positive electrode material layer arranged on the surface of the current collector, wherein the material of the positive electrode material layer comprises the lithium iron phosphate positive electrode material according to claim 4.

6. A battery, characterized in that: Including the positive electrode sheet as claimed in claim 5.

Citation Information

Patent Citations

  • Method for repair and regeneration of waste lithium iron phosphate battery cathode material

    CN102208707A

  • Preparation method for lithium iron phosphate

    WO2015196853A1

Cited By

  • Composite repairing and regenerating method for waste lithium iron phosphate material

    CN121790578A