A preparation method of high permeability hybrid silicon membrane and its application

By using 1,2-bis(triethoxysilyl)ethane sol as the intermediate layer material, the preparation process of the organic silicon film is simplified, forming a loose structure, and solving the cumbersome preparation and throughput of the intermediate layer material in the existing technology. Solve the problem of shortcomings and achieve the preparation of high permeability membranes, significantly improving membrane flux and process efficiency.

CN115445449BActive Publication Date: 2024-10-15CHANGZHOU UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202211151089.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-21
Publication Date
2024-10-15
Estimated Expiration
2042-09-21

AI Technical Summary

Technical Problem

The preparation process of existing organic silicon membrane interlayer materials is cumbersome and time-consuming, which affects the membrane flux. Moreover, the preparation process of silica-zirconia sol is complicated, making it difficult to form a high-permeability interlayer.

Method used

1,2-bis(triethoxysilyl)ethane sol is used as the intermediate layer material. Through rapid acidification and high-temperature calcination, the preparation process of the intermediate layer and separation layer is simplified, and a loose structure is formed to increase the membrane flux.

Benefits of technology

The membrane flux is significantly improved, the preparation process is simplified, time and labor costs are reduced, while the selectivity of the membrane is maintained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115445449B_ABST
    Figure CN115445449B_ABST
Patent Text Reader

Abstract

The present invention provides a preparation method of a high-permeability hybrid silicon membrane and its application, which comprises the following steps: preparation of an intermediate layer sol, preparation of a separation layer sol, preparation of an intermediate layer, and preparation of a separation layer. In the present invention, by replacing the silicon dioxide-zirconium dioxide intermediate layer, the corresponding microstructure generated is made looser, the transmission resistance is reduced, and the membrane flux is significantly improved. The preparation method has simplified preparation steps, and reduces production time, manpower, and raw material consumption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of membrane material preparation, and in particular relates to a preparation method of a high-permeability hybrid silicon membrane and application thereof. Background Art

[0002] Membrane separation technology has attracted extensive attention from researchers due to its advantages of being green, environmentally friendly, efficient and energy-saving. The selection of membrane materials is also a very important part of this. Silicone stands out among many materials because of its excellent molecular sieving performance, strong hydrothermal stability and adjustable pore size.

[0003] The support body commonly used in the preparation of organosilicon membranes is an alumina ceramic support body. The advantages of this support body are high porosity and strong mechanical properties, which can provide good support for the membrane. Its disadvantage is that it has a large average pore size, and the particle size of the organosilicon separation layer sol is small. Directly coating the separation layer sol on the support body will cause the sol particles to fall into the large pores of the support body, blocking the pores, and it is difficult to form a complete and uniform membrane layer. Therefore, before coating the separation layer, the support body needs to be modified to reduce its average pore size so that it can meet the requirements of coating the separation layer. According to the initial specifications of the support body, the support body used in the present invention is a tubular alumina ceramic support body, and the specific specifications are: average pore size 200nm, outer diameter 10mm, length 100mm, porosity 30-50%. The average pore size of 200nm still does not meet the requirements for directly coating the separation layer sol, so it is necessary to coat the intermediate layer to further modify the support. After the modification of the intermediate layer, the pore size of the support is reduced to about 0.7-1.5nm. At this time, when the separation layer sol is coated, it can be evenly distributed on the intermediate layer to form a complete and uniform membrane layer, and there will be no problem of sol particles falling and affecting the quality of the membrane layer and then affecting the separation performance of the membrane.

[0004] After consulting a large number of literatures, it was found that most of the intermediate layers of organic silicon membranes currently use silica-zirconium dioxide sol. Although silica-zirconium dioxide as an intermediate layer can effectively prevent the penetration of the separation layer sol, it also has major problems. For example: the transmission resistance of the target molecule in the separation system is too large, which will greatly affect the flux of the membrane. The preparation process of silica-zirconium dioxide sol is cumbersome and extremely time-consuming (it takes about 20 hours). And in the preparation process of the intermediate layer, it is necessary to repeat the coating and calcination process a large number of times (more than eight times) to form a complete intermediate layer. Therefore, the development of a simple preparation strategy for a high-permeability intermediate layer is one of the major breakthroughs in effectively improving the flux of organic silicon membranes. The 1,2-bis(triethoxysilyl)ethane sol used in the present invention has been shown to be used as an intermediate layer material after research and experiments. By increasing the amount of acid and rapidly acidifying, 1,2-bis(triethoxysilyl)ethane sol with a particle size comparable to that of silica-zirconia sol can be prepared. Compared with silica-zirconia sol, the preparation of 1,2-bis(triethoxysilyl)ethane sol only takes 0.5 to 1 hour, and in the preparation process of the membrane intermediate layer, only about three coating and calcination processes are required to prepare a relatively complete and uniform intermediate layer, which greatly reduces the time cost and reduces the consumption of manpower and material resources; more importantly, 1,2-bis(triethoxysilyl)ethane can form a looser structure than silica-zirconia after the sol-gel process, and such a structure is of great help in improving the membrane flux. In summary, as an intermediate layer material, 1,2-bis(triethoxysilyl)ethane has two main advantages, one is higher membrane flux, and the other is simpler sol preparation and membrane preparation process. Summary of the invention

[0005] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.

[0006] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.

[0007] Therefore, the object of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing a high-permeability hybrid silicon membrane and its application.

[0008] In order to solve the above technical problems, the present invention provides the following technical solution: a method for preparing a high permeability hybrid silicon membrane, comprising the following steps:

[0009] Preparation of intermediate layer sol: mixing an organosilicon precursor, deionized water and an acid and dissolving them in a solvent to prepare an intermediate layer sol;

[0010] Preparation of separation layer sol: mixing an organosilicon precursor, deionized water and an acid and dissolving them in a solvent to prepare a separation layer sol;

[0011] Preparation of the intermediate layer: dissolve and dilute the intermediate layer sol, apply it completely and evenly on the support, dry it and calcine it, repeat this process several times to form the intermediate layer;

[0012] Preparation of separation layer: dissolve and dilute the separation layer sol, apply it completely and evenly on the support, dry it and then calcine it, and repeat several times to form a separation layer.

[0013] As a preferred embodiment of the method for preparing the high-permeability hybrid silicon membrane described in the present invention, in which: in the preparation of the intermediate layer sol, the organosilicon precursor is first completely dispersed in the solvent and then a mixture of deionized water and acid is quickly added dropwise, and then the organosilicon precursor sol is obtained after continuous reaction for a period of time under stirring in a heated water bath; the molar ratio of organosilicon precursor: acid = 1: 0.5-1, and the mass fraction of the organosilicon precursor relative to the sol is maintained at 1.0-5.0wt%; the average particle size of the prepared organosilicon precursor sol is 30-50nm.

[0014] As a preferred embodiment of the method for preparing the high permeability hybrid silicon membrane of the present invention, in the preparation of the intermediate layer sol, the heating water bath condition is 60-70° C., and the heating time is 0.5-1 h.

[0015] As a preferred embodiment of the method for preparing the high permeability hybrid silicon membrane described in the present invention, in which: in the preparation of the intermediate layer, the high-temperature calcination is to coat the outer surface of the support with an organosilicon precursor sol, and calcine at high temperature under an inert atmosphere, and repeat the coating and calcination process for many times to form a complete and uniform high permeability intermediate layer. After coating the intermediate layer, the membrane pore size can be adjusted to about 0.7 to 1.5 nm, which is convenient for coating the separation layer.

[0016] As a preferred embodiment of the method for preparing the high permeability hybrid silicon membrane described in the present invention, the separation layer is prepared by coating a separation layer sol on the intermediate layer, calcining at high temperature under an inert atmosphere, and repeating the coating and calcining process multiple times to form a complete and uniform separation layer.

[0017] As a preferred embodiment of the method for preparing the high permeability hybrid silicon membrane described in the present invention, in which: in the preparation of the intermediate layer sol and the separation layer sol, the organic silicon precursor is one or more of 1,2-bis(triethoxysilyl)ethane, 1,2-bis(triethoxysilyl)ethylene, 1,2-bis(triethoxysilyl)acetylene, 1,4-bis(triethoxymethoxy)benzene, 4,4'-bis(triethoxysilyl)biphenyl, bis(triethoxysilyl)methane, etc.

[0018] As a preferred embodiment of the method for preparing the high permeability hybrid silicon membrane of the present invention, in the preparation of the intermediate layer sol and the separation layer sol, the acid is one or more of hydrochloric acid, nitric acid and the like.

[0019] As a preferred embodiment of the method for preparing the high permeability hybrid silicon membrane of the present invention, in the preparation of the intermediate layer sol and the separation layer sol, the solvent is one or more of ethanol, isopropanol, tetrahydrofuran and the like.

[0020] As a preferred embodiment of the method for preparing the high permeability hybrid silicon membrane of the present invention, in the preparation of the intermediate layer, the calcination is carried out under an inert atmosphere such as nitrogen and argon, and the calcination temperature is 200-350°C.

[0021] Another object of the present invention is to overcome the defects of the prior art and provide an application of a high permeability hybrid silicon membrane.

[0022] In order to solve the above technical problems, the present invention provides the following technical solutions: an application of a high permeability hybrid silicon membrane, which includes: the hybrid silicon membrane is used for gas separation, carbon capture, and pervaporation.

[0023] Beneficial effects of the present invention:

[0024] The present invention provides a method for preparing a high-permeability hybrid silicon membrane and its application. The high-permeability hybrid silicon membrane prepared by the present invention has the characteristics of a more loose structure and low transmission resistance in the membrane intermediate layer, and the membrane flux is significantly improved under the premise of ensuring the selectivity of the membrane. In addition, the strategy of increasing the amount of acid and high-temperature rapid acid catalysis simplifies the sol preparation and membrane preparation processes, greatly reduces the time cost, and significantly reduces the consumption of manpower and material resources. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 Schematic diagram of the network structure formed by the hydrolysis polymerization of 1,2-bis(triethoxysilyl)ethane and silicon dioxide-zirconium dioxide;

[0026] Figure 2 This is the result diagram of measuring the pore size of the middle layer membrane;

[0027] Figure 3Particle size distribution diagram of 1,2-bis(triethoxysilyl)ethane sol and silica-zirconium dioxide sol prepared with different acid ratios;

[0028] Figure 4 This is a physical picture obtained according to an embodiment of the present invention;

[0029] In the figure, from left to right are the actual products obtained in Example 2, Example 3, Example 1, Comparative Example 1, and Example 4. DETAILED DESCRIPTION

[0030] Example 1

[0031] The core point of the present invention lies in the innovation of the intermediate layer material and the preparation process, that is, using 1,2-bis(triethoxysilyl)ethane sol instead of the commonly used silicon dioxide-zirconium dioxide sol, so that the membrane obtains an intermediate layer with low transmission resistance and thus improves the membrane flux. The membrane preparation method used in the present invention is a sol-gel method, that is, first preparing a sol, and then calcining it at a high temperature to gel it into a membrane. The specific implementation process is also divided into a sol preparation process and a membrane preparation process.

[0032] Sol preparation: It is divided into intermediate layer sol preparation and separation layer sol preparation.

[0033] Preparation process of the intermediate layer sol: The molar ratio of each component in the sol is 1,2-bis(triethoxysilyl)ethane: deionized water: concentrated hydrochloric acid = 1:240:0.5, wherein 1,2-bis(triethoxysilyl)ethane accounts for 5% of the total mass ratio of the sol. Specifically, 1g of 1,2-bis(triethoxysilyl)ethane is completely dispersed in 6.7651g of ethanol solvent, and then 12.1834g of deionized water and 0.0515g of concentrated hydrochloric acid are quickly added dropwise under stirring conditions, and after being stirred evenly, it is placed in a water bath magnetic stirrer at 70°C and reacted for 0.5 hours to obtain a 5% 1,2-bis(triethoxysilyl)ethane sol.

[0034] Preparation process of separation layer sol: In order to reflect the change in membrane flux caused by the difference in the intermediate layer, the separation layer is prepared using the same organic silicon sol to ensure the consistency of the separation layer effect. For the sake of uniformity, the preparation of the separation layer in the embodiment uses 1,4-di(triethoxymethoxy)benzene as an organic silicon precursor. The molar ratio of each component in the sol is 1,4-di(triethoxymethoxy)benzene: deionized water: concentrated hydrochloric acid = 1:240:0.01, of which 1,4-di(triethoxymethoxy)benzene accounts for 5% of the total mass ratio of the sol. Specific preparation steps: 1g of 1,4-di(triethoxymethoxy)benzene is dispersed in 8.2656g of ethanol solvent, and then 10.7335g of deionized water and 0.0009g of concentrated hydrochloric acid are quickly added under stirring conditions. After stirring evenly, it is placed in a water bath magnetic stirrer at 50°C and reacted for 2 hours to obtain a 5% 1,4-di(triethoxymethoxy)benzene sol.

[0035] Membrane preparation: divided into the preparation of the intermediate layer and the separation layer.

[0036] Preparation process of the intermediate layer: 5% 1,2-bis(triethoxysilyl)ethane sol is diluted to 0.25% with solvent ethanol. A small amount of it is applied on the support in sequence and evenly, and after drying, it is placed in a nitrogen atmosphere tube furnace at 300°C and calcined for 30 minutes. The rubbing and calcining process is repeated three times to form the intermediate layer.

[0037] Preparation process of separation layer: 5% 1,4-bis(triethoxymethoxy)benzene sol was diluted to 0.25% with ethanol. A small amount of 1,4-bis(triethoxymethoxy)benzene sol was applied to the outside of the middle layer of the support in sequence and evenly, so that the sol on the support was evenly and completely covered, and then placed in a nitrogen atmosphere tube furnace at 300°C for calcination for 30 minutes after drying, and the rubbing and calcination process was repeated twice to form a separation layer.

[0038] The organic silicon film can be obtained through the above steps.

[0039] Example 2

[0040] This example is prepared by the preparation method in Example 1, with the following specific differences:

[0041] The molar ratio of each component in the sol is 1,2-bis(triethoxysilyl)ethane: deionized water: concentrated hydrochloric acid = 1:240:0.01, wherein 1,2-bis(triethoxysilyl)ethane accounts for 5% of the total mass ratio of the sol. Specific preparation steps: 1g of 1,2-bis(triethoxysilyl)ethane is completely dispersed in 6.8156g of ethanol solvent, and then 12.1834g of deionized water and 0.0010g of concentrated hydrochloric acid are quickly added dropwise under stirring conditions, and after being stirred evenly, it is placed in a water bath magnetic stirrer at 70°C and reacted for 0.5 hours to obtain a 5% 1,2-bis(triethoxysilyl)ethane sol.

[0042] Example 3

[0043] This example is prepared by the preparation method in Example 1, with the following specific differences:

[0044] The molar ratio of each component in the sol is 1,2-bis(triethoxysilyl)ethane: deionized water: concentrated hydrochloric acid = 1:240:0.1, wherein 1,2-bis(triethoxysilyl)ethane accounts for 5% of the total mass ratio of the sol. Specific preparation steps: 1g of 1,2-bis(triethoxysilyl)ethane is completely dispersed in 6.8066g of ethanol solvent, and then 12.1834g of deionized water and 0.0100g of concentrated hydrochloric acid are quickly added dropwise under stirring conditions, and after being stirred evenly, it is placed in a water bath magnetic stirrer at 70°C and reacted for 0.5 hours to obtain a 5% 1,2-bis(triethoxysilyl)ethane sol.

[0045] Example 4

[0046] This example is prepared by the preparation method in Example 1, with the following specific differences:

[0047] The molar ratio of each component in the sol is 1,2-bis(triethoxysilyl)ethane: deionized water: concentrated hydrochloric acid = 1:240:1, wherein 1,2-bis(triethoxysilyl)ethane accounts for 5% of the total mass ratio of the sol. Specific preparation steps: 1g of 1,2-bis(triethoxysilyl)ethane is completely dispersed in 6.7166g of ethanol solvent, and then 12.1834g of deionized water and 0.1000g of concentrated hydrochloric acid are quickly added dropwise under stirring conditions, and after being stirred evenly, it is placed in a water bath magnetic stirrer at 70°C and reacted for 0.5 hours to obtain a 5% 1,2-bis(triethoxysilyl)ethane sol.

[0048] Comparative Example 1

[0049] This example is prepared by the preparation method in Example 1, with the following specific differences:

[0050] Silica-zirconia sol was used to replace 1,2-bis(triethoxysilyl)ethane sol. Silica-zirconia sol was synthesized according to relevant literature reports, and the other steps were the same.

[0051] The organosilicon membranes prepared in Examples 1 to 4 and Comparative Example 1 were applied to CO2 / N2 separation. The membrane tube was placed in a membrane assembly, connected to a gas cylinder, the inlet pressure was controlled to be 100 kPa, and the test temperature was 200°C. The test results are shown in Table 1.

[0052] Table 1 CO2, N2 flux and CO2 / N2 selectivity of Examples 1 to 4 and Comparative Example 1 at 200°C

[0053]

[0054]

[0055] As can be seen from Table 1, Example 1 and Example 4 have more outstanding performance, among which Example 1 achieves better performance under the condition of less acid amount. Example 1 has the significant advantage of less acid usage and better performance, and more acid is used in Example 4, which will lead to an increase in the pore size of the membrane, resulting in weaker selectivity for gas, so the parameters in Example 1 are preferred parameters.

[0056] The organosilicon membranes prepared in Examples 1 to 4 and Comparative Example 1 were applied to pervaporation butanol dehydration, and the specific implementation steps were carried out according to the corresponding steps in Journal of Environmental Management 242 (2019) 415–429. The feed liquid composition was: 10% water, 90% butanol. The test temperature was 75°C. The test results are shown in Table 2.

[0057] Table 2 Water flux and separation factor of Examples 1 to 4 and Comparative Example 1 at 75°C

[0058] <![CDATA[Water flux [kg h -1 m -2 > Separation Factor Example 1 (acid ratio 0.5) 1.42 934 Example 2 (acid ratio 0.01) 0.55 135 Example 3 (acid ratio 0.1) 0.62 340 Example 4 (acid ratio 1) 1.5 720 Comparative Example 1 (Silicon Dioxide-Zirconium Dioxide) 0.73 958

[0059] As can be seen from Table 2, the finished product prepared in Example 1 has a significant advantage in water flux, and the preferred parameters of the present invention are the parameters in Example 1.

[0060] When the raw materials used are replaced with 1,2-bis(triethoxysilyl)ethane sol as the material for preparing the intermediate layer instead of the traditional commonly used silica-zirconium dioxide sol. Compared with silica-zirconium dioxide, due to the bridging structure of carbon-carbon single bonds between the two Si atoms of 1,2-bis(triethoxysilyl)ethane, the structure formed by the copolymerization of 1,2-bis(triethoxysilyl)ethane during the hydrolysis polymerization process is looser, thereby reducing the transmission resistance of the membrane intermediate layer and significantly improving the membrane flux while ensuring the selectivity of the membrane.

Claims

1. A method for preparing a high permeability hybrid silicon membrane, characterized in that: The following steps are included: Preparation of intermediate layer sol: mixing an organosilicon precursor, deionized water and an acid and dissolving them in a solvent to prepare an intermediate layer sol; Preparation of separation layer sol: mixing an organosilicon precursor, deionized water and an acid and dissolving them in a solvent to prepare a separation layer sol; Preparation of the intermediate layer: dissolve and dilute the intermediate layer sol, apply it completely and evenly on the support, dry it and calcine it, repeat this process several times to form the intermediate layer; Preparation of separation layer: dissolve and dilute the separation layer sol, apply it completely and evenly on the support, dry it and calcine it, repeat several times to form the separation layer; In the preparation of the intermediate layer sol, the organosilicon precursor is first completely dispersed in a solvent and then a mixture of deionized water and an acid is quickly added dropwise, and then the reaction is continued for a period of time under stirring in a heated water bath to obtain an organosilicon precursor sol, wherein the molar ratio of organosilicon precursor: acid is 1:0.5-1; The organosilicon precursor is 1,2-bis(triethoxysilyl)ethane.

2. The method for preparing a high permeability hybrid silicon membrane according to claim 1, characterized in that: The mass fraction of the organosilicon precursor relative to the sol is maintained at 1.0-5.0wt%, and the average particle size of the prepared organosilicon precursor sol is 30-50nm.

3. The method for preparing a high permeability hybrid silicon membrane according to claim 1 or 2, characterized in that: In the preparation of the intermediate layer sol, the heating water bath condition is 60-70° C., and the heating time is 0.5-1 h.

4. The method for preparing a high permeability hybrid silicon membrane according to claim 1, characterized in that: In the preparation of the intermediate layer, high-temperature calcination is to coat the outer surface of the support with an organosilicon precursor sol, and high-temperature calcination is performed under an inert atmosphere. The coating and calcination processes are repeated multiple times to form a complete and uniform high-permeability intermediate layer. After coating the intermediate layer, the membrane pore size can be adjusted to 0.7 to 1.5 nm, which is convenient for coating the separation layer.

5. The method for preparing a high permeability hybrid silicon membrane according to claim 1, characterized in that: The separation layer is prepared by coating a separation layer sol on the intermediate layer, calcining at high temperature under an inert atmosphere, and repeating the coating and calcining process for multiple times to form a complete and uniform separation layer.

6. The method for preparing a high permeability hybrid silicon membrane according to claim 1, characterized in that: In the preparation of the intermediate layer sol and the separation layer sol, the acid is one or more of hydrochloric acid and nitric acid.

7. The method for preparing a high permeability hybrid silicon membrane according to claim 3, characterized in that: In the preparation of the intermediate layer sol and the separation layer sol, the solvent is one or more of ethanol, isopropanol and tetrahydrofuran.

8. The method for preparing a high permeability hybrid silicon membrane according to claim 5, characterized in that: In the preparation of the intermediate layer, the calcination is carried out in an inert atmosphere of nitrogen or argon, and the calcination temperature is 200-350°C.

9. An application of a high permeability hybrid silicon membrane prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The hybrid silicon membrane is used for gas separation, carbon capture, and pervaporation.

Citation Information

Patent Citations

  • Phenyl decorated organic-inorganic hybridization millipore silicon dioxide film preparation method

    CN102218270A

  • Silicon dioxide film for separating CH4 / CO2 gas and preparation method thereof

    CN103157390A

  • Hydroxypropyl cellulose-silicone hybrid membrane and preparation method thereof

    CN109925889A

  • Polycarbonate diol crosslinking organosilicone hybrid membrane and preparation method thereof

    CN109966937A

  • Solvent-resistant bridged polysilsesquioxane nanofiltration composite membrane and preparation method thereof