Spiroacridine triazine bisphosphine oxide-containing ternary thermally excited delayed fluorescent guest material and preparation method and application thereof

By designing a ternary thermally excited delayed fluorescence material containing spiroacridine triazine bisphosphine oxide, and using the spirocyclic and diphenylphosphine oxide group structures, the problem of non-radiative consumption of triplet excitons in OLED materials has been solved and achieved Efficient thermally excited delayed fluorescence device performance improvement and environmentally friendly blue-green light emitting effect.

CN115433232BActive Publication Date: 2024-09-27HEILONGJIANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110622195.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-06-03
Publication Date
2024-09-27
Estimated Expiration
2041-06-03

AI Technical Summary

Technical Problem

The non-radiative consumption of triplet excitons in existing OLED materials results in low internal quantum efficiency and only 5.0% external quantum efficiency. In addition, limited heavy metal material resources and environmental pollution problems make it difficult to achieve efficient and sustainable luminescent material applications.

Method used

A ternary thermally excited delayed fluorescence material containing spiroacridine triazine bisphosphine oxygen was designed. By introducing diphenylphosphine oxygen groups and spirocyclic structures, the molecular rigidity was enhanced, intermolecular interactions were weakened, and the spectral red shift was suppressed. and aggregation quenching, optimizing the ICT effect and improving TADF performance.

Benefits of technology

A high-efficiency thermally excited delayed fluorescence blue light device driven by ultra-low voltage is realized. The current efficiency reaches 28.0cd·A-1 and the power efficiency reaches 39.8lm·W-1. It has good TADF performance and thermodynamic stability, and improves the luminous efficiency and brightness. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003099989930000016
    Figure HDA0003099989930000016
  • Figure HDA0003099989930000041
    Figure HDA0003099989930000041
  • Figure HDA0003099989930000011
    Figure HDA0003099989930000011
Patent Text Reader

Abstract

The present invention discloses a ternary thermally excited delayed fluorescent guest material containing spiroacridine triazine diphosphine oxide and its preparation method and application. Specifically, the acceptor triazine unit is further modified by a diphenylphosphine oxide group to obtain a spiroacridine triazine group aromatic phosphine oxide thermally excited delayed fluorescent guest material, the guest material has a certain rigidity and twisted configuration and a strong charge transfer effect, and can achieve strong luminescence. In a binary D-A type TADF system, a diphenylphosphine oxide group is introduced as a second acceptor, thereby constructing a ternary blue light TADF material, enhancing delayed fluorescence emission, having good thermodynamic stability, improving the luminous efficiency and brightness of an organic electroluminescent material, and being able to prepare an organic electroluminescent diode with excellent performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electroluminescent materials, and in particular relates to a ternary thermally excited delayed fluorescent guest material containing spiroacridine triazine diphosphine oxide, a preparation method and application thereof. Background Art

[0002] Organic Light Emitting Diode (OLED) has the advantages of high color quality, wide viewing angle, low cost, light weight, low driving voltage and fast response speed, which promotes its implementation in many daily applications, such as display technology, solid-state lighting, mobile phones, smart watches, etc. The electrons and holes generated by the electric field of OLED are injected from the cathode and anode into the light-emitting layer through the charge transport layer respectively. The injected holes and electrons recombine in the light-emitting layer, and according to the spin statistics rule, singlet and triplet excitons are generated in a ratio of 1:3. In essence, organic molecules can only use singlet excitons to radiate light, while most triplet excitons consume energy in non-radiative forms such as heat. Therefore, the internal quantum efficiency (IQE) of fluorescent OLED is limited to 25%, resulting in an external quantum efficiency (EQE) of only 5.0%.

[0003] In order to solve this key problem, researchers have been focusing on utilizing the remaining 75% triplet excitons in the form of radiation to find a suitable solution to improve device efficiency. In 1998, Forrest et al. first demonstrated a platinum-based complex as a phosphorescence (PH) luminescent material electroluminescent luminescent material, utilizing the strong spin-orbit coupling effect of heavy metals to achieve the conversion and luminescence of singlet and triplet excitons. Although this luminescent material only achieved an EQE of 4.0%. Subsequently, a large number of heavy metal complexes, such as iridium and platinum complex luminescent materials, were reported, and their device performance was significantly improved. However, heavy metals, especially precious metals, have limited resources, high costs and environmental pollution, which restrict their large-scale sustainable application. Organic molecules are relatively cheap and easy to design and prepare. Therefore, organic molecules have developed several methods that utilize triplet, localized and charge transfer hybrid states and triplet-polaron annihilation (TPA). In particular, the discovery of thermally excited delayed fluorescence technology has attracted widespread attention and achieved great success in the field of OLEDs. Adachi et al. first reported an OLED device with EQE>20% by utilizing pure organic matter. Currently, blue light TADF devices have achieved an EQE of up to 38%.

[0004] A core problem of TADF materials is the existence of concentration quenching and triplet-triplet annihilation. The linear DA structure of the luminescent material can achieve a large dihedral angle between the donor and the acceptor, thereby increasing the separation of HOMO and LUMO and reducing ΔE ST However, this often leads to low PLQY and red-shifted emission. Therefore, regulating the conjugation length and radiative transition rate constant of TADF molecules is an effective strategy to improve the performance of OLED devices. ST In the molecule, since the energy level of S1 is higher than that of T1, intersystem crossing (ISC) is also considered to be a competition for RISC. Therefore, the T1 state of the TADF molecule should be highly stable to allow the exciton to quickly transition from T1 to S1 and suppress triplet quenching. Summary of the invention

[0005] In order to overcome the above problems, the inventors have conducted intensive research and found that the spiro ring donor has a large spatial volume, which can extend the molecular skeleton of the macromolecular non-conjugated fragment, and can increase the distance between adjacent luminophores, weaken the interaction between adjacent molecules, thereby effectively weakening the aggregation quenching, and connecting with triazine with a large planar structure and strong electron-withdrawing ability can increase the tendency of horizontal arrangement, thereby effectively improving the horizontal orientation dipole ratio. Specifically, the acceptor triazine unit is further modified by a diphenylphosphine oxygen group to obtain a spiroacridine triazine group aromatic phosphine oxygen thermal excitation delayed fluorescence guest material. By designing the molecular structure, a spiro ring structure with an orthogonal geometric configuration is introduced to reduce the interaction between molecules, inhibit the quenching caused by the red shift of the spectrum and aggregation, and promote blue shift emission. The spiro carbon structure can enhance the rigidity of the molecule without increasing the π conjugation length, which helps the electron cloud overlap of HOMO and LUMO and improves the luminescence performance. The spiroacridine structure provides the basis for TADF materials and DA structure luminophores. The present invention is completed by introducing diphenylphosphinoyl groups into a binary DA system to construct a ternary TADF luminescent material based on a DA structure, utilizing the moderate electron-withdrawing induction effect and large steric effect of the phosphinoyl groups, optimizing the ICT effect while retaining the luminescent color to the maximum extent, inhibiting the quenching of excited states caused by non-radiative transitions and intermolecular interactions, thereby improving the TADF performance of the material and the efficiency of the device.

[0006] Specifically, the purpose of the present invention is to provide the following aspects:

[0007] In a first aspect, a ternary thermally excited delayed fluorescent guest material containing spiroacridine triazine diphosphine oxide is provided, wherein the guest material has spiroacridine triazine as a matrix and aromatic phosphine oxide as a second receptor.

[0008] In a second aspect, a method for preparing a ternary thermally excited delayed fluorescent guest material containing spiroacridine triazine bisphosphine oxide is provided, the method comprising: reacting a spiroacridine compound and a phosphine oxide compound in an organic solvent, extracting after the reaction, and then oxidizing the organic layer, optionally extracting and / or purifying to obtain the guest material.

[0009] In a third aspect, an electroluminescent device is provided, which is prepared by using a ternary thermally excited delayed fluorescent guest material containing a spiroacridine triazine bisphosphine oxide, which is prepared by the method described in the first aspect or the second aspect, wherein the electroluminescent device comprises a substrate layer, an anode, a hole injection layer, a hole transport layer, an exciton blocking layer, a light-emitting layer, a hole blocking layer, an electron transport layer, an electron injection layer and a cathode.

[0010] The beneficial effects of the present invention include:

[0011] (1) The ternary thermally excited delayed fluorescent guest material containing spiroacridine triazine diphosphine oxide provided by the present invention uses diphenylphosphine oxide group as the second acceptor, which can effectively increase the charge transfer effect and enhance the luminescence performance, which is beneficial to the design and performance improvement of the device.

[0012] (2) The ternary thermally excited delayed fluorescent guest material containing spiroacridine triazine bisphosphine oxide provided by the present invention has an orthogonal rigid twisted structure, which can effectively inhibit the interaction between molecules and thus inhibit the quenching effect.

[0013] (3) The ternary thermally excited delayed fluorescent guest material containing spiroacridine triazine bisphosphine oxide provided by the present invention can realize the preparation of high-efficiency thermally excited delayed fluorescent blue light devices driven by ultra-low voltage, and its current efficiency reaches a maximum value of 28.0 cd·A -1 , the power efficiency reaches a maximum of 39.8lm·W -1 .

[0014] (4) The ternary thermally excited delayed fluorescent guest material containing spiroacridine triazine bisphosphine oxide provided in the present invention has a small ΔE ST , has good TADF performance, enhances the charge transfer effect, and inhibits excited state quenching, thereby effectively improving the luminescence performance of the material.

[0015] (5) The ternary thermally excited delayed fluorescent guest material containing spiroacridine triazine bisphosphine provided by the present invention is used as the light-emitting layer of the blue-green light device, has high brightness and luminous efficiency, can well regulate the device performance, and is an excellent light emitter.

[0016] (6) The ternary thermally excited delayed fluorescent guest material containing spiroacridine triazine bisphosphine oxide provided by the present invention has good thermodynamic stability, the pyrolysis temperature can reach above 500°C, and the luminous efficiency and brightness of the organic electroluminescent material are improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 The ultraviolet spectrum and fluorescence spectrum of compound (I) in Example 1 of the present invention are shown;

[0018] Figure 2 The thermogravimetric analysis diagram of compound (I) in Example 1 of the present invention is shown;

[0019] Figure 3 The ultraviolet spectrum and fluorescence spectrum of compound (II) in Example 2 of the present invention are shown;

[0020] Figure 4 The thermogravimetric analysis diagram of compound (II) in Example 2 of the present invention is shown;

[0021] Figure 5 The ultraviolet spectrum and fluorescence spectrum of compound (III) in Example 3 of the present invention are shown;

[0022] Figure 6 The thermogravimetric analysis diagram of compound (III) in Example 3 of the present invention is shown;

[0023] Figure 7 The ultraviolet spectrum and fluorescence spectrum of compound (IV) in Example 4 of the present invention are shown;

[0024] Figure 8 The thermogravimetric analysis diagram of compound (IV) in Example 4 of the present invention is shown;

[0025] Fig. 9 The voltage-current density relationship curve of the electro-induced deep blue light device in Example 1 of the present invention is shown;

[0026] Fig.10 The voltage-brightness relationship curve of the electro-induced deep blue light device in Example 1 of the present invention is shown;

[0027] Fig.11 The brightness-current efficiency relationship curve of the electro-induced deep blue light device in Example 1 of the present invention is shown;

[0028] Fig.12 The brightness-power efficiency relationship curve of the electro-induced deep blue light device in Example 1 of the present invention is shown;

[0029] Fig.13 The relationship curve between brightness and external quantum efficiency of the electro-deep blue light emitting device in Example 1 of the present invention is shown;

[0030] Fig.14 The electroluminescence spectrum of the electroluminescent deep blue light device in Example 1 of the present invention is shown;

[0031] Fig.15 The voltage-current density relationship curve of the electro-induced deep blue light device in Example 2 of the present invention is shown;

[0032] Fig.16 The voltage-brightness relationship curve of the electro-induced deep blue light device in Example 2 of the present invention is shown;

[0033] Fig.17 The brightness-current efficiency relationship curve of the electro-induced deep blue light device in Example 2 of the present invention is shown;

[0034] Fig.18 The brightness-power efficiency relationship curve of the electro-induced deep blue light device in Example 2 of the present invention is shown;

[0035] Fig.19 The relationship curve between brightness and external quantum efficiency of the electro-deep blue light device in Example 2 of the present invention is shown;

[0036] Fig. 20 The electroluminescence spectrum of the electroluminescent deep blue light device in Example 2 of the present invention is shown;

[0037] Fig.21 The voltage-current density relationship curve of the electro-induced deep blue light device in Example 3 of the present invention is shown;

[0038] Fig. 22 The voltage-brightness relationship curve of the electro-induced deep blue light device in Example 3 of the present invention is shown;

[0039] Fig.23 The brightness-current efficiency relationship curve of the electro-induced deep blue light device in Example 3 of the present invention is shown;

[0040] Fig.24 The brightness-power efficiency relationship curve of the electro-induced deep blue light device in Example 3 of the present invention is shown;

[0041] Fig.25 The relationship curve between brightness and external quantum efficiency of the electro-deep blue light emitting device in Example 3 of the present invention is shown;

[0042] Fig.26 The electroluminescence spectrum of the electroluminescent deep blue light device in Example 3 of the present invention is shown;

[0043] Fig. 27 The voltage-current density relationship curve of the electro-induced deep blue light device in Example 4 of the present invention is shown;

[0044] Fig.28 The voltage-brightness relationship curve of the electro-induced deep blue light device in Example 4 of the present invention is shown;

[0045] Fig.29 The brightness-current efficiency relationship curve of the electro-induced deep blue light device in Example 4 of the present invention is shown;

[0046] Fig.30The brightness-power efficiency relationship curve of the electro-induced deep blue light device in Example 4 of the present invention is shown;

[0047] Fig.31 The relationship curve between brightness and external quantum efficiency of the electro-deep blue light emitting device in Example 4 of the present invention is shown;

[0048] Fig.32 The electroluminescence spectrum of the electroluminescent deep blue light device in Example 4 of the present invention is shown. DETAILED DESCRIPTION

[0049] According to a first aspect of the present invention, a ternary thermally excited delayed fluorescent guest material containing spiroacridine triazine bisphosphine oxide is provided. The guest material has spiroacridine triazine as a matrix and aromatic phosphine oxide as an acceptor.

[0050] Furthermore, the guest material comprises a compound having the following structural formula:

[0051]

[0052] Wherein, X is spiroacridinyl, and Y is diphenylphosphinoyl (Ph2OP).

[0053] Further, X is spiroacridiniumfluorenyl (SFA), spiroacridiniumoxanthenyl (SXA), spiroacridiniumthioanthenyl (STA) or spiroacridiniumsulfoneanthenyl (STOA).

[0054] In the present invention, the ternary thermally excited delayed fluorescent guest material containing spiroacridine triazine bisphosphine oxide has a rigid orthogonal molecular configuration, and its structure can effectively inhibit the interaction between molecules, thereby inhibiting the quenching effect.

[0055] In the present invention, the ternary thermally excited delayed fluorescent guest material containing spiroacridine triazine diphosphine oxide has spiroacridine triazine as the matrix, aromatic phosphine oxide as the receptor, specifically diphenylphosphine oxide as the receptor, wherein the phosphine oxide (P=O) group connects the aromatic group through the CP saturated bond, which can not only effectively block the conjugation effect, but also realize the role of the second receptor to enhance the charge transfer characteristics and improve the luminescence performance. Since the spiroacridine structure itself has a rigid orthogonal geometric configuration, the large torsion angle has the effect of interrupting the conjugation, so that the matrix itself has a higher triplet energy level, and the P=O group has the effect of polarizing the molecule, which can improve the electron injection and transmission ability of the molecule, and has a certain electron injection and transmission ability.

[0056] In the present invention, a phosphine oxygen group is introduced into the spiroacridine triazine system to realize the role of the second acceptor, so as to achieve a balance between a high triplet excited state energy level and a good charge transfer ability.

[0057] Specifically, the ternary thermally excited delayed fluorescent guest material containing spiroacridine triazine bisphosphine oxide comprises one or more of the compounds represented by the following formula (I) to formula (IV):

[0058] When X is SFA and Y is Ph2OP, the compound is SFATPTZDPO, and its structural formula is (Ⅰ);

[0059] When X is SXA and Y is Ph2OP, the compound is SXATPTZDPO, and its structural formula is (Ⅱ);

[0060] When X is STA and Y is Ph2OP, the compound is STATPTZDPO, and its structural formula is (III);

[0061] When X is STOA and Y is Ph2OP, the compound is STOATPTZDPO, and its structural formula is (IV);

[0062] The structural formulas of the compounds are as follows:

[0063]

[0064] According to a second aspect of the present invention, a method for preparing a ternary thermally excited delayed fluorescent guest material containing a spiroacridine triazine bisphosphine oxide is provided, the method comprising: reacting a spiroacridine compound and a phosphine oxide compound in an organic solvent, extracting after the reaction, and then oxidizing the organic layer, optionally extracting and / or purifying to obtain the guest material.

[0065] According to the present invention, the spiroacridine compound is preferably selected from spiroacridine fluorene, spiroacridine oxyanthracene, spiroacridine thioanthracene or spiroacridine sulfoneanthracene, and the phosphorus oxide compound is p-bromotriphenyltriazine bisphosphine oxide.

[0066] According to a preferred embodiment, the p-bromotriphenyltriazine bisphosphine oxide is prepared by catalytic and oxidative reaction of diphenylphosphine and its reaction ligand p-bromotriphenyltriazine in a solvent.

[0067] In the present invention, since diphenylphosphine is easily oxidized by air and has strong water absorption, diphenylphosphine is preferably added under anhydrous and oxygen-free conditions.

[0068] According to the present invention, the solvent is preferably a stable aprotic organic solvent, such as acetonitrile, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, hexamethylphosphoric triamide, and more preferably N,N-dimethylformamide in which bromotriphenyltriazine is extremely soluble.

[0069] According to the present invention, the catalytic reaction is carried out under alkaline conditions, and the substance that maintains the reaction in an alkaline environment is preferably a strong base weak acid salt, such as sodium acetate, sodium carbonate, sodium phosphate, sodium bicarbonate, and more preferably sodium acetate.

[0070] The sodium acetate can be used as a buffer to control the progress of the reaction and to keep the reaction alkaline.

[0071] In the present invention, the catalyst used in the catalytic reaction is a palladium compound with high activity and good selectivity. The palladium compound is preferably selected from any one or more of palladium chloride, palladium acetate, and dicyanobenzene palladium chloride, and palladium acetate is more preferred, such as palladium acetate with a concentration of 0.3-0.5%.

[0072] According to the present invention, the molar ratio of p-bromotriphenyltriazine, diphenylphosphine and strong base weak acid salt is (0.2-2.0):(0.5-5.0):(0.01-4), preferably (0.6-1.5):(1.0-3.0):(1.0-3.0), more preferably (0.9-1.1):(1.8-2.2):(2.0-2.6), for example 1:2.2:2.2.

[0073] According to the present invention, the catalytic reaction temperature is 60-180°C, preferably 100-140°C, more preferably 125-130°C; the catalytic reaction time is 8-20h, preferably 10-15h, more preferably 12-13h.

[0074] According to the present invention, the oxidant used in the oxidation reaction is preferably a peroxide, such as hydrogen peroxide, sodium peroxide, potassium peroxide, and more preferably hydrogen peroxide without producing side reactions.

[0075] In the present invention, spiroacridine compounds react with bromotriphenyltriazine bisphosphine oxide to generate p-bromotriphenyltriazine bisphosphine oxide compounds with spiroacridine triazine compounds as the matrix and phosphine oxide groups as the acceptors, so that the spiroacridine triazine compounds have higher triplet energy levels and improved luminescence performance.

[0076] According to the present invention, the organic solvent includes alcohols, organic acids, and benzene series, preferably benzene series, such as toluene, ethylbenzene, xylene, etc., and more preferably toluene with good solubility.

[0077] According to the present invention, the reaction for preparing the guest material is preferably carried out in a reaction system in which a catalyst participates, and the catalyst comprises a palladium compound and a phosphorus compound capable of forming a ligand structure with palladium.

[0078] Among them, the palladium compound is preferably selected from any one or more of palladium chloride, palladium acetate, and dicyanobenzene palladium chloride, more preferably palladium acetate, and most preferably palladium acetate with a concentration of 0.3-0.5%; the phosphorus compound is preferably selected from any one or more of tri-tert-butylphosphine, tri(2-furyl)phosphine, and tri-o-tolylphosphine, more preferably tri-tert-butylphosphine.

[0079] In the present invention, the palladium acetate contains only carbon, hydrogen, oxygen and palladium elements, and no new groups are introduced. The ligand structure formed between the tri-tert-butylphosphine and palladium acetate is more stable.

[0080] Furthermore, since tri-tert-butyl phosphine is easily oxidized by air and absorbs water, when adding tri-tert-butyl phosphine, in order to avoid the influence of tert-butyl phosphine being oxidized by air and absorbing water on the reaction, it is preferably added under anhydrous and oxygen-free conditions.

[0081] According to the present invention, the reaction is carried out under alkaline conditions, and the base providing the alkaline conditions is not limited to any organic base or inorganic base, preferably an organic base, such as potassium tert-butoxide, potassium hydroxide, sodium hydroxide, sodium tert-butoxide, potassium carbonate, and more preferably potassium tert-butoxide, which has extremely strong alkalinity.

[0082] In the present invention, the potassium tert-butoxide has three methyl groups, has very strong alkalinity and activity, and is very stable.

[0083] According to the present invention, the molar ratio of the spiroacridine compound, the phosphorus oxide compound, the phosphorus compound and the base is 1:(0.1-2):(0.01-1):(0.5-3), preferably 1:(0.8-1.2):(0.1-0.5):(0.7-1.3), more preferably 1:(1-1.1):(0.3-0.4):(0.9-1.2), for example 1:1:0.3:1.

[0084] According to the present invention, the reaction temperature is 80-200°C, preferably 120-150°C, more preferably 130-135°C; the reaction time is 5-20h, preferably 10-15h, more preferably 12-13h.

[0085] In the present invention, the reaction temperature and time have a great influence on the steric hindrance of the ternary thermally excited delayed fluorescent guest material containing spiroacridine triazine diphosphine oxide. The guest material prepared within the above reaction temperature and time range has the best steric hindrance and can effectively improve the triplet energy level of the spiroacridine triazine compound parent.

[0086] According to the present invention, the oxidant used in the oxidation process is preferably a peroxide, such as peracetic acid, hydrogen peroxide, sodium peroxide, and more preferably hydrogen peroxide.

[0087] The hydrogen peroxide reaction products are only water and oxygen, with high activity and no by-products.

[0088] According to the present invention, the solvent used for the purification is a mixed solvent of petroleum ether, dichloromethane and ethanol.

[0089] According to a third aspect of the present invention, there is provided an electroluminescent device prepared using a ternary thermally excited delayed fluorescent guest material containing a spiroacridine triazine bisphosphine oxide.

[0090] The electroluminescent device comprises a substrate layer, an anode, a hole injection layer, a hole transport layer, an exciton blocking layer, a light-emitting layer, a hole blocking layer, an electron transport layer, an electron injection layer and a cathode.

[0091] Furthermore, the method for preparing an electroluminescent device using a ternary thermally excited delayed fluorescent guest material containing a spiroacridine triazine bisphosphine oxide comprises:

[0092] 1. Prepare anode;

[0093] The anode is prepared on the substrate layer. The anode is selected from tin oxide conductive glass, transparent conductive polymers such as polyaniline, and semi-transparent metals such as gold, preferably tin oxide conductive glass or semi-transparent metals, and more preferably tin oxide conductive glass.

[0094] Wherein, the anode is evaporated by vacuum evaporation method.

[0095] In the present invention, the vacuum evaporation vacuum degree is 1×10 -7 ~1×10 -5 mbar, for example 1×10 -6 mbar, the evaporation rate is set to 0.1-0.3 nm / s, and an anodic indium tin oxide with a thickness of 1-100 nm is evaporated on a glass or plastic substrate. The thickness of the evaporated indium tin oxide is preferably 8-20 nm, more preferably 10-15 nm, such as 10 nm.

[0096] 2. preparing a hole injection layer;

[0097] The hole injection layer is evaporated on the anode, and the thickness of the evaporated layer is 2 to 20 nm, preferably 5 to 15 nm, more preferably 8 to 12 nm, such as 10 nm.

[0098] The hole injection layer material is selected from molybdenum oxide or poly (3,4-ethylenedioxythiophene): polystyrene sulfonate) (PEDOT:PSS), preferably molybdenum oxide, more preferably molybdenum oxide.

[0099] 3. Preparation of hole transport layer;

[0100] The hole transport layer is evaporated on the hole injection layer, and the evaporated thickness is 15 to 70 nm, preferably 25 to 55 nm, and more preferably 35 to 40 nm, such as 40 nm.

[0101] The hole transport layer material is selected from aromatic amine derivatives, such as N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine (NPB).

[0102] 4. preparing an exciton blocking layer;

[0103] The exciton blocking layer is evaporated on the hole transport layer, and the evaporated thickness is 5 to 35 nm, preferably 8 to 25 nm, more preferably 12 to 18 nm, such as 15 nm.

[0104] The exciton blocking layer material is selected from 9,9'-(1,3-phenyl)di-9H-carbazole (mCP) or bis[2-((oxy)diphenylphosphino)phenyl]ether (DPEPO), preferably 9,9'-(1,3-phenyl)di-9H-carbazole (mCP).

[0105] 5. preparing a light-emitting layer;

[0106] The light-emitting layer is evaporated on the exciton blocking layer, and the evaporated thickness is 5 to 80 nm, preferably 25 to 65 nm, more preferably 45 to 55 nm, such as 50 nm.

[0107] The light-emitting layer material is a mixture of a ternary thermally excited delayed fluorescent guest material containing spiroacridine triazine bisphosphine oxide and diphenyl ether bisphosphine oxide (DPEPO).

[0108] 6. preparing a hole blocking layer;

[0109] The hole blocking layer is evaporated on the light-emitting layer, and the evaporated thickness is 5 to 70 nm, preferably 25 to 55 nm, more preferably 35 to 45 nm, such as 40 nm.

[0110] The hole blocking layer material is diphenyl ether bisphosphine oxide (DPEPO).

[0111] 7. Preparing an electron transport layer;

[0112] The electron transport layer is evaporated on the hole blocking layer, and the evaporated thickness is 10 to 110 nm, preferably 45 to 95 nm, and more preferably 75 to 85 nm, such as 80 nm.

[0113] The electron transport layer material is selected from tris(8-hydroxyquinoline)aluminum (Alq3), 1,3,5-tris(1-phenyl-1H-benzimidazol-2-yl)benzene (TPBi), 4,7-diphenyl-1,10-phenanthroline (Bphen), 3-(biphenyl-4-yl)-5-(4-tert-butylphenyl)-4-phenyl-4H-1,2,4-triazole (TAZ), preferably Bphen.

[0114] 8. preparing an electron injection layer;

[0115] The electron injection layer is evaporated on the electron transport layer, and the evaporated thickness is 1 to 20 nm, preferably 5 to 15 nm, more preferably 8 to 12 nm, such as 10 nm.

[0116] The electron injection layer material is selected from lithium tetrakis(8-hydroxyquinoline)borate (LiBq4) or LiF, preferably LiF.

[0117] 9. Prepare the cathode, encapsulate it, and obtain a thermally excited delayed fluorescence electroluminescent deep blue light device.

[0118] The cathode is evaporated on the electron injection layer, and the evaporated thickness is 1 to 100 nm, preferably 8 to 30 nm, more preferably 10 to 15 nm, such as 10 nm.

[0119] The cathode material is selected from a single metal cathode or an alloy cathode, such as calcium, magnesium, silver, aluminum, a calcium alloy, a magnesium alloy, a silver alloy or an aluminum alloy.

[0120] According to a preferred embodiment, the hole injection layer, hole transport layer, exciton blocking layer, light-emitting layer, hole blocking layer, electron transport layer, electron injection layer and cathode are all prepared by vacuum evaporation.

[0121] In the present invention, the electroluminescent blue-green light device prepared from the ternary thermally excited delayed fluorescent guest material containing spiroacridine triazine bisphosphine oxide reduces the turn-on voltage to 2.9V, and has good thermodynamic stability, and the pyrolysis temperature reaches above 500°C. At the same time, the luminous efficiency and brightness of the organic electroluminescent material are improved, and an organic electroluminescent diode with excellent performance can be prepared.

[0122] Example

[0123] The present invention is further described below through specific examples, but these examples are merely exemplary and do not constitute any limitation to the scope of protection of the present invention.

[0124] Example 1

[0125] 1 mmol of p-bromotriphenyltriazine, 0.03 mmol of palladium acetate, 2.2 mmol of sodium acetate and 5 mL of N,N-dimethylformamide were added into a reaction flask, 2.2 mmol of diphenylphosphine was injected into the reaction flask under anhydrous and oxygen-free conditions, and the reaction was carried out at 130°C for 12 hours, followed by oxidation with 0.25 mL of hydrogen peroxide to obtain p-bromotriphenyltriazine diphosphine oxide.

[0126] Take 1mmol of the prepared p-bromotriphenyltriazine bisphosphine oxide and add it into a reaction bottle, and add 1mmol of spiracidine fluorene, 1mmol of potassium tert-butoxide, 0.005 of palladium acetate and 10mL of toluene thereto, and then inject 0.3mmol of tri-tert-butylphosphine into the reaction bottle under anhydrous and oxygen-free conditions, reflux at 110°C for 12h. After the reaction is completed, the resulting solution is extracted to obtain an organic layer, the organic layer is dried and concentrated, and then H2O2 is added for oxidation, and then extracted with dichloromethane, dried and concentrated, and purified by column chromatography with a mixed solvent of petroleum ether, dichloromethane and ethanol as the eluent to obtain a ternary thermally excited delayed fluorescent guest material containing spiracidine triazine bisphosphine oxide, which is SFATPTZDPO, and its structural formula is shown in compound (Ⅰ).

[0127] The obtained compound (I) was subjected to mass spectrometry test, and the time-of-flight mass spectrum data were: m / z (%): 1039 (100) [M + ].

[0128] The obtained compound (I) was subjected to elemental analysis, and the test data were: molecular formula C 70 H 48 N4O2P2, theoretical value: C80.91, H 4.66, N 5.39, O 3.08, P 5.96; measured value: C 80.83, H 4.70, N 5.37.

[0129] The obtained compound (I) was characterized by hydrogen nuclear magnetic resonance spectroscopy. 1 HNMR (TMS, CDCl3, 400MHz), the data obtained are: δ = 7.729-7.691 (t, J = 7.6 Hz, 2H); 7.608-7.571 (t, J = 7.4 Hz; 1H); 7.455-7.419 (m, 4H); 7.395-7.344 (m, 4H); 7.304-7.259 (m, 3H); 7.239-7.206 (m, 1H); 7.189-7.140 (m, 2H); 7.105-7.082 (dd, J1=1.2Hz; J2=1.6Hz, 2H); 7055-7.033 (dd, J1= 0.8Hz, J2=0.8Hz, 2H); 7.013-6.892 (m, 5H); 6.772-6.732 (m, 1H); 6.356-6.317ppm (m, 2H).

[0130] The obtained compound (I) was tested by UV spectrum and fluorescence spectrum. The test spectrum is as follows: Figure 1 shown.

[0131] The obtained compound (I) was subjected to thermogravimetric analysis, and the test data were as follows: Figure 2 As shown, it can be seen that the pyrolysis temperature of compound (I) is 522°C.

[0132] The obtained compound (I) is used as the main material of the light-emitting layer and the hole blocking layer material to prepare an electroluminescent deep blue light device, and the method is as follows:

[0133] 1. Place the glass or plastic substrate washed with deionized water into a vacuum evaporator for evaporation at a vacuum degree of 1×10 -6 mbar, the evaporation rate was set to 0.1 nm / s, the evaporation material was indium tin oxide (ITO), and the anode thickness was 10 nm;

[0134] 2. Evaporating the hole injection layer material MoOx on the anode to obtain a hole injection layer with a thickness of 6 nm;

[0135] 3. Evaporating the hole transport layer material NPB on the hole injection layer to obtain a hole transport layer with a thickness of 50 nm;

[0136] 4. Vapor depositing a blocking layer material mCP on the hole transport layer to obtain an exciton blocking layer with a thickness of 5 nm;

[0137] 5. Evaporating a light-emitting layer material on the exciton blocking layer: the light-emitting layer material is a mixture of compound (I) and diphenyl ether bisphosphine oxide (DPEPO), wherein the mass fraction of compound (I) is 20%, and a light-emitting layer with a thickness of 50 nm is obtained;

[0138] 6. Continue to evaporate DPEPO on the light-emitting layer to obtain a hole blocking layer with a thickness of 5 nm;

[0139] 7. Evaporating the electron transport layer material Bphen on the hole blocking layer to form an electron transport layer with a thickness of 55 nm;

[0140] 8. Vapor depositing electron injection layer material LiF on the electron transport layer to form an electron injection layer with a thickness of 1 nm;

[0141] 9. A cathode with aluminum as the material and a thickness of 100 nm is evaporated on the electron injection layer to obtain an electro-induced deep blue light device.

[0142] The structure of the prepared electro-deep blue light device is: ITO / MoOx (10nm) / NPB (40nm) / mCP (15nm) / DPEPO: (Ⅰ) (20%) 50nm / DPEPO (40nm) / Bphen (80nm) / LiF (10nm) / Al.

[0143] The voltage-current density relationship curve of the prepared electro-deep blue light device is as follows: Fig. 9 As shown, it can be seen that SFATPTZDPO material has semiconductor properties and its threshold voltage is 4.6V.

[0144] The voltage-brightness curve of the prepared electro-induced deep blue light device is as follows: Fig.10 As shown, it can be seen that the turn-on voltage of the device is 4.8V.

[0145] The brightness-current efficiency curve of the prepared electro-deep blue light device is as follows: Fig.11 As shown in the figure, it can be seen that the device has a brightness of 9.5cd·m -2 When the current efficiency reaches the maximum value of 30.2cd·A -1 .

[0146] The brightness-power efficiency curve of the prepared electro-deep blue light device is as follows: Fig.12 As shown in the figure, it can be seen that the device has a brightness of 11.2cd·m -2 When the power efficiency reaches the maximum value of 38.5lm·W -1 .

[0147] The relationship between the brightness and external quantum efficiency of the electro-deep blue light device is shown in Fig.13 As shown in the figure, it can be seen that the device has a brightness of 34.1 mA cm -2 When , the maximum external quantum efficiency of 38.1% was obtained.

[0148] The electroluminescence spectrum of the prepared electroluminescent blue phosphorescent device is shown in Fig.14 As shown, it can be seen that the electroluminescence peak of the device is at 492nm.

[0149] Example 2

[0150] A ternary thermally excited delayed fluorescent guest material containing spiroacridinium triazine bisphosphine oxide was prepared in a manner similar to Example 1, except that 1 mmol of spiroacridinium oxygen anthracene was added and the prepared guest material was SXATPTZDPO, whose structural formula is shown in compound (II).

[0151] The obtained compound (II) was subjected to mass spectrometry test, and the time-of-flight mass spectrum data were: m / z (%): 1055 (100) [M + ];

[0152] The obtained compound (II) was subjected to elemental analysis, and the test data were: molecular formula C 70 H 48 N4O3P2, theoretical value: C 79.68, H 4.59, N 5.31, O 4.55, P 5.87; measured value: C 79.20, H 4.55, N 5.35.

[0153] The obtained compound (II) was characterized by hydrogen nuclear magnetic resonance spectroscopy. 1H-NMR (TMS,CDCl3,400MHz), the data obtained are:δ=9.067-9.046(d,J=8.4Hz,2H);8.866-8.870(dd,J1=2.4Hz,J2=2.0Hz4H);7.960-7.911(dd,J1=8.0Hz,J2=8.4Hz,4H);7.763-7.712(m,2H);7.764-7.716(m,8H);7. 684-7.663 (d, J=8.4Hz, 2H); 7.615-7.574 (m, 4H); 7.532-7.488 (m, 8H); 7.214-7.160 (m, 6H); 6.969- 6.956 (m, 2H); 6.911-6.875 (m, 4H); 6.728-6.691 (q, J=7.4Hz, 2H); 6.366-6.346ppm (d, J=8.0Hz, 2H).

[0154] The obtained compound (II) was tested by UV spectrum and fluorescence spectrum. The test spectrum is as follows: Figure 3 shown.

[0155] The obtained compound (II) was subjected to thermogravimetric analysis, and the test data were as follows: Figure 4 As shown, it can be seen that the pyrolysis temperature of compound (II) is 518°C.

[0156] An electroluminescent deep blue light emitting device was prepared in a manner similar to Example 1, except that a mixture of diphenyl ether bisphosphine oxide (DPEPO) and compound (II) (wherein the mass fraction of compound (II) was 20%) was used as the light emitting layer material, and DPEPO was used as the hole blocking layer material.

[0157] The structure of the prepared electro-deep blue light device is: ITO / MoOx (10nm) / NPB (40nm) / mCP (15nm) / DPEPO: (Ⅱ) (20%) 50nm / DPEPO (40nm) / Bphen (80nm) / LiF (10nm) / Al.

[0158] The voltage-current density relationship curve of the prepared electro-deep blue light device is as follows: Fig.15 As shown, it can be seen that the SXATPTZDPO material has semiconductor characteristics and its threshold voltage is 5.8V.

[0159] The voltage-brightness curve of the prepared electro-induced deep blue light device is as follows: Fig.16 As shown, it can be seen that the turn-on voltage of the device is 5.2V.

[0160] The brightness-current efficiency curve of the prepared electro-deep blue light device is as follows: Fig.17 As shown in the figure, it can be seen that the device has a brightness of 27.6cd·m-2 When the current efficiency reaches the maximum value of 32.8cd·A -1 .

[0161] The brightness-power efficiency relationship curve of the prepared electro-deep blue light device is as follows: Fig.18 As shown in the figure, it can be seen that the device has a brightness of 13.5cd·m -2 When the power efficiency reaches the maximum value of 36.5lm·W -1 .

[0162] The relationship between the brightness and external quantum efficiency of the electro-deep blue light device is shown in Fig.19 As shown in the figure, it can be seen that the device has a brightness of 57.3mA·cm -2 When , the maximum external quantum efficiency of 39.2% is obtained.

[0163] The electroluminescence spectrum of the prepared electroluminescent blue phosphorescent device is shown in Fig. 20 As shown, it can be seen that the electroluminescence peak of the device is at 496nm.

[0164] Example 3

[0165] A ternary thermally excited delayed fluorescent guest material containing spiroacridine triazine bisphosphine oxide was prepared in a manner similar to Example 1, except that 1 mmol of spiroacridine thioanthene was added. The guest material obtained was STATPTZDPO, and its structural formula was shown in compound (III).

[0166] The obtained compound (III) was subjected to mass spectrometry test, and the time-of-flight mass spectrum data were: m / z (%): 1071 (100) [M + ];

[0167] The obtained compound (III) was subjected to elemental analysis, and the test data were: molecular formula C 70 H 48 N4O2P2S, theoretical value: C 78.49, H 4.52, N 5.23, O 2.99, P 5.78, S 2.99; measured value: C 78.62, H 4.51, N 5.82.

[0168] The obtained compound (III) was tested by UV spectrum and fluorescence spectrum. The test spectrum is as follows: Figure 5 shown.

[0169] The obtained compound (III) was subjected to thermogravimetric analysis, and the test data were as follows: Figure 6 As shown, it can be seen that the pyrolysis temperature of compound (III) is 527°C.

[0170] An electroluminescent deep blue light emitting device was prepared in a manner similar to Example 1, except that a mixture of diphenyl ether bisphosphine oxide (DPEPO) and compound (III) (wherein the mass fraction of compound (III) is 20%) was used as the light emitting layer material, and DPEPO was used as the hole blocking layer material.

[0171] The structure of the prepared electro-deep blue light device is: ITO / MoOx (10nm) / NPB (40nm) / mCP (15nm) / DPEPO: (III) (20%) 50nm / DPEPO (40nm) / Bphen (80nm) / LiF (10nm) / Al.

[0172] The voltage-current density relationship curve of the prepared electro-deep blue light device is as follows: Fig.21 As shown, it can be seen that STATPTZDPO material has semiconductor properties and its threshold voltage is 5.9V.

[0173] The voltage-brightness curve of the prepared electro-induced deep blue light device is as follows: Fig. 22 As shown, it can be seen that the turn-on voltage of the device is 5.5V.

[0174] The brightness-current efficiency curve of the prepared electro-deep blue light device is as follows: Fig.23 As shown in the figure, it can be seen that the device has a brightness of 17.2cd·m -2 When the current efficiency reaches the maximum value of 28.9cd·A -1 .

[0175] The brightness-power efficiency relationship curve of the prepared electro-deep blue light device is as follows: Fig.24 As shown in the figure, it can be seen that the device has a brightness of 29.6cd·m -2 When the power efficiency reaches the maximum value of 38.2lm·W -1 .

[0176] The relationship between the brightness and external quantum efficiency of the electro-deep blue light device is shown in Fig.25 As shown in the figure, it can be seen that the device has a brightness of 28.9 mA cm -2 The maximum external quantum efficiency of 39.0% was obtained.

[0177] The electroluminescence spectrum of the prepared electroluminescent blue phosphorescent device is shown in Fig.26 As shown, it can be seen that the electroluminescence peak of the device is at 500nm.

[0178] Example 4

[0179] A ternary thermally excited delayed fluorescent guest material containing spiroacridine triazine bisphosphine oxide was prepared in a manner similar to Example 1, except that 1 mmol of spiroacridine sulfone anthracene was added, and the guest material obtained was compound STOATPTZDPO, whose structural formula is shown in compound (IV).

[0180] The obtained compound (IV) was subjected to mass spectrometry test, and the time-of-flight mass spectrum data were: m / z (%): 1103 (100) [M + ];

[0181] The obtained compound (Ⅳ) was subjected to elemental analysis, and the test data was: molecular formula C 70 H 48 N4O4P2S, theoretical value: C76.21, H 4.39, N 5.08, O 5.80, P 5.62, S 2.91; measured value: C 76.68, H 4.40, N 5.05.

[0182] The obtained compound (IV) was tested by UV spectrum and fluorescence spectrum. The test spectrum is as follows: Figure 7 shown.

[0183] The obtained compound (IV) was subjected to thermogravimetric analysis, and the test data were as follows: Figure 8 As shown, it can be seen that the pyrolysis temperature of compound (IV) is 519°C.

[0184] An electroluminescent deep blue light emitting device was prepared in a manner similar to Example 1, except that a mixture of diphenyl ether bisphosphine oxide (DPEPO) and compound (IV) (wherein the mass fraction of compound (IV) is 20%) was used as the light emitting layer material, and DPEPO was used as the hole blocking layer material.

[0185] The structure of the prepared electro-deep blue light device is: ITO / MoOx (10nm) / NPB (40nm) / mCP (15nm) / DPEPO: (IV) (20%) 50nm / DPEPO (40nm) / Bphen (80nm) / LiF (10nm) / Al.

[0186] The voltage-current density relationship curve of the prepared electro-deep blue light device is as follows: Fig. 27 As shown by Fig. 27 It can be seen that STOATPTZDPO material has semiconductor properties and its threshold voltage is 2.9V.

[0187] The voltage-brightness curve of the prepared electro-induced deep blue light device is as follows: Fig.28 As shown by Fig.28 It can be seen that the turn-on voltage of the device is 4.1V.

[0188] The brightness-current efficiency curve of the prepared electro-deep blue light device is as follows: Fig.29 As shown by Fig.29 It can be seen that the device has a brightness of 3.2cd·m -2 When the current efficiency reaches the maximum value of 32.7cd·A -1 .

[0189] The brightness-power efficiency curve of the prepared electro-deep blue light device is as follows: Fig.30 As shown by Fig.30 It can be seen that the device has a brightness of 2.0 cd·m -2 When the power efficiency reaches the maximum value of 53.8lm·W -1 .

[0190] The relationship between the brightness and external quantum efficiency of the electro-deep blue light device is shown in Fig.31 As shown by Fig.31 It can be seen that the device has a brightness of 112.1 mA cm -2 When , the maximum external quantum efficiency of 39.1% was obtained.

[0191] The electroluminescence spectrum of the prepared deep blue light device is shown in Fig.32 As shown by Fig.32 It can be seen that the electroluminescence peak of the device is at 462nm.

[0192] The present invention has been described in detail above in conjunction with preferred embodiments and exemplary examples. However, it should be noted that these specific embodiments are only illustrative explanations of the present invention and do not constitute any limitation on the protection scope of the present invention. Without exceeding the spirit and protection scope of the present invention, various improvements, equivalent substitutions or modifications may be made to the technical content of the present invention and its embodiments, all of which fall within the protection scope of the present invention. The protection scope of the present invention shall be subject to the attached claims.

Claims

1. A ternary thermally excited delayed fluorescent guest material containing a spiroacridine triazine bisphosphine oxide, characterized in that: The guest material has a spiroacridine triazine group as a parent and an aromatic phosphine group as a second receptor. The guest material is selected from compounds having the following structural formula:

2. An electroluminescent device prepared using the ternary thermally excited delayed fluorescent guest material containing spiroacridine triazine bisphosphine oxide according to claim 1, characterized in that: The electroluminescent device comprises a substrate layer, an anode, a hole injection layer, a hole transport layer, an exciton blocking layer, a light emitting layer, a hole blocking layer, an electron transport layer, an electron injection layer and a cathode.