A kind of ethylene-vinyl alcohol copolymer and its preparation method and application

By using alkaline deep eutectic solvent as catalyst and solvent, the problems of metal ions residues and three waste emissions in ethylene-vinyl alcohol copolymers are solved, and efficient and environmentally friendly preparation of alcoholylated EVA is achieved, and high alcoholylated EVOH products are obtained. , suitable for industrial applications.

CN115433295BActive Publication Date: 2024-12-06DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211251317.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-12
Publication Date
2024-12-06
Estimated Expiration
2042-10-12

AI Technical Summary

Technical Problem

In the existing preparation method of ethylene-vinyl alcohol copolymer, metal ions are introduced by the alkali catalyst, resulting in residual metal ions in the product, increasing ash and generating a large amount of three wastes, limiting industrial applications.

Method used

The alkaline deep eutectic solvent is used as the catalyst and solvent for the alcoholylation reaction, and the eutectic mixture formed by combining hydrogen bond donor and hydrogen bond acceptor is achieved to prepare EVOH by alcoholylation, avoiding the residual metal ions, and passing through multiple times Recycling reduces waste emissions.

Benefits of technology

EVOH products with alcohol resolution of more than 99% have been achieved, which reduces separation costs and waste emissions. The deep eutectic solvent is low in toxicity and easy to recycle, making it suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115433295B_ABST
    Figure CN115433295B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing an ethylene-vinyl alcohol copolymer: an ethylene-vinyl acetate copolymer, a solvent and a catalyst are mixed and reacted, and an ethylene-vinyl alcohol copolymer is prepared through post-treatment; the catalyst is an alkaline deep eutectic solvent. The alkaline deep eutectic solvent of the present invention does not contain metal ions. As a catalyst in the method for preparing EVOH by catalytic alcoholysis of EVA, it effectively avoids the influence of metal ion residues on EVOH products, reduces the metal removal and purification steps in subsequent treatment, and reduces the separation cost; and the alkaline deep eutectic solvent of the present invention can be recycled for multiple times, reducing the discharge of three wastes. In addition, the present invention adopts an alkaline deep eutectic solvent as a catalyst, and provides a method for preparing EVOH by alcoholysis of EVA with low cost, low toxicity, high efficiency and no introduction of metal ions, and the alcoholysis degree of the EVOH product can reach more than 99%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material preparation, and specifically relates to an ethylene-vinyl alcohol copolymer and a preparation method and application thereof. Background Art

[0002] EVOH is a random copolymer of ethylene-vinyl alcohol, a crystalline polymer with a chain molecular structure, which is composed of 20-50% ethylene and 50-80% vinyl alcohol by mole fraction. EVOH has both the barrier properties of polyvinyl alcohol (PVA) and the processing properties of polyethylene (PE), and is known as the three major barrier resins together with polyvinylidene chloride (PVDC) and polyamide (PA). EVOH has many advantages such as gas barrier properties, oil resistance, chemical corrosion resistance, weather resistance, processability, excellent transparency, non-toxic and tasteless, and complies with the European Community Food Packaging Guidelines and the US Food and Drug Administration (FDA) requirements. It is widely used in packaging materials, structural materials, textile materials, medical materials and other fields.

[0003] Since vinyl alcohol cannot stably exist in the form of monomers under normal conditions, the preparation of ethylene-vinyl alcohol copolymer is mainly achieved by the alcoholysis and saponification reaction of ethylene-vinyl acetate copolymer. Bayer AG of Germany first reported in the 1960s in patent US3325460A that C1-C4 alcohol was used as solvent, and ethylene and vinyl acetate were used as raw materials to prepare (ethylene-vinyl acetate copolymer) EVA copolymer under high pressure and specific reaction temperature by solution polymerization. This method was later widely used to prepare the precursor EVA copolymer of EVOH copolymer. Kuraray Co., Ltd. of Japan and Sinopec Group reported in patents US4485225 and CN102942649A that an alcohol solution of EVA was first obtained by this method, and then EVOH copolymer was obtained by alcoholysis and saponification.

[0004] In the entire preparation process of EVOH, the alcoholysis of EVA to prepare EVOH is a key step. The alcoholysis degree of EVOH determines its gas barrier properties. Generally, the alcoholysis degree of EVOH should reach more than 95%. Usually, the catalyst used for alcoholysis is a large amount of strong alkali such as sodium hydroxide and potassium hydroxide that cannot be recovered, which is carried out in an alcohol solvent. In this way, residual metal ions such as sodium and potassium are inevitably introduced into the EVOH product, increasing the ash content in the EVOH product. For this reason, the EVOH resin solution after alcoholysis needs to be neutralized and washed with a large amount of water, and a large amount of three wastes is generated.

[0005] CN109651557A discloses a method for preparing an ethylene-vinyl alcohol copolymer. The invention uses alkaline catalysts such as sodium hydroxide, potassium hydroxide, sodium methoxide, sodium ethoxide and potassium methoxide to hydrolyze EVA in an alcohol solvent to prepare EVOH. However, the use of alkaline catalysts will inevitably introduce metal ions. In addition, a large amount of three wastes will be generated during the neutralization and large-scale water washing process of the EVOH resin solution after the alcoholysis.

[0006] CN113861313A and CN113736004A respectively report a method for preparing an ethylene-vinyl alcohol copolymer, wherein alkaline ionic liquids such as 1,8-diazabicyclo[5,4,0]undec-7-ene imidazole salt and acidic ionic liquids such as 1-octyl-3-methylimidazolium hydrogen sulfate are used as catalysts to prepare EVOH by alcoholysis of EVA in an alcohol solvent, and such methods successfully solve the problem that traditional catalysts introduce metal ions. However, most ionic liquids still have some defects, such as high price (the price of imidazole ionic liquids is about 783-26 120US$ / kg), toxicity, corrosiveness, etc., thus limiting the large-scale industrial application of ionic liquids.

[0007] Therefore, researchers in this field hope to develop a method for preparing EVOH by alcoholysis of EVA which is low-cost, low-toxic, efficient and does not introduce metal ions. Summary of the invention

[0008] In order to overcome the above problems, the present invention provides an ethylene-vinyl alcohol copolymer and a preparation method and application thereof. The present invention uses an alkaline deep eutectic solvent as a catalyst and solvent for alcoholysis reaction, which can be used to prepare EVOH by alcoholysis of EVA in a simple, efficient and environmentally friendly manner, and the alcoholysis degree of the obtained EVOH product can reach more than 99%.

[0009] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:

[0010] In a first aspect, the present invention provides a method for preparing an ethylene-vinyl alcohol copolymer, the preparation method comprising:

[0011] The ethylene-vinyl acetate copolymer, the solvent and the catalyst are mixed and reacted, and then post-treated to obtain the ethylene-vinyl alcohol copolymer;

[0012] The catalyst is a basic deep eutectic solvent.

[0013] A deep eutectic solvent is a two-component or three-component eutectic mixture composed of a certain stoichiometric ratio of hydrogen bond donors (polyols, urea and carboxylic acids) and hydrogen bond acceptors (ammonium salts, such as choline chloride, etc.). It has the characteristics of low melting point, non-volatility, non-flammability, good solubility, easy synthesis, low cost, low toxicity, low corrosiveness, good biodegradability, etc., and can be used as a solvent or catalyst. The alkaline deep eutectic solvent described in the present invention is a non-metallic deep eutectic solvent, does not contain metal ions, avoids the influence of residual metal ions on EVOH products, reduces the steps of metal removal and purification in subsequent treatment, and greatly reduces the separation cost. The EVOH after alcoholysis can be filtered by adding water to precipitate to obtain the EVOH product, and the filtrate can be dried in high temperature vacuum to recover the deep eutectic solvent. In addition, the alkaline deep eutectic solvent in the present invention can be recycled many times, greatly reducing the discharge of three wastes, and is called a "green solvent".

[0014] Preferably, the reaction is an alcoholysis reaction.

[0015] Preferably, the temperature of the alcoholysis reaction is 20-90°C, such as 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 85°C, 90°C, etc., preferably 50-80°C.

[0016] Preferably, the alcoholysis reaction time is 0.5-24 h, for example, 0.5 h, 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h, 11 h, 13 h, 15 h, 17 h, 19 h, 21 h, 23 h or 24 h, etc., preferably 1-15 h.

[0017] Preferably, the post-treatment comprises precipitation, filtration and vacuum drying.

[0018] Preferably, the alkaline deep eutectic solvent includes: 1,5-diazabicyclo[4.3.0]-5-nonene-triethanolamine deep eutectic solvent (DBN-TEOA), 1,5-diazabicyclo[4.3.0]-5-nonene-benzyl alcohol deep eutectic solvent (DBN-BA), 1,8-diazabicycloundec-7-ene-triethanolamine deep eutectic solvent (DBU-TEOA), 1,8-diazabicycloundec-7-ene-benzyl alcohol deep eutectic solvent (DBU-BA), 1,1,3,3-tetramethylguanidine-triethanolamine deep eutectic solvent (TMG-TEOA), 1,1,3,3-tetramethylguanidine-benzyl alcohol deep eutectic solvent (TMG-BA), etc. When two or more alkaline deep eutectic solvents are used, the two or more alkaline deep eutectic solvents can be mixed in any proportion.

[0019] In the present invention, the alkaline deep eutectic solvent can be used as both a catalyst and a solvent. The alkaline deep eutectic solvent described in the present invention does not contain metal ions, thereby avoiding the influence of residual metal ions on EVOH products, thereby reducing subsequent metal removal and purification steps, and greatly reducing separation costs. After the alcoholysis reaction is completed, EVOH can be filtered out by adding water for precipitation, and the filtrate can be recycled by high-temperature vacuum drying. Therefore, the choline chloride-toluenesulfonic acid type deep eutectic solvent in the present invention can be recycled multiple times, thereby reducing the discharge of three wastes.

[0020] Preferably, the basic deep eutectic solvent is prepared by the following method: mixing a hydrogen bond donor and a hydrogen bond acceptor, reacting them, and obtaining the basic deep eutectic solvent;

[0021] The hydrogen bond donor is triethanolamine (TEOA) or benzyl alcohol (BA), and the hydrogen bond acceptor is 1,5-diazabicyclo[4.3.0]-5-nonene (DBN), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU) or 1,1,3,3-tetramethylguanidine (TMG).

[0022] Preferably, the molar ratio of the hydrogen bond donor to the hydrogen bond acceptor is 1:1.

[0023] Preferably, the reaction temperature is 60-120°C, for example 60°C, 70°C, 80°C, 90°C, 100°C, 110°C or 120°C, and the reaction time is 1-8h, for example 1h, 2h, 3h, 4h, 5h, 6h, 7h or 8h.

[0024] As a preferred technical solution of the present invention, the alkaline deep eutectic solvent is prepared by the following method: a hydrogen bond donor (TEOA or BA) and a hydrogen bond acceptor (DBN, DBU or TMG) ​​are uniformly mixed in a molar ratio of 1:1, and reacted at 60-120°C for 1-8h to obtain the alkaline deep eutectic solvent.

[0025] Preferably, based on the added amount of the ethylene-vinyl acetate copolymer as 1g, the added amount of the catalyst is 0.1-10g, for example, 0.2g, 0.5g, 1g, 2g, 3g, 4g, 5g, 6g, 7g, 8g, 9g or 9.5g, etc., preferably 0.2-8g, more preferably 0.2-5g.

[0026] Preferably, the solvent comprises an alcohol solvent, preferably a C1-C4 alcohol solvent, and further preferably any one of methanol, ethanol, tert-butanol, n-butanol or isopropanol, or a combination of at least two thereof.

[0027] In the present invention, the C1-C4 alcohol solvent refers to an alcohol solvent containing 1-4 carbon atoms, such as methanol, ethanol, propanol or butanol.

[0028] Preferably, based on 1 g of the ethylene-vinyl acetate copolymer, the amount of the solvent added is 5-50 mL, for example, 5 mL, 10 mL, 15 mL, 20 mL, 25 mL, 30 mL, 35 mL, 40 mL, 45 mL or 50 mL, etc., preferably 10-30 mL.

[0029] Preferably, the molar content of ethylene units in the ethylene-vinyl acetate copolymer is 5%-90%, for example 5%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80% or 90%, etc., preferably 10%-60%, more preferably 20%-50%.

[0030] Preferably, the weight average molecular weight of the ethylene-vinyl acetate copolymer is 1000-500000, for example, 2000, 5000, 10000, 50000, 100000, 200000, 300000, 400000 or 500000, preferably 5000-400000, more preferably 20000-300000.

[0031] Preferably, the ethylene-vinyl acetate copolymer includes ethylene-vinyl acetate copolymer obtained by solution polymerization, emulsion polymerization or bulk polymerization.

[0032] As a preferred technical solution of the present invention, the preparation method comprises:

[0033] Ethylene-vinyl acetate copolymer, alcohol solvent and alkaline deep eutectic solvent are mixed, and alcoholysis reaction is carried out at 50-80° C. for 1-15 hours to prepare ethylene-vinyl alcohol copolymer solution, and then water is added for precipitation, filtered and vacuum dried to obtain the ethylene-vinyl alcohol copolymer.

[0034] In a second aspect, the present invention provides an ethylene-vinyl alcohol copolymer, wherein the ethylene-vinyl alcohol copolymer is prepared by the preparation method as described in the first aspect.

[0035] Preferably, the alcoholysis degree of the ethylene-vinyl alcohol copolymer is ≥99%.

[0036] In a third aspect, the present invention provides a use of the ethylene-vinyl alcohol copolymer as described in the second aspect in packaging materials, structural materials, textile materials or medical materials.

[0037] The beneficial effects of the present invention are:

[0038] The alkaline deep eutectic solvent of the present invention does not contain metal ions. It is used as a catalyst in the method for preparing EVOH by alcoholysis of EVA, avoiding the influence of metal ion residues on EVOH products, reducing the metal removal and purification steps in subsequent treatments, and greatly reducing the separation cost. In addition, the alkaline deep eutectic solvent of the present invention can be recycled for multiple times, reducing the discharge of three wastes. Compared with ionic liquids, deep eutectic solvents have the advantages of being non-volatile, low-toxic and degradable, low-priced, easy to prepare, and recyclable. In addition, the present invention uses an alkaline deep eutectic solvent as a catalyst, which can prepare EVOH by alcoholysis of EVA with low cost, low toxicity, simplicity, high efficiency, and environmental protection, and the alcoholysis degree of the obtained EVOH product can reach more than 99% (99.39-99.86%). BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 This is the Fourier transform infrared spectrum of the 1,5-diazabicyclo[4.3.0]-5-nonene-benzyl alcohol deep eutectic solvent (DBN-BA) prepared in Example 1.

[0040] Figure 2 This is the Fourier transform infrared spectrum of the 1,5-diazabicyclo[4.3.0]-5-nonene-triethanolamine deep eutectic solvent (DBN-TEOA) prepared in Example 2.

[0041] Figure 3 This is the Fourier transform infrared spectrum of the 1,8-diazabicycloundec-7-ene-benzyl alcohol deep eutectic solvent (DBU-BA) prepared in Example 3.

[0042] Figure 4 This is the Fourier transform infrared spectrum of the 1,8-diazabicycloundec-7-ene-triethanolamine deep eutectic solvent (DBU-TEOA) prepared in Example 4.

[0043] Figure 5 This is the Fourier transform infrared spectrum of the 1,1,3,3-tetramethylguanidine-benzyl alcohol deep eutectic solvent (TMG-BA) prepared in Example 5.

[0044] Figure 6 This is the Fourier transform infrared spectrum of the 1,1,3,3-tetramethylguanidine-triethanolamine deep eutectic solvent (TMG-TEOA) prepared in Example 6. DETAILED DESCRIPTION

[0045] The following non-limiting embodiments may enable a person of ordinary skill in the art to more fully understand the present invention, but do not limit the present invention in any way. Any person familiar with the present technical field may make equivalent replacements or changes according to the technical solution and inventive concept of the present invention within the technical scope disclosed by the present invention, which shall fall within the protection scope of the present invention.

[0046] Example 1

[0047] In this embodiment, a preparation method of an ethylene-vinyl alcohol copolymer is provided, the preparation method comprising: placing 1 g of ethylene-vinyl acetate copolymer, 30 mL of methanol and 0.18 g of 1,5-diazabicyclo[4.3.0]-5-nonene-benzyl alcohol deep eutectic solvent (DBN-BA) in a 100 mL two-necked flask, stirring and heating to 70° C., reacting for 10 hours and then terminating the reaction to obtain an ethylene-vinyl alcohol copolymer solution, adding water to precipitate, washing, filtering and vacuum drying to obtain the ethylene-vinyl alcohol copolymer.

[0048] The molar content of ethylene units in the ethylene-vinyl acetate copolymer is 38%, and the weight average molecular weight of the ethylene-vinyl acetate copolymer is 130,000.

[0049] 1,5-diazabicyclo[4.3.0]-5-nonene-benzyl alcohol deep eutectic solvent (DBN-BA) is prepared by the following method: 1,5-diazabicyclo[4.3.0]-5-nonene and benzyl alcohol are uniformly mixed in a molar ratio of 1:1, and reacted at 80°C for 2h to obtain the 1,5-diazabicyclo[4.3.0]-5-nonene-benzyl alcohol deep eutectic solvent (DBN-BA), whose structural formula is shown in Formula I and whose Fourier transform infrared spectrum is shown in Figure 1 As shown in the figure, it can be seen that the above reaction obtains the target product DBN-BA.

[0050]

[0051] Example 2

[0052] The only difference between this embodiment and Example 1 is that the alkaline deep eutectic solvent used is 1,5-diazabicyclo[4.3.0]-5-nonene-triethanolamine deep eutectic solvent (DBN-TEOA), and the amount of deep eutectic solvent added is 0.22 g. Other conditions are the same as in Example 1.

[0053] 1,5-diazabicyclo[4.3.0]-5-nonene-triethanolamine deep eutectic solvent (DBN-TEOA) is prepared by the following method: 1,5-diazabicyclo[4.3.0]-5-nonene and triethanolamine are uniformly mixed in a molar ratio of 1:1, and reacted at 80°C for 2h to obtain the 1,5-diazabicyclo[4.3.0]-5-nonene-triethanolamine deep eutectic solvent (DBN-TEOA), whose structural formula is shown in Formula II and whose Fourier transform infrared spectrum is shown in Figure 2 As shown in the figure, it can be seen that the above reaction obtains the target product DBN-TEOA.

[0054]

[0055] Example 3

[0056] The only difference between this embodiment and Example 1 is that the alkaline deep eutectic solvent used is 1,8-diazabicycloundec-7-ene-benzyl alcohol deep eutectic solvent (DBU-BA), and the amount of deep eutectic solvent added is 0.21 g. Other conditions are the same as those in Example 1.

[0057] 1,8-diazabicycloundec-7-ene-benzyl alcohol deep eutectic solvent (DBU-BA) is prepared by the following method: 1,8-diazabicycloundec-7-ene and benzyl alcohol are uniformly mixed in a molar ratio of 1:1, and reacted at 80° C. for 2 hours to obtain the 1,8-diazabicycloundec-7-ene-benzyl alcohol deep eutectic solvent (DBU-BA), whose structural formula is shown in Formula III and whose Fourier transform infrared spectrum is shown in Figure 3 As shown in the figure, it can be seen that the above reaction obtains the target product DBN-BA.

[0058]

[0059] Example 4

[0060] The only difference between this embodiment and embodiment 1 is that the alkaline deep eutectic solvent used is 1,8-diazabicycloundec-7-ene-triethanolamine deep eutectic solvent (DBU-TEOA), and the amount of deep eutectic solvent added is 0.24 g. Other conditions are the same as those in embodiment 1.

[0061] 1,8-diazabicycloundec-7-ene-triethanolamine deep eutectic solvent (DBU-TEOA) is prepared by the following method: 1,8-diazabicycloundec-7-ene and triethanolamine are uniformly mixed in a molar ratio of 1:1, and reacted at 80° C. for 2 hours to obtain the 1,8-diazabicycloundec-7-ene-triethanolamine deep eutectic solvent (DBU-TEOA), whose structural formula is shown in Formula IV and whose Fourier transform infrared spectrum is shown in Figure 4 As shown in the figure, it can be seen that the above reaction obtains the target product DBU-TEOA.

[0062]

[0063] Example 5

[0064] The only difference between this embodiment and Example 1 is that the alkaline deep eutectic solvent used is 1,1,3,3-tetramethylguanidine-benzyl alcohol deep eutectic solvent (TMG-BA), and the amount of deep eutectic solvent added is 0.18 g. Other conditions are the same as those in Example 1.

[0065] 1,1,3,3-tetramethylguanidine-benzyl alcohol deep eutectic solvent (TMG-BA) is prepared by the following method: 1,1,3,3-tetramethylguanidine and benzyl alcohol are uniformly mixed in a molar ratio of 1:1, and reacted at 80° C. for 2 hours to obtain the 1,1,3,3-tetramethylguanidine-benzyl alcohol deep eutectic solvent (TMG-BA), whose structural formula is shown in Formula V and whose Fourier transform infrared spectrum is shown in Figure 5 As shown in the figure, it can be seen that the above reaction obtains the target product TMG-BA.

[0066]

[0067] Example 6

[0068] The only difference between this embodiment and Example 1 is that the alkaline deep eutectic solvent used is 1,1,3,3-tetramethylguanidine-triethanolamine deep eutectic solvent (TMG-TEOA), and the amount of deep eutectic solvent added is 0.21 g. Other conditions are the same as those in Example 1.

[0069] 1,1,3,3-tetramethylguanidine-triethanolamine deep eutectic solvent (TMG-TEOA) is prepared by the following method: 1,1,3,3-tetramethylguanidine and triethanolamine are uniformly mixed in a molar ratio of 1:1, and reacted at 80° C. for 2 hours to obtain the 1,1,3,3-tetramethylguanidine-triethanolamine deep eutectic solvent (TMG-TEOA), whose structural formula is shown in Formula VI and whose Fourier transform infrared spectrum is shown in Figure 6 As shown in the figure, it can be seen that the above reaction obtains the target product TMG-TEOA.

[0070]

[0071] Comparative Example 1

[0072] The difference between this comparative example and Example 1 is that DBN-BA is replaced with an equal amount of choline chloride-urea deep eutectic solvent (ChCl-2urea). The preparation method of ChCl-2urea is as follows: choline chloride and urea are uniformly mixed in a molar ratio of 1:2, reacted at 80°C for 2h, collected and used, and its structure is shown in Formula VII.

[0073]

[0074] Other conditions are the same as in Example 1.

[0075] Comparative Example 2

[0076] The difference between this comparative example and Example 1 is that DBN-BA is replaced by an equal amount of 1-hydroxyethyl-3-methylimidazolium chloride-urea deep eutectic solvent ([EMImOH]Cl-2urea). The preparation method of [EMImOH]Cl-2urea is as follows: 1-hydroxyethyl-3-methylimidazolium chloride and urea are uniformly mixed in a molar ratio of 1:2, reacted at 80°C for 2h, collected and used, and its structure is shown in Formula VIII.

[0077]

[0078] Other conditions are the same as in Example 1.

[0079] The alcoholysis degree of EVOH prepared in Examples 1-6 and Comparative Examples 1-2 was tested for performance, and the test characterization method was as follows: The alcoholysis degree of EVOH was characterized by FTIR-ATR (Nicolet TM iS50 FTIR spectrometer), scanning range 400-4000cm -1 , resolution 4cm, scan times 32 times. The calculation formula of alcoholysis degree is: alcoholysis degree = 1-A1 / 4.56A2, where A1 is 1730cm in the infrared spectrum. -1 The peak area at (corresponding to the C=O double bond stretching vibration peak in the ester group) is 3000-2800cm -1 The peak area at (corresponding to the CH stretching vibration peak).

[0080] The type and amount of the deep eutectic solvent used in the examples and comparative examples of the present invention, the amount of solvent used, the alcoholysis time, the temperature and the alcoholysis degree of the prepared EVOH are shown in Table 1.

[0081] Table 1

[0082]

[0083]

[0084] It can be seen from Table 1 that the alcoholysis degree of EVOH prepared in Examples 1-6 of the present invention can reach more than 99% (99.39%-99.86%).

[0085] Compared with Examples 1-6, the alcoholysis degree of EVOH prepared in Comparative Examples 1-2 was significantly reduced.

[0086] The applicant declares that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for a person skilled in the art to modify the technical solutions described in the aforementioned embodiments without departing from the principles of the present invention, or to make equivalent replacements for the raw materials used in the present invention, add auxiliary components, select specific methods, etc., all of which fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing an ethylene-vinyl alcohol copolymer, characterized in that: The preparation method comprises: The ethylene-vinyl acetate copolymer, the solvent and the catalyst are mixed and reacted, and then the mixture is post-treated to prepare the ethylene-vinyl alcohol copolymer; The catalyst is an alkaline deep eutectic solvent, and the alkaline deep eutectic solvent includes any one of 1,5-diazabicyclo[4.3.0]-5-nonene-triethanolamine deep eutectic solvent, 1,5-diazabicyclo[4.3.0]-5-nonene-benzyl alcohol deep eutectic solvent, 1,8-diazabicycloundec-7-ene-triethanolamine deep eutectic solvent, 1,8-diazabicycloundec-7-ene-benzyl alcohol deep eutectic solvent, 1,1,3,3-tetramethylguanidine-triethanolamine deep eutectic solvent, and 1,1,3,3-tetramethylguanidine-benzyl alcohol deep eutectic solvent, or a combination of at least two thereof.

2. The preparation method according to claim 1, characterized in that: The reaction is an alcoholysis reaction.

3. The preparation method according to claim 2, characterized in that: The temperature of the alcoholysis reaction is 20-90°C.

4. The preparation method according to claim 3, characterized in that: The temperature of the alcoholysis reaction is 50-80°C.

5. The preparation method according to claim 2, characterized in that: The alcoholysis reaction time is 0.5-24h.

6. The preparation method according to claim 5, characterized in that: The alcoholysis reaction time is 1-15h.

7. The preparation method according to claim 1, characterized in that: The post-treatment includes precipitation, filtration and vacuum drying.

8. The preparation method according to claim 1, characterized in that: Based on the addition amount of the ethylene-vinyl acetate copolymer being 1 g, the addition amount of the catalyst is 0.1-10 g.

9. The preparation method according to claim 8, characterized in that: Based on the addition amount of the ethylene-vinyl acetate copolymer being 1 g, the addition amount of the catalyst is 0.2-8 g.

10. The preparation method according to claim 9, characterized in that: Based on the addition amount of the ethylene-vinyl acetate copolymer being 1 g, the addition amount of the catalyst is 0.2-5 g.

11. The preparation method according to claim 1, characterized in that: The solvent includes an alcohol solvent.

12. The preparation method according to claim 11, characterized in that: The solvent includes a C1-C4 alcohol solvent.

13. The preparation method according to claim 12, characterized in that: The solvent includes any one of methanol, ethanol, tert-butanol, n-butanol or isopropanol, or a combination of at least two thereof.

14. The preparation method according to claim 1, characterized in that: Based on the addition amount of the ethylene-vinyl acetate copolymer being 1 g, the addition amount of the solvent is 5-50 mL.

15. The preparation method according to claim 14, characterized in that: Based on the addition amount of the ethylene-vinyl acetate copolymer being 1 g, the addition amount of the solvent is 10-30 mL.

16. The preparation method according to claim 1, characterized in that: The molar content of ethylene units in the ethylene-vinyl acetate copolymer is 5%-90%.

17. The preparation method according to claim 16, characterized in that: The molar content of ethylene units in the ethylene-vinyl acetate copolymer is 10%-60%.

18. The preparation method according to claim 17, characterized in that: The molar content of ethylene units in the ethylene-vinyl acetate copolymer is 20%-50%.

19. The preparation method according to claim 1, characterized in that: The weight average molecular weight of the ethylene-vinyl acetate copolymer is 1,000-500,000.

20. The preparation method according to claim 19, characterized in that: The weight average molecular weight of the ethylene-vinyl acetate copolymer is 5,000-400,000.

21. The preparation method according to claim 20, characterized in that: The weight average molecular weight of the ethylene-vinyl acetate copolymer is 20,000-300,000.

22. The preparation method according to claim 1, characterized in that: The ethylene-vinyl acetate copolymer includes an ethylene-vinyl acetate copolymer obtained by solution polymerization, emulsion polymerization or bulk polymerization.

23. The method for preparing ethylene-vinyl alcohol copolymer according to claim 1, characterized in that: The preparation method comprises: Ethylene-vinyl acetate copolymer, alcohol solvent and alkaline deep eutectic solvent are mixed, and alcoholyzed at 50-80° C. for 1-15 hours to obtain an ethylene-vinyl alcohol copolymer solution, and water is added for precipitation, filtered and vacuum dried to obtain the ethylene-vinyl alcohol copolymer.

Citation Information

Patent Citations

  • Preparation method of ethylene-vinyl alcohol copolymer

    CN102942649A

  • Method for preparing ethylene-vinyl alcohol copolymer

    CN109651557A

  • Ethylene-vinyl alcohol copolymer as well as preparation method and application thereof

    CN113736004A

  • Method for continuous copolymerization of ethylene and vinyl acetate

    US4485225A

  • Ethylene-vinyl alcohol copolymer, and preparation method and application thereof

    CN113861313A