A method for preparing wrinkle-resistant cotton fabric at low temperature
By immersing the anti-wrinkle finishing solution at low temperature and pre-baking, the problem of high anti-wrinkle finishing temperature of cotton fabrics is solved, effective cross-linking is achieved at low temperature, process flow is simplified, energy consumption is reduced and fabric performance is improved , has significant economic and environmental value.
Patent Information
- Application Number
- CN202210998652.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-08-19
AI Technical Summary
The baking temperature in the existing cotton fabric anti-wrinkle finishing technology is too high, resulting in high energy consumption in the production process, heavy equipment burden, serious environmental pollution, and is not conducive to sustainable development.
The method of immersing the anti-wrinkle finishing solution at low temperature and pre-baking is adopted. By stacking the finishing agent, the molecules can be diffused and cross-linked better, reducing the interaction between the finishing agent molecules and increasing the probability of collision between cellulose molecules. Thus, effective crosslinking is achieved at lower temperatures.
It realizes the preparation of anti-wrinkle cotton fabrics at low temperatures, simplifies the process flow, reduces energy consumption, improves the wrinkle recovery angle and strong retention rate of the fabric, and has significant industrial application value.
Smart Images

Figure SMS_1 
Figure SMS_3 
Figure SMS_4
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of anti-wrinkle finishing of fabrics, and particularly relates to a method for preparing anti-wrinkle cotton fabrics at low temperature. Background Art
[0002] Natural cellulose fabrics are soft, breathable, and comfortable to wear, so they are popular among the public. But at the same time, cotton fiber fabrics are very easy to form wrinkles during daily wear, which affects the appearance. Therefore, anti-wrinkle finishing of cotton fabrics has important practical significance. At present, the main problem of anti-wrinkle finishing of cotton fabrics in industry is that the baking temperature is too high. The finishing temperature of low-formaldehyde N-hydroxymethyl compounds is about 150°C, while the finishing temperature of polycarboxylic acid cross-linking agents is 170-180°C. This not only greatly increases the energy consumption in the production process, increases the burden on equipment, and increases the operating costs of enterprises, but also emits too much greenhouse gas, which is not conducive to environmental protection and social sustainable development. Therefore, reducing the anti-wrinkle finishing temperature of cotton fabrics has important economic value and ecological environmental value. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a method for preparing wrinkle-resistant cotton fabric at low temperature, so as to overcome the defect of high anti-wrinkle finishing temperature of cotton fabric in the prior art.
[0004] The present invention provides a method for preparing wrinkle-resistant cotton fabric at low temperature, comprising:
[0005] (1) immersing cotton fabric in an anti-wrinkle finishing liquid, dipping, double dipping and double rolling, and sealing and stacking the cotton fabric after dipping and rolling; (2) pre-baking and baking the fabric after stacking in step (1), wherein the baking temperature is 120-155°C.
[0006] Preferably, the anti-wrinkle finishing liquid in step (1) is a polycarboxylic acid finishing liquid or a formaldehyde 2D resin finishing liquid.
[0007] Preferably, the anti-wrinkle finishing liquid is a polycarboxylic acid finishing liquid, and the baking temperature is 130-155°C.
[0008] Preferably, the anti-wrinkle finishing liquid is formaldehyde 2D resin finishing liquid, and the baking temperature is 120-135°C.
[0009] Preferably, the polycarboxylic acid finishing liquid or formaldehyde 2D resin finishing liquid comprises: 10g / L-100g / L of anti-wrinkle finishing agent, 10g / L-40g / L of catalyst, 1g / L-11g / L of penetrant and 5g / L-20g / L of silicone softener, wherein the anti-wrinkle finishing agent is polycarboxylic acid or formaldehyde 2D resin.
[0010] Preferably, the polycarboxylic acid is one or more of butanetetracarboxylic acid, maleic acid, and itaconic acid; the catalyst is sodium hypophosphite or magnesium chloride; the penetrant is JFC, and the softener is a silicone softener.
[0011] More preferably, the anti-wrinkle finishing liquid comprises: 80 g / L of polycarboxylic acid, 36.2 g / L of catalyst, 5 g / L of penetrant, and 20 g / L of softener, wherein the catalyst is sodium hypophosphite, the penetrant is JFC, and the softener is silicone softener.
[0012] More preferably, the anti-wrinkle finishing liquid comprises: 90 g / L formaldehyde 2D resin, 15 g / L catalyst, 5 g / L penetrant, and 20 g / L softener, wherein the catalyst is magnesium chloride, the penetrant is JFC, and the softener is a silicone softener.
[0013] Preferably, the immersion time in step (1) is 10 to 15 seconds.
[0014] Preferably, the liquid rolling rate of the double dipping and double rolling in step (1) is 60% to 100%.
[0015] Preferably, in step (1), the stacking temperature is 25-40° C., the stacking time is 1-4 hours, and the stacking is sealed with a film.
[0016] Preferably, the pre-drying method in step (2) is drying on a heat setting machine.
[0017] Preferably, the pre-baking temperature in step (2) is 80-100°C, and the pre-baking time is 1-10 minutes. More preferably, the pre-baking temperature is 85°C, and the pre-baking time is 3 minutes.
[0018] Preferably, the baking time in step (2) is 3 to 6 minutes. More preferably, the baking temperature is 140° C. and the baking time is 5 minutes.
[0019] The present invention reduces the baking temperature mechanism: after stacking, the finishing agent molecules further diffuse into the fiber interior, which not only makes them more dispersed inside the fiber, but also reduces the interaction between the finishing agent molecules, increases the probability of effective collision between the finishing agent molecules and the cellulose macromolecules during the reaction process, and increases the reaction rate. Secondly, sufficient diffusion also increases the reaction area between the finishing agent and cellulose, allowing more finishing agent molecules to participate in cross-linking. Based on the above two reasons, effective cross-linking can be achieved at a lower temperature.
[0020] Beneficial Effects
[0021] Compared with the traditional anti-wrinkle process, the invention has a simple production method and controllable cost. The prepared fabric has a higher wrinkle recovery angle and strength retention rate. The wrinkle recovery angle of the finished fabric is higher than 240°, and the strength retention rate is higher than 60%.
[0022] The baking temperature adopted by the present invention is relatively low, which is 10-40° C. lower than that of the traditional process, greatly reducing the energy consumption and equipment depreciation in the production process, and has obvious industrial application value. DETAILED DESCRIPTION
[0023] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0024] Sources of reagents: low formaldehyde 2D resin (2D, Sane Chemical Technology (Shanghai) Co., Ltd.); butanetetracarboxylic acid (BTCA, Sane Chemical Technology (Shanghai) Co., Ltd.); maleic acid (MA, Sinopharm Chemical Reagent Co., Ltd.); itaconic acid (IA, Sinopharm Chemical Reagent Co., Ltd.); sodium hypophosphite (SHP, Shanghai McLean Biochemical Technology Co., Ltd.); magnesium chloride (MGC, Shanghai McLean Biochemical Technology Co., Ltd.).
[0025] Wrinkle recovery angle test standard: AATCC 66-2008.
[0026] Strength retention rate test standard: GB3923.1-1997.
[0027] Standard water washing method: AATCC 124.
[0028] DP grade test standard: AATCC 128-2003.
[0029] Example 1
[0030] Untreated cotton fabric was immersed in anti-wrinkle finishing liquid for 10 seconds, then double-immersed and double-rolled, with the rolling rate controlled to be 100%, and piled at 30℃ for 1.5 hours. Then pre-baked at 85℃ for 3 minutes and baked at 140℃ for 5 minutes. The anti-wrinkle finishing liquid includes 80g / L butane tetracarboxylic acid, 36.2g / L sodium hypophosphite, 10g / L penetrant JFC, and 20g / L silicone softener. After one standard water wash, the wrinkle recovery angle of the fabric is 248°, the strength retention rate is 64.5%, and the DP grade is 3.0.
[0031] Example 2
[0032] The untreated cotton fabric was immersed in the anti-wrinkle finishing liquid for 10 seconds, then double-immersed and double-rolled, with the rolling rate controlled to be 100%, and piled at 25°C for 2 hours. Then it was pre-baked at 85°C for 3 minutes and baked at 150°C for 3 minutes. The anti-wrinkle finishing liquid included 25g / L maleic acid, 28.1g / L itaconic acid, 36.2g / L sodium hypophosphite, 10g / L penetrant JFC, and 20g / L silicone softener. After one standard water wash, the wrinkle recovery angle of the fabric was 242°, the strength retention rate was 68.2%, and the DP grade was 2.5.
[0033] Example 3
[0034] The untreated cotton fabric was immersed in the anti-wrinkle finishing liquid for 10 seconds, then double-immersed and double-rolled, the rolling rate was controlled to be 100%, and then piled at 40°C for 1 hour. Then it was pre-baked at 80°C for 65 seconds, and then baked at 130°C for 3 minutes. The anti-wrinkle finishing liquid includes 90g / L low formaldehyde 2D resin, 15g / L magnesium chloride, 5g / L penetrant JFC, and 20g / L silicone softener. After one standard water wash, the wrinkle recovery angle of the fabric was 249°, the strength retention rate was 65.7%, and the DP grade was 2.9.
[0035] Example 4
[0036] The untreated cotton fabric was immersed in the anti-wrinkle finishing liquid for 10 seconds, then double-immersed and double-rolled, the rolling rate was controlled to be 100%, and then piled at 30°C for 3 hours. Then it was pre-baked at 80°C for 65 seconds, and then baked at 150°C for 3 minutes. The anti-wrinkle finishing liquid includes 80g / L of butane tetracarboxylic acid, 36.2g / L of sodium hypophosphite, 5g / L of penetrant JFC, and 20g / L of softener silicone softener. After a standard water wash, the wrinkle recovery angle of the fabric was 254°, the strength retention rate was 60.12%, and the DP grade was 3.2.
[0037] Comparative Example 1
[0038] The untreated cotton fabric was immersed in the anti-wrinkle finishing liquid for 10 seconds, then double-immersed and double-rolled, the rolling rate was controlled to be 100%, and then pre-baked at 85°C for 3 minutes and baked at 140°C for 5 minutes. The anti-wrinkle finishing liquid includes 80g / L butane tetracarboxylic acid, 36.2g / L sodium hypophosphite, 10g / L penetrant JFC, and 20g / L softener silicone softener. After a standard water wash, the wrinkle recovery angle of the fabric is 232°, the strength retention rate is 68.5%, and the DP grade is 2.6.
[0039] Comparative Example 2
[0040] The untreated cotton fabric was immersed in the anti-wrinkle finishing liquid for 10 seconds, then double-immersed and double-rolled, the rolling rate was controlled to be 100%, and then pre-baked at 85℃ for 3 minutes and baked at 150℃ for 3 minutes. The anti-wrinkle finishing liquid includes 25g / L maleic acid, 28.1g / L itaconic acid, 36.2g / L sodium hypophosphite, 10g / L penetrant JFC, and 20g / L silicone softener. After one standard water wash, the wrinkle recovery angle of the fabric is 222°, the strength retention rate is 72.5%, and the DP grade is 2.3.
[0041] Comparative Example 3
[0042] The untreated cotton fabric was immersed in the anti-wrinkle finishing liquid for 10 seconds, then double-immersed and double-rolled, and the rolling rate was controlled to be 100%. Then it was pre-baked at 80℃ for 65 seconds, and then baked at 150℃ for 3 minutes. The anti-wrinkle finishing liquid includes 90g / L low formaldehyde 2D resin, 15g / L magnesium chloride, 5g / L penetrant JFC, and 20g / L silicone softener. After one standard water wash, the wrinkle recovery angle of the fabric was 248°, the strength retention rate was 66.7%, and the DP grade was 3.0.
[0043] Comparative Example 4
[0044] The untreated cotton fabric was immersed in the anti-wrinkle finishing liquid for 10 seconds, then double-immersed and double-rolled, and the rolling rate was controlled to be 100%. Then it was pre-baked at 80℃ for 65 seconds, and then baked at 160℃ for 3 minutes. The anti-wrinkle finishing liquid includes 80g / L butane tetracarboxylic acid, 36.2g / L sodium hypophosphite, 5g / L penetrant JFC, and 20g / L softener silicone softener. After a standard water wash, the wrinkle recovery angle of the fabric was 255°, the strength retention rate was 59.6%, and the DP grade was 3.2.
[0045] Comparative Example 5
[0046] The untreated cotton fabric was immersed in the anti-wrinkle finishing liquid for 10 seconds, then double-immersed and double-rolled, the rolling rate was controlled to be 100%, and then dried at 80°C for 65 seconds, at which time the moisture content of the fabric was 7%. The fabric was then placed in a sealed stack at 30°C for 3 hours and then baked at 150°C for 3 minutes. The anti-wrinkle finishing liquid includes 80g / L of butane tetracarboxylic acid, 36.2g / L of sodium hypophosphite, 5g / L of penetrant JFC, and 20g / L of silicone softener. After a standard water wash, the wrinkle recovery angle of the fabric was 230°, the strength retention rate was 64.8%, and the DP grade was 2.5.
[0047] Comparative Example 6
[0048] The untreated cotton fabric was immersed in the anti-wrinkle finishing liquid for 10 seconds, then double-immersed and double-rolled, the rolling rate was controlled to be 100%, and then dried at 80°C for 65 seconds, at which time the moisture content of the fabric was 7%. The fabric was then wrapped and sealed and piled at 30°C for 3 hours. The finished fabric was washed and dried. The anti-wrinkle finishing liquid includes 80g / L of butane tetracarboxylic acid, 36.2g / L of sodium hypophosphite, 5g / L of penetrant JFC, and 20g / L of silicone softener. After one standard wash, the wrinkle recovery angle of the fabric was 132°, the strength retention rate was 84.8%, and the DP grade was 1.2.
[0049] Comparative Example 7
[0050] The untreated cotton fabric was immersed in the anti-wrinkle finishing liquid for 10 seconds, then double-immersed and double-rolled, the rolling rate was controlled to be 100%, and piled at 30°C for 22 hours, and then washed and dried. The anti-wrinkle finishing liquid includes 80g / L butane tetracarboxylic acid, 36.2g / L sodium hypophosphite, 5g / L penetrant JFC, and 20g / L silicone softener. After one standard wash, the wrinkle recovery angle of the fabric is 136°, the strength retention rate is 93.2%, and the DP grade is 1.3.
[0051] Comparative Example 8
[0052] The untreated cotton fabric was immersed in the anti-wrinkle finishing liquid for 10 seconds, then double-immersed and double-rolled, the rolling rate was controlled to be 100%, and then dried at 80℃ for 65 seconds, at which time the moisture content of the fabric was 7%. The fabric was then piled at 40℃ for 1 hour. Then it was baked at 130℃ for 3 minutes, and the fabric was washed and dried after finishing. The anti-wrinkle finishing liquid includes 90g / L low formaldehyde 2D resin, 15g / L magnesium chloride, 5g / L penetrant JFC, and 20g / L silicone softener. After one standard wash, the wrinkle recovery angle of the fabric was 228°, the strength retention rate was 74.1%, and the DP grade was 2.3.
[0053] Comparative Example 9
[0054] The untreated cotton fabric was immersed in the anti-wrinkle finishing liquid for 10 seconds, then double-immersed and double-rolled, the rolling rate was controlled to be 100%, and piled at 40°C for 22 hours, and then washed and dried. The anti-wrinkle finishing liquid includes 90g / L low formaldehyde 2D resin, 15g / L magnesium chloride, 5g / L penetrant JFC, and 20g / L silicone softener. The wrinkle recovery angle of the fabric is 130°, the strength retention rate is 95.1%, and the DP grade is 1.3.
[0055] Comparative Example 10
[0056] The untreated cotton fabric was immersed in the anti-wrinkle finishing liquid for 10 seconds, then double-immersed and double-rolled, the rolling rate was controlled to be 100%, then pre-baked at 80℃ for 65 seconds, and then baked at 130℃ for 3 minutes. The anti-wrinkle finishing liquid includes 100g / L low formaldehyde 2D resin, 20g / L magnesium chloride, 10g / L penetrant JFC, and 20g / L silicone softener. After one standard water wash, the wrinkle recovery angle of the fabric is 230°, the strength retention rate is 69.7%, and the DP grade is 2.4.
[0057] Comparative Example 11
[0058] The untreated cotton fabric was immersed in the anti-wrinkle finishing liquid for 10 seconds, then double-immersed and double-rolled, and the rolling rate was controlled to be 100%. Then it was pre-baked at 80℃ for 65 seconds, and then baked at 150℃ for 3 minutes. The anti-wrinkle finishing liquid includes 80g / L of butane tetracarboxylic acid, 36.2g / L of sodium hypophosphite, 5g / L of penetrant JFC, and 20g / L of softener silicone softener. After a standard water wash, the wrinkle recovery angle of the fabric was 235°, the strength retention rate was 62.8%, and the DP grade was 2.6.
[0059] The comparison between Examples 1-2 of the present invention and Comparative Examples 1-2 is shown in Table 1.
[0060] The comparison between Examples 3-4 of the present invention and Comparative Examples 3-4, 10-11 is shown in Table 2.
[0061] The comparison between Examples 3-4 of the present invention and Comparative Examples 5-9 is shown in Table 3.
[0062] Table 1: Comparison of finishing effects between stacking and non-stacking (same finishing temperature and time)
[0063]
[0064]
[0065] Table 2: Comparison of stacking and non-stacking sorting conditions
[0066]
[0067] Table 3: Comparison of stacking methods
[0068]
Claims
1. A method for preparing wrinkle-resistant cotton fabric at low temperature, include: (1) immersing the cotton fabric in an anti-wrinkle finishing liquid, dipping, double dipping and double rolling, and sealing and stacking the cotton fabric after the rolling; wherein the stacking temperature is 25 to 40° C. and the stacking time is 1 to 4 hours; (2) pre-baking and baking the fabrics after stacking in step (1); wherein the pre-baking temperature is 80-100° C. and the pre-baking time is 1-10 min; the anti-wrinkle finishing liquid is a polycarboxylic acid finishing liquid, and the baking temperature is 130-155° C.; or the anti-wrinkle finishing liquid is a formaldehyde 2D resin finishing liquid, and the baking temperature is 120-135° C.; the polycarboxylic acid finishing liquid or the formaldehyde 2D resin finishing liquid comprises: an anti-wrinkle finishing agent of 10 g / L-100 g / L, a catalyst of 10 g / L-40 g / L, a penetrant of 1 g / L-11 g / L and a softener of 5 g / L-20 g / L, the anti-wrinkle finishing agent is a polycarboxylic acid or a formaldehyde 2D resin; and the catalyst is sodium hypophosphite or magnesium chloride.
2. The method according to claim 1, It is characterized in that In step (1), the liquid rolling rate of the double dipping and double rolling is 60% to 100%.
3. The method according to claim 1, It is characterized in that The baking time in step (2) is 3 to 6 minutes.