A method for efficiently removing heavy metals from water based on lignin sulfonate modified cobalt-doped zero-valent iron composites
Preparation of lignin sulfonate modified cobalt-doped zero-valent iron composite material through ball milling, solving the problem of reducing zero-valent iron activity and large-scale production waste liquid, achieving efficient removal of heavy metals in water, with significant economic and environmental effect.
Patent Information
- Application Number
- CN202211095761.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-08
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-09-08
AI Technical Summary
The existing zero-valent iron has reduced activity and application limitations in removing heavy metals in water, and the problem of waste liquid synthesis by wet chemical method is difficult to solve on a large-scale production.
Lignosulfonate modified cobalt-doped zero-valent iron composite material by ball milling, modifying the zero-valent iron surface to improve its activity in removing heavy metals, using sodium lignin sulfonate, cobalt chloride hexahydrate and zero-valent iron Modification.
It significantly improves the efficiency and long-term effectiveness of zero-valent iron to remove heavy metals, simplifies the process flow, is suitable for large-scale promotion, and has economic and environmental benefits.
Smart Images

Figure CN115432796B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of environmental chemistry, and in particular to a method for efficiently removing heavy metals from water based on a lignin sulfonate-modified cobalt-doped zero-valent iron composite material. Background Art
[0002] Heavy metal pollution in water bodies seriously restricts the use of water resources and seriously harms the ecological environment and human health. Zero-valent iron, as an economical and environmentally friendly engineering material that has attracted widespread attention at home and abroad, has been widely used in treating heavy metal pollution in wastewater and groundwater because it can remove different heavy metals through adsorption, reduction or synergistic effects, thereby reducing the heavy metal toxicity in the water environment.
[0003] But the core of zero-valent iron, Fe 0 The easy oxidation property will make the iron oxide layer on its surface thicker, greatly reducing the effectiveness of zero-valent iron. In order to promote the activity of zero-valent iron, domestic and foreign scholars have designed a variety of modification methods to change the surface structure of zero-valent iron, such as metal doping, stabilization and sulfidation, but the synthesis of modified zero-valent iron in the past was mainly wet chemical method, which is easy to produce waste liquid and is not conducive to large-scale production. At present, zero-valent iron-based materials synthesized by mechanical ball milling based on "solid-solid reaction" have begun to be used in actual environmental remediation due to their synthetic advantages, but a single modifier cannot solve the application defects of zero-valent iron well. Therefore, further improving the activity of ball-milled zero-valent iron-based materials is crucial to improving the effectiveness and long-term effectiveness of zero-valent iron. Summary of the invention
[0004] The purpose of the present invention is to provide a method for efficiently removing heavy metals from water bodies based on a lignin sulfonate-modified cobalt-doped zero-valent iron composite material, which has the advantage of improving the activity of zero-valent iron in treating heavy metals by a co-modification method in view of the limitations of existing zero-valent iron modification and application.
[0005] The above technical objectives of the present invention are achieved through the following technical solutions:
[0006] A method for efficiently removing heavy metals from water based on a lignin sulfonate modified cobalt-doped zero-valent iron composite material comprises the following steps:
[0007] S1: Sodium lignin sulfonate, cobalt chloride hexahydrate and zero-valent iron were used to prepare lignin sulfonate modified cobalt-doped zero-valent iron composites by ball milling;
[0008] S2: Add lignin sulfonate modified cobalt doped zero-valent iron into the pollutant solution to remove the pollutants.
[0009] The lignin sulfonate modified cobalt-doped zero-valent iron is zero-valent iron whose surface is modified by lignin sulfonic acid groups and doped with cobalt.
[0010] Preferably, the ball milling method described in S1 comprises the steps of placing sodium lignin sulfonate, cobalt chloride hexahydrate and iron powder in a ball mill of a ball mill, and starting the ball mill to complete the ball milling process.
[0011] Preferably, the ball mill is a planetary ball mill, a vibrating ball mill or a sand mill.
[0012] Preferably, the ball mill is equipped with grinding media, which are iron beads, steel balls, silicon nitride beads or zirconium oxide beads, and the diameter of the grinding media is 0.15-10 mm.
[0013] Preferably, the ball milling speed in the ball milling process in S1 is 400 rpm, and the ball milling time is 2-20 h.
[0014] Preferably, the iron powder is micron-sized zero-valent iron.
[0015] Preferably, the pollutant concentration of the pollutant solution in S2 is 5-20 mg / L, the reaction temperature in S2 is 0-30° C., and the reaction pH is 5-7.
[0016] Preferably, the amount of lignin sulfonate modified cobalt doped zero-valent iron in S2 is 1-2 g / L.
[0017] Preferably, the pollutant removal process of the lignin sulfonate-modified cobalt-doped zero-valent iron is carried out by mechanical stirring or shaking.
[0018] The beneficial effects of the present invention are:
[0019] 1. The ball milling method for preparing lignin sulfonate modified cobalt-doped zero-valent iron composites is simple and easy to operate;
[0020] 2. The lignin sulfonate modified cobalt doped zero-valent iron composite material provided by the present invention has a better effect of removing heavy metals than simple lignin sulfonate modified zero-valent iron and cobalt doped zero-valent iron;
[0021] 3. The technology of the present invention does not have excessively high requirements on equipment, is conducive to large-scale promotion, and has significant economic, environmental and social effects. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The SEM-EDS images of the 4% LS-1% Co-ZVI composite material prepared in Example 1, wherein a is a SEM image; b is an EDS image;
[0023] Figure 2 The XPS spectra of cobalt and sulfur elements of 4% LS-1% Co-ZVI prepared in Example 1;
[0024] Figure 3This is a comparative diagram of the removal of hexavalent chromium from water by ball-milling lignin sulfonate-modified cobalt-doped zero-valent iron and modified composite materials with different mass ratios prepared in Example 1;
[0025] Figure 4 This is a comparative diagram of the removal of hexavalent chromium from water by ball-milling lignin sulfonate-modified cobalt-doped zero-valent iron and different sodium lignin sulfonate quality-modified materials in Example 2;
[0026] Figure 5 This is a comparative diagram of the removal of hexavalent chromium from water by ball-milling lignin sulfonate modified cobalt-doped zero-valent iron and modified materials with different ball-milling times in Example 3;
[0027] Figure 6 This is a diagram showing the effect of ball-milling lignin sulfonate to modify cobalt-doped zero-valent iron and remove nickel from water in Example 4;
[0028] Figure 7 This is a diagram showing the effect of ball-milled lignin sulfonate modified with cobalt-doped zero-valent iron and removing zinc from water in Example 5. DETAILED DESCRIPTION
[0029] The present invention will be further described below in conjunction with specific embodiments. The following are only specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto.
[0030] The main raw materials involved in the following examples, such as commercial iron powder, sodium lignin sulfonate and cobalt chloride hexahydrate, were all from Aladdin (Shanghai, China), and all reagents were analytically pure, of which the iron powder had a particle size of 37 μm, and sodium lignin sulfonate and cobalt chloride hexahydrate were in powder form. The ball milling medium used was a zirconium oxide ball milling bead with a particle size of 6 mm and a volume of 20% of the cavity. The ball milling speed was adjusted to 400 rpm and the ball milling time was 10 h. After the ball milling was completed, the obtained sodium lignin sulfonate modified zero-valent iron was separated from the grinding medium with a sieve under a nitrogen atmosphere.
[0031] Example 1
[0032] Comparative effect of ball-milled lignin sulfonate-modified cobalt-doped zero-valent iron and modified composite materials with different mass ratios on removing hexavalent chromium from water.
[0033] Weigh 2.5g of zero-valent iron powder and a certain mass of sodium lignin sulfonate and cobalt chloride hexahydrate and place them in a ball mill, and fill the mill with argon; turn on the ball mill to obtain lignin sulfonate-modified cobalt-doped zero-valent iron x% LS-y% Co–ZVI (x% and y% are the mass ratios of sodium lignin sulfonate and cobalt chloride hexahydrate to zero-valent iron, respectively). Add 200mL of 10mg / L Cr(VI) solution to a 250mL beaker, the pH of the solution is 5.15, add 0.2g of lignin sulfonate-modified cobalt-doped zero-valent iron, and mix by mechanical stirring in an open aerobic environment at a speed of 400r / min. Take samples at regular intervals to measure the concentration of Cr(VI) in the system. The experimental results are as follows: Figure 3 As shown in the figure, the removal effect of unmodified zero-valent iron on Cr(VI) is almost negligible, while the removal effect of zero-valent iron modified with lignin sulfonate and doped with cobalt on Cr(VI) is significantly improved, among which 4% LS-1% Co-ZVI can remove 72.6% of Cr(VI) within 2 minutes, with the fastest removal speed.
[0034] Example 2
[0035] Preparation of lignin sulfonate modified cobalt-doped zero-valent iron by ball milling and removal of different quality-modified materials of sodium lignin sulfonate
[0036] Comparative effect diagram of hexavalent chromium in water.
[0037] Weigh 2.5g of zero-valent iron powder and 0.025g of cobalt chloride hexahydrate and place them in a ball mill. Then add different masses of sodium lignin sulfonate and fill the mill with argon. Turn on the ball mill to obtain lignin sulfonate-modified cobalt-doped zero-valent iron x% LS-1% Co–ZVI (x% is the mass ratio of sodium lignin sulfonate to zero-valent iron). Add 200mL of 10mg / L Cr(VI) solution to a 250mL beaker. The pH of the solution is 5.15. Add 0.2g of lignin sulfonate-modified cobalt-doped zero-valent iron. Mix by mechanical stirring in an open aerobic environment. The speed is set to 400r / min. Take samples at regular intervals to measure the concentration of Cr(VI) in the system. The experimental results are as follows: Figure 4 As shown in Figure 2, with the increase of the mass of lignin sulfonate, the removal rate of Cr(VI) by LS-1%Co-ZVI was faster and significantly higher than that by 1%Co-ZVI, and the performance of 4%LS-1%Co-ZVI was better than that of 4%LS-ZVI.
[0038] Example 3
[0039] Comparative effect of ball-milled lignin sulfonate modified cobalt-doped zero-valent iron and modified materials with different ball-milling times on removing hexavalent chromium from water.
[0040] Weigh 2.5g of zero-valent iron powder, 0.1g of sodium lignin sulfonate and 0.025g of cobalt chloride hexahydrate and place them in a ball mill jar, and fill the jar with argon; turn on the ball mill and mill for a certain period of time to obtain lignin sulfonate-modified cobalt-doped zero-valent iron 4% LS-1% Co–ZVI(x) (x is a different ball milling time, unit: h). Add 200mL of 10mg / L Cr(VI) solution to a 250mL beaker, the pH of the solution is 5.15, add 0.2g of lignin sulfonate-modified cobalt-doped zero-valent iron, and mix by mechanical stirring in an open aerobic environment, with the speed set to 400r / min. Take samples at regular intervals to measure the concentration of Cr(VI) in the system. The experimental results are as follows: Figure 5 As shown in Figure 3, the removal rate of Cr(VI) by 4% LS-1% Co–ZVI increased with the increase of ball milling time, but when the ball milling time was 10 h, its removal effect within 2 min was better than that of the material milled for 20 h.
[0041] Example 4
[0042] Effect of ball-milled lignin sulfonate modified cobalt-doped zero-valent iron and nickel removal from water.
[0043] Weigh 2.5g zero-valent iron powder, 0.1g sodium lignin sulfonate and 0.025g cobalt chloride hexahydrate into a ball mill, and fill the mill with argon; turn on the ball mill and mill for 10h to obtain lignin sulfonate modified cobalt-doped zero-valent iron 4% LS-1% Co–ZVI. Add 200mL of a solution containing 10mg / L nickel in a 250mL three-necked flask, the pH of the solution is 5.79, add 0.2g of lignin sulfonate modified cobalt-doped zero-valent iron material, mix with mechanical stirring in an open aerobic environment, and set the speed to 400r / min. Take samples regularly to measure the nickel concentration in the solution. The results are as follows: Figure 6 In 40 min, ZVI and 1% Co–ZVI could only remove 16.7% and 68.0% of nickel, respectively, while the efficiency of nickel removal by 4% LS-1% Co–ZVI reached 93.5%.
[0044] Example 5
[0045] Effect of ball-milled lignin sulfonate modified cobalt-doped zero-valent iron and zinc removal from water.
[0046] Weigh 2.5g zero-valent iron powder, 0.1g sodium lignin sulfonate and 0.025g cobalt chloride hexahydrate into a ball mill, and fill the mill with argon; turn on the ball mill and mill for 10h to obtain lignin sulfonate modified cobalt-doped zero-valent iron 4% LS-1% Co–ZVI. Add 200mL of a solution containing 10mg / L zinc in a 250mL three-necked flask, the pH of the solution is 4.96, add 0.16g of lignin sulfonate modified cobalt-doped zero-valent iron material, mix with mechanical stirring in an open aerobic environment, and set the speed to 400r / min. Take samples regularly to measure the zinc concentration in the solution. The results are as follows: Figure 7 As shown in the figure, ZVI can only remove 5% of zinc within 40 min, 1% Co–ZVI can only remove 54.8% of zinc, while 4% LS-1% Co–ZVI can remove 82% of zinc within 2 min and completely remove zinc within 5 min.
[0047] The specific embodiments described above further illustrate the technical problems, technical solutions and beneficial effects solved by the present invention. It should be understood that the above are only specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for efficiently removing heavy metals from water based on lignin sulfonate modified cobalt-doped zero-valent iron composite material, characterized in that: The following steps are involved: S1: Sodium lignin sulfonate, cobalt chloride hexahydrate and zero-valent iron were used to prepare lignin sulfonate modified cobalt-doped zero-valent iron composites by ball milling; The operation in S1 is specifically as follows: weighing 2.5 g of zero-valent iron powder and 0.025 g of cobalt chloride hexahydrate and placing them in a ball mill, then adding different masses of sodium lignin sulfonate, and filling the mill with argon; turning on the ball mill to obtain lignin sulfonate-modified cobalt-doped zero-valent iron x% LS-1% Co–ZVI, where x% is the mass ratio of sodium lignin sulfonate to zero-valent iron; S2: Add lignin sulfonate modified cobalt doped zero-valent iron into the pollutant solution to remove the pollutants. The lignin sulfonate modified cobalt-doped zero-valent iron is zero-valent iron whose surface is modified by lignin sulfonic acid groups and doped with cobalt; The operation in S2 is specifically as follows: adding 200 mL of 10 mg / L Cr(VI) solution into a 250 mL beaker, the solution pH is 5.15, adding 0.2 g of lignin sulfonate-modified cobalt-doped zero-valent iron, mixing by mechanical stirring in an open aerobic environment, the speed is set to 400 r / min, and sampling at regular intervals to determine the concentration of Cr(VI) in the system; The raw materials involved in the above method steps - commercial iron powder, sodium lignin sulfonate and cobalt chloride hexahydrate are all from Aladdin and Shanghai, and all reagents are of analytical grade. The iron powder has a particle size of 37 μm, sodium lignin sulfonate and cobalt chloride hexahydrate are in powder form, and the ball milling medium used is zirconium oxide ball milling beads with a particle size of 6 mm and a cavity volume of 20%. The ball milling speed is adjusted to 400 rpm, and the ball milling time is 10 h. After the ball milling, the obtained sodium lignin sulfonate-modified zero-valent iron is separated from the grinding medium with a sieve under a nitrogen atmosphere.
2. The method for efficiently removing heavy metals from water based on lignin sulfonate modified cobalt-doped zero-valent iron composite material according to claim 1, characterized in that: The ball mill is a planetary ball mill, a vibrating ball mill or a sand mill.