A method for preparing low-melting-point high-shrinkage recycled polyester
Through the combination of alcoholysis-regeneration one-step method and acetate catalyst, the problem of carbonization of the spandex component in recycled polyester is solved, the preparation of low melting point and high shrinkage recycled polyester is achieved, the quality and differentiation are improved, and the process is simplified. process and reduce costs.
Patent Information
- Application Number
- CN202211271243.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-18
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-10-18
AI Technical Summary
The spandex component in the existing recycled polyester process is easy to carbonize at high temperatures, resulting in a decline in the quality of recycled polyester, and there are few differentiated and functional products, which limits its application.
The one-step alcoholysis-regeneration method is used to modify the flexible segments produced by the alcoholysis of polyurethane. Through the alcoholysis-repolymerization process, acetate catalysts and antioxidants are combined to avoid high-temperature carbonization and achieve low melting point and high shrinkage regenerated polyester. Preparation of esters without adding comonomers.
It effectively solves the problem of carbonization of spandex components, improves the quality and differentiation of recycled polyester, and realizes the efficient use of waste polyester. The melting point of the product is 100-180°C, and the elastic recovery rate reaches more than 90% at 5% elongation. , the process is simple and the cost is reduced.
Abstract
Description
Technical Field
[0001] The present application relates to a method for preparing low-melting-point high-shrinkage recycled polyester, and belongs to the technical field of chemical fiber preparation. Background Art
[0002] Polyethylene terephthalate (PET) is widely used due to its excellent performance, but due to its poor degradation performance, it has serious environmental pollution problems after use. Therefore, it is an important issue in the current polyester industry to achieve effective circulation of resources and reduce degradation load through recycling.
[0003] During the recycling process, we found that existing polyester fabrics often contain a large amount of spandex components. On the one hand, these spandex components will undergo depolymerization reactions accompanied by alcoholysis, and the large amount of aliphatic chain segments produced will be difficult to repolymerize in the subsequent polyester polycondensation stage. On the other hand, the polycondensation stage is a long-term high-temperature environment, and the spandex depolymerization components have poor heat resistance and are prone to carbonization. The above two reasons have led to the deterioration of the appearance quality of recycled polyester, serious homogeneity problems, and a low degree of differentiation.
[0004] Among them, there are some studies on the differentiation of recycled polyester in the prior art, such as: CN107652423A regulates the quality of esterification by adding comonomers after alcoholysis of waste polyester; patent CN104327259A uses diol titanium alkali metal coordination compounds soluble in ethylene glycol as catalysts to catalyze the co-condensation process; CN111995739A introduces crystal nucleating agents into the polyester macromolecular structure to improve the impaired crystallization performance caused by modifiers. But overall, the high-value utilization level of recycled polyester is still low, and differentiated and functional recycled polyester products are still rare.
[0005] However, the carbonization problem of spandex in the process of recycled polyester is still a technical bottleneck that the industry has not been able to solve. If the above problems cannot be solved, the effective application of recycled polyester will inevitably be limited. Summary of the invention
[0006] In view of this, the present application provides a method for preparing low-melting point and high-shrinkage recycled polyester to solve the problems of degradation and carbonization of spandex components and deterioration of recycled polyester quality during the regeneration of waste polyester. The preparation method does not require the addition of comonomers, which is conducive to the efficient utilization of waste polyester and the differentiated development of recycled polyester.
[0007] Specifically, the present application is implemented through the following scheme:
[0008] A method for preparing low-melting-point high-shrinkage recycled polyester, using waste polyester containing polyurethane as raw material, and performing the following steps:
[0009] (1) Firstly, ethylene terephthalate and oligomers are placed in an alcoholysis kettle, and then raw materials, ethylene glycol and catalyst are added therein for alcoholysis. The alcoholysis temperature is 190-210°C, and the alcoholysis is carried out for 2-6 hours. Insoluble components are removed by hot filtration. The filtrate is subjected to reduced pressure distillation to recover ethylene glycol, and then cooled to obtain an alcoholysis product. The mass content of spandex component in the raw materials is 3-5%, the molar ratio of raw materials to ethylene glycol is 1:2-6, the amount of ethylene terephthalate and oligomers added is 20-40% of the mass of the raw materials, and the catalyst is an acetate catalyst, and the amount added is 1-3‰ of the mass of the raw materials.
[0010] (2) Add stabilizer and antioxidant to the alcoholysis product and directly repolymerize to obtain esterification product. The repolymerization temperature is 220-240°C and the reaction time is 1-2h.
[0011] (3) The esterification product enters the pre-condensation reactor for condensation to obtain the finished recycled polyester. The melting point of the recycled polyester is 100-180 °C, and the elastic recovery rate is more than 90% when the elongation is 5%. The condensation is divided into two stages: the initial condensation temperature is controlled at 240-260 °C, the vacuum degree is 1-100 Kpa, and the reaction time is 3-4 hours; the final condensation reaction temperature is 260-270 °C, the vacuum degree is 0.1-1 Kpa, and the reaction time is 1-2 hours.
[0012] The above process utilizes the flexible chain segments produced by polyurethane alcoholysis to modify the recycled polyester. Through the alcoholysis-regeneration one-step method, no additional modifier is needed to prepare recycled polyester with a melting point of 100-180°C and an elastic recovery rate of more than 90% when the elongation is 5%, thereby giving the recycled polyester the characteristics of low melting point and high shrinkage. The alcoholysis product is mainly dihydroxyethyl terephthalate (BHET) and its oligomers, and the composite system is directly re-condensed. There is no need to add additional comonomers before re-condensation, so high-temperature polymerization is avoided, the carbonization problem of the spandex component is effectively solved, and the process is simple.
[0013] Further, as a preference:
[0014] In step (1), the catalyst is any one of manganese acetate, zinc acetate, cobalt acetate and lead acetate.
[0015] In step (1), the hot filtration refers to filtering the liquid obtained by alcoholysis at about 200°C.
[0016] In step (1), the molar ratio of raw materials to ethylene glycol is 1: 4-6, the amount of ethylene terephthalate and oligomers added is 20-30% of the raw material mass, the alcoholization temperature is 200-210°C, and the reaction time is 5-6 hours. At this time, the finished recycled polyester obtained has a lower melting point and an elastic recovery rate of more than 95% at 5% elongation.
[0017] In step (2), the repolymerization temperature is 220-230°C and the reaction time is 1.5-2h. The esterification reaction of the alcoholysis product is more effective and will not cause high temperature carbonization problems.
[0018] In step (2), the stabilizer is selected from the group consisting of triphenyl phosphate, phosphorous acid, and trimethyl phosphate, and the added amount accounts for 0.01 to 0.1‰ of the mass of the raw material.
[0019] In step (2), the antioxidant includes but is not limited to hindered phenol antioxidants, and the added amount is 0.3 to 0.8 ‰ of the mass of the raw material. In this case, the hindered phenol antioxidant can be 2,6-di-tert-butyl-4-methylphenol (BHT), and the added amount is 0.5 to 0.8 ‰ of the mass of the obtained product.
[0020] In step (3), the initial polycondensation temperature is controlled at 240-250°C to avoid high temperature carbonization.
[0021] The beneficial effects of the present invention are:
[0022] 1) After alcoholysis of ethylene glycol, the preparation of low-melting-point and high-shrinkage recycled polyester can be achieved without adding additional modifiers.
[0023] 2) It effectively solves the problem of carbonization of spandex components in polyester during the recycling process of waste polyester, which reduces the recycling quality.
[0024] 3) Add stabilizer during the polymerization process to avoid yellowing side reactions.
[0025] 4) The product preparation process is short, with high yield and good quality. DETAILED DESCRIPTION
[0026] Example 1
[0027] The present embodiment provides a method for preparing a low melting point high shrinkage recycled polyester, comprising the following steps:
[0028] (1) Pretreatment of waste polyester: waste polyester containing spandex is selected as the treatment object, and the spandex content is not higher than 5%. The waste polyester is cleaned, cut and sent to the silo for the next process;
[0029] (2) Alcoholysis of waste polyester: The pretreated waste polyester and ethylene glycol are put into an alcoholysis reactor together, with the molar ratio of waste polyester to ethylene glycol being 1:2. The alcoholysis reactor contains ethylene terephthalate and oligomers accounting for 40% of the total mass of the input waste polyester, and manganese acetate accounting for 1‰ of the mass of the raw materials is added as a catalyst. The alcoholysis reaction temperature is 210°C and the reaction time is 2 hours.
[0030] (3) subjecting the product after alcoholysis to rapid hot filtration, subjecting the filtrate to vacuum distillation to recover ethylene glycol, dissolving the liquid after vacuum distillation in a hot alcohol solution, subjecting the filtrate to hot filtration to remove insoluble matter, and naturally cooling the filtrate to obtain bis(hydroxyethyl) terephthalate and its oligomers;
[0031] (4) adding the obtained alcoholysis product to an esterification kettle, controlling the esterification reaction temperature in the esterification kettle to 240°C and the reaction time to 1 hour, and adding 0.01‰ of triphenyl phosphate as a stabilizer and 0.3‰ of a hindered phenol antioxidant to the raw material weight;
[0032] (5) When the esterified product enters the pre-polycondensation reactor for polycondensation, the temperature is controlled at 250°C, the vacuum degree is 1Kpa, and the reaction time is 3.5 hours; then it enters the final polycondensation reactor, the reaction temperature is controlled at 260°C, the vacuum degree is 0.1Kpa, and the reaction time is 1 hour;
[0033] The final polyester has a melting point of 178°C and an elastic recovery rate of 95% at an elongation of 5%.
[0034] Example 2
[0035] A method for preparing a low-melting-point high-shrinkage recycled polyester in this embodiment comprises the following steps:
[0036] (1) Pretreatment of waste polyester: Use waste polyester of polyester-type spandex, where the content of polyester-type spandex components is not higher than 5%. Cut the clean waste polyester fibers and send them into the silo for the next process;
[0037] (2) Alcoholysis of waste polyester: the pretreated waste polyester is fed into an alcoholysis reactor at a molar ratio of 1:2 between waste polyester and ethylene glycol, wherein the alcoholysis reactor contains 40% by mass of ethylene terephthalate and oligomers of the total waste polyester, and 2‰ by mass of zinc acetate catalyst is added. The alcoholysis reaction temperature is 190°C and the reaction time is 4 hours.
[0038] (3) subjecting the product after alcoholysis to rapid hot filtration, subjecting the filtrate to vacuum distillation to recover ethylene glycol, dissolving the liquid after vacuum distillation in a hot alcohol solution, subjecting the filtrate to hot filtration to remove insoluble matter, and naturally cooling the filtrate to obtain bis(hydroxyethyl) terephthalate and its oligomers;
[0039] (4) adding the obtained alcoholysis product to an esterification kettle, controlling the esterification reaction temperature in the esterification kettle to be 240°C and the reaction time to be 1 hour, and simultaneously adding 0.02‰ of phosphorous acid as a stabilizer and 0.5‰ of a hindered phenol antioxidant to the raw material weight;
[0040] (5) When the esterified product enters the pre-polycondensation reactor for polycondensation, the temperature is controlled at 260°C, the vacuum degree is 100Kpa, and the reaction time is 3 hours; then it enters the final polycondensation reactor, the reaction temperature is controlled at 270°C, the vacuum degree is 0.1Kpa, and the reaction time is 2 hours;
[0041] The final polyester has a melting point of 170°C and an elastic recovery rate of 92% at an elongation of 5%.
[0042] Example 3
[0043] A method for preparing a low-melting-point high-shrinkage recycled polyester in this embodiment comprises the following steps:
[0044] (1) Pretreatment of waste polyester: Use waste polyester of polyester-type spandex, where the content of polyester-type spandex components is not higher than 5%. Cut the clean waste polyester fibers and send them into the silo for the next process;
[0045] (2) Alcoholysis of waste polyester: the pretreated waste polyester is fed into an alcoholysis reactor at a molar ratio of 1:4 between waste polyester and ethylene glycol, wherein the alcoholysis reactor contains 30% by mass of ethylene terephthalate and oligomers of the total amount of the input waste polyester, and 2‰ by mass of cobalt acetate catalyst is added. The alcoholysis reaction temperature is 200°C and the reaction time is 5 hours.
[0046] (3) subjecting the product after alcoholysis to rapid hot filtration, subjecting the filtrate to vacuum distillation to recover ethylene glycol, dissolving the liquid after vacuum distillation in a hot alcohol solution, subjecting the filtrate to hot filtration to remove insoluble matter, and naturally cooling the filtrate to obtain bis(hydroxyethyl) terephthalate and its oligomers;
[0047] (4) adding the obtained alcoholysis product to an esterification kettle, controlling the esterification reaction temperature in the esterification kettle to be 230°C and the reaction time to be 1.5 hours, and simultaneously adding 0.05‰ of triphenyl phosphate as a stabilizer and 0.5‰ of a hindered phenol antioxidant to the raw material weight;
[0048] (5) When the esterified product enters the pre-polycondensation reactor for polycondensation, the temperature is controlled at 250°C, the vacuum degree is 1Kpa, and the reaction time is 3.5 hours; then it enters the final polycondensation reactor, the reaction temperature is controlled at 260°C, the vacuum degree is 0.1Kpa, and the reaction time is 1 hour;
[0049] The final polyester has a melting point of 165°C and an elastic recovery rate of 96% at an elongation of 5%.
[0050] Example 4
[0051] A method for preparing a low-melting-point high-shrinkage recycled polyester in this embodiment comprises the following steps:
[0052] (1) Pretreatment of waste polyester: Use waste polyester of polyester-type spandex, where the content of polyester-type spandex components is not higher than 5%. Cut the clean waste polyester fibers and send them into the silo for the next process;
[0053] (2) Alcoholysis of waste polyester: the pretreated waste polyester is fed into an alcoholysis reactor at a molar ratio of 1:6 between waste polyester and ethylene glycol, wherein the alcoholysis reactor contains ethylene terephthalate and oligomers accounting for 20% by mass of the total amount of the input waste polyester, and lead acetate catalyst accounting for 3‰ by mass of the raw materials is added. The alcoholysis reaction temperature is 210°C and the reaction time is 6 hours.
[0054] (3) subjecting the product after alcoholysis to rapid hot filtration, subjecting the filtrate to vacuum distillation to recover ethylene glycol, dissolving the liquid after vacuum distillation in a hot alcohol solution, subjecting the filtrate to hot filtration to remove insoluble matter, and naturally cooling the filtrate to obtain bis(hydroxyethyl) terephthalate and its oligomers;
[0055] (4) adding the obtained alcoholysis product to an esterification kettle, controlling the esterification reaction temperature in the esterification kettle to be 220°C and the reaction time to be 2 hours, and adding 0.01‰ of trimethyl phosphate as a stabilizer and 0.8‰ of a hindered phenol antioxidant to the raw material weight;
[0056] (5) When the esterified product enters the pre-polycondensation reactor for polycondensation, the temperature is controlled at 240°C, the vacuum degree is 1Kpa, and the reaction time is 4 hours; then it enters the final polycondensation reactor, the reaction temperature is controlled at 260°C, the vacuum degree is 0.1Kpa, and the reaction time is 1 hour;
[0057] The final polyester has a melting point of 160°C and an elastic recovery rate of 95% at an elongation of 5%.
[0058] It can be seen from the above embodiments that: by adopting the alcoholysis process of this case, the melting point of the final recycled polyester can be achieved at 160-178°C, and the elastic recovery rate at 5% elongation can reach 92-95%, which meets the quality requirements of recycling, and there is no longer any quality limitation during differentiated treatment; during the reaction process, except for the ethylene terephthalate and oligomers added in the alcoholysis stage, no additional comonomers are required. During the alcoholysis process, the greater the addition ratio of ethylene glycol, the lower the corresponding addition ratio of ethylene terephthalate and oligomers can be, which effectively reduces the addition ratio of comonomers, and further reflects the reduction in overall cost.
Claims
1. A method for preparing low-melting-point high-shrinkage recycled polyester, characterized in that: Use waste polyester containing polyurethane as raw material and carry out the following treatment steps: (1) Firstly, ethylene terephthalate and oligomers are placed in an alcoholysis kettle, and then raw materials, ethylene glycol and catalyst are added therein for alcoholysis. The alcoholysis temperature is 200-210°C, and the alcoholysis is carried out for 5-6 hours. The liquid obtained by alcoholysis is hot filtered at 200°C to remove insoluble components. The filtrate is subjected to reduced pressure distillation to recover ethylene glycol, and then cooled to obtain an alcoholysis product. The mass content of spandex component in the raw materials is 3-5%, the molar ratio of raw materials to ethylene glycol is 1:4-6, the amount of ethylene terephthalate and oligomers added is 20-30% of the mass of the raw materials, and the catalyst is any one of manganese acetate, zinc acetate, cobalt acetate and lead acetate, and the amount added is 1-3‰ of the mass of the raw materials; (2) Adding a stabilizer and an antioxidant to the alcoholysis product and directly repolymerizing it to obtain an esterification product, the repolymerization temperature is 220-230°C, the reaction time is 1.5-2h, the stabilizer is one of triphenyl phosphate, phosphorous acid, and trimethyl phosphate, the addition amount is 0.01-0.1‰ of the raw material mass, the antioxidant includes but is not limited to hindered phenol antioxidants, the addition amount of the antioxidant is 0.5-0.8‰ of the raw material mass; (3) The esterification product enters the pre-condensation reactor for condensation. The condensation is divided into two stages: the initial condensation temperature is controlled at 240-250°C, the vacuum degree is 1-100 kPa, and the reaction time is 3-4 hours; the final condensation reaction temperature is 260-270°C, the vacuum degree is 0.1-1 kPa, and the reaction time is 1-2 hours to obtain the finished recycled polyester. The melting point of the recycled polyester is 100-180°C, and the elastic recovery rate is more than 90% when the elongation is 5%.