Medical polyester and production method thereof

By adding a flow accelerator prepared by the esterification reaction of fatty alcohol and tricarboxylic acid at the outlet of the final shrinkage kettle during the preparation of medical polyester, the problem of insufficient material fluidity and low product qualification rate is solved, and the fluidity of the polyester is improved. and demoulding ability, which improves the appearance transparency and dimensional stability of the product, achieving the goals of high qualification rate and environmental protection and energy saving.

CN115477830BActive Publication Date: 2024-10-29CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202110603062.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-05-31
Publication Date
2024-10-29
Estimated Expiration
2041-05-31

AI Technical Summary

Technical Problem

In the current preparation process of medical polyester, there are problems such as insufficient material fluidity, difficulty in demoulding, product eccentricity, flow marks, and low product qualification rate.

Method used

The esterification reaction uses dibasic acid and glycol as raw materials, and a flow accelerator is added to the side of the melt pipeline at the outlet of the final shrinkage kettle to generate polyester with an intrinsic viscosity of 0.55-0.70dL/g through the esterification reaction. Slicing, the flow promoter is prepared by the esterification reaction of fatty alcohol and tricarboxylic acid under acidic catalytic conditions, the molar ratio is 1 to 8:1, and the addition amount is 0.01%-3%.

Benefits of technology

Significantly improve the fluidity and demoulding ability of medical polyester materials, increase the melt index by more than 30%, reduce haze by 20%-50%, solve problems such as eccentricity of blood collection tubes and surface flow marks, and the product qualification rate is as high as 99.5%. Meet the industry trend of green environmental protection, energy saving and consumption reduction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to a medical polyester and a production method thereof, and belongs to the field of polyester. The method uses dibasic acid and diol as raw materials b, and the raw materials, polymerization catalyst, toner, and phosphorus stabilizer are mixed into slurry and put into an esterification kettle. After esterification reaction, the slurry enters a final reduction kettle for polycondensation reaction, and a flow promoter is added to the side end of the melt pipeline at the outlet of the final reduction kettle to fully mix with the polymer, and the material is discharged to obtain a polyester slice with a characteristic viscosity of 0.55-0.70dL / g. The present invention adopts a flow promoter monomer, which solves the problems that the flow promoter in the prior art has a small molecular weight, unstable properties, is not resistant to high temperatures, and is easy to increase the haze of polyester materials and affect the appearance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polyester, and in particular to a medical polyester and a production method thereof. Background Art

[0002] In recent years, with the continuous development and breakthroughs in medical science and biotechnology, the application of polyethylene terephthalate (PET) in the medical equipment and packaging industries has grown rapidly. It has stable chemical properties, is not easy to react chemically with the substances in the package, and is light, transparent, has excellent barrier properties, is non-toxic and not easy to break. The demand for heavy-weight PET blood collection tubes as virus sampling tubes has skyrocketed. Compared with traditional ordinary glass blood collection tubes, they are light and not easy to break, easy to transport and store; the probability of tube wall damage is extremely small, and the possibility of sample leakage is extremely small; after use, they can be directly sterilized by high pressure or incinerated and destroyed, without disinfection and reuse; low cost and easy processing.

[0003] Medicine bottles, disposable blood collection tubes and other polyester medical containers are products with a large flow length ratio. These products are generally small and thin-walled. Compared with ordinary PET polyester materials, there is a big difference in processing technology. When performing injection molding production, polyester materials are required to have good fluidity, easy demoulding, good appearance quality and dimensional stability, and be able to withstand large static loads. The appearance and manufacturability of the products should be considered in the production process. In view of the high fluidity of the material, the intrinsic viscosity of polyester is generally required to be less than 0.70dL / g. Since it needs to withstand a large static load, the intrinsic viscosity should not be too low, and 0.55-0.70dL / g is more appropriate.

[0004] Chinese patent CN104448720A discloses a medical modified polyester masterbatch and its preparation method. The invention uses medical polyester chips as carriers, adds lubricant polyethylene wax to the medical polyester chips, and the polyethylene wax has a number average molecular weight of 500-10000 and a content of 3%-15% of the weight of the polyester. It is easy to demould during injection molding and the qualified rate of the products is increased.

[0005] Chinese patent CN104017338A discloses a polyester slice for manufacturing vacuum blood collection tubes and its preparation method. The patent adds 0.1%-5% stearate and 0.1%-1% polyethylene wax to the polyester slice, so that the polyester slice has the advantages of high fluidity, high stability and rapid demoulding.

[0006] Chinese patent CN105860038A discloses a new production process for medical slices. The production process is to prepare a mixed solution of stearate and ethylene glycol and add it to the PET esterification system, add polyethylene wax to the melt pipeline at the outlet of the final reactor, and then granulate it, aiming to improve production efficiency and improve product qualification rate.

[0007] In addition, Chinese patent CN106589857A discloses a polyester chip masterbatch for blood collection tubes, a preparation method and an application thereof. The invention uses rheology modifiers polyester polyol, stearate, montanic acid and its derivatives, polyethylene glycol and rheology modifier promoter silicone resin to improve the melt fluidity of polyester chips for blood collection tubes.

[0008] Existing patents mainly add stearate, montanic acid, polyethylene glycol, polyester polyol, silicone resin and polyethylene wax to medical polyester carriers. These flow promoters have the problems of small molecular weight, unstable properties, high temperature resistance and easy increase of the haze of polyester materials. Summary of the invention

[0009] The purpose of the present invention is to solve the problems of insufficient material fluidity, difficulty in demoulding, product eccentricity, flow marks, low product qualification rate, etc. in the existing medical polyester preparation process, and to propose a medical polyester production method.

[0010] The purpose of the present invention can be achieved through the following technical solutions:

[0011] A preparation method of medical polyester, which uses dibasic acid and diol as raw materials b, mixes the raw materials, polymerization catalyst, toner and phosphorus stabilizer into slurry and puts it into an esterification kettle, after esterification reaction, enters a final reduction kettle for polycondensation reaction, adds a flow promoter to the side end of the melt pipeline at the outlet of the final reduction kettle and mixes it with the polymer thoroughly and evenly, and obtains polyester chips with a characteristic viscosity of 0.55-0.70dL / g.

[0012] A medical polyester is prepared by the following method:

[0013] With dibasic acid and diol as raw material b, raw material b, polymerization catalyst, colorant and phosphorus stabilizer are prepared into slurry and put into esterification kettle. After esterification reaction, it enters into final reduction kettle for polycondensation reaction. Flow promoter is added to the side end of melt pipeline at the outlet of final reduction kettle and mixed with polymer thoroughly and evenly, and polyester chips with characteristic viscosity of 0.55-0.70dL / g are obtained.

[0014] In the technical scheme of the present invention: the flow promoter is prepared by the following method: using fatty alcohol and tricarboxylic acid as raw materials a, carrying out esterification reaction under acidic catalyst conditions to obtain the flow promoter; or: the flow promoter is fatty alcohol.

[0015] In the technical solution of the present invention: the fatty alcohol is a C16-C24 fatty alcohol; preferably: the fatty alcohol is at least one of octadecyl alcohol, hexadecanol, tetracosanol, C16-18 alcohol and C20-22 alcohol.

[0016] In the technical solution of the present invention: the tricarboxylic acid is trimellitic anhydride, phosphoric acid or citric acid.

[0017] In the technical solution of the present invention, the molar ratio of fatty alcohol to tricarboxylic acid is 1-8:1.

[0018] Furthermore: the molar ratio of fatty alcohol to tricarboxylic acid is 2-5:1.

[0019] In the technical solution of the present invention: the acidic catalyst is concentrated sulfuric acid, and the amount of the catalyst is 0.01%-3% of the raw material a.

[0020] In the technical solution of the present invention, the added amount of the flow promoter monomer is 0.01%-3% of the weight of the medical polyester material.

[0021] Further: the added amount of the flow promoter monomer is 0.02%-0.4% by weight of the medical polyester material.

[0022] The present invention solves the problems of small molecular weight, unstable properties, high temperature resistance, and easy increase of polyester material haze affecting appearance in the flow promoter in the prior art. A flow promoter monomer is used to greatly improve the fluidity of medical polyester materials and the demoulding ability at the same time. The obtained product has good appearance transparency and stable dimensions. Compared with ordinary medical polyester with the same characteristic viscosity, the melt index is increased by more than 30%, and the haze is reduced by 20%-50%. The problems of eccentricity of blood collection tubes and surface flow marks are solved. The product qualification rate is as high as 99.5%, which meets the current industry trend of green environmental protection, energy saving and consumption reduction, and has great market prospects.

[0023] Beneficial effects of the present invention:

[0024] The invention adopts a flow promoter monomer, which solves the problems of small molecular weight, unstable properties, high temperature resistance, easy increase of polyester material haze and affecting appearance of the flow promoter in the prior art, and can greatly improve the fluidity of medical polyester materials, and at the same time improve the demoulding ability. The obtained product has good transparency and stable size. Compared with ordinary medical polyester with the same characteristic viscosity, the melt index is increased by more than 30%, and the haze is reduced by 20%-50%. The problems of eccentricity of blood collection tubes and surface flow marks are solved. The product qualification rate is as high as 99.5%, which meets the current industry trend of green environmental protection, energy saving and consumption reduction, and has great market prospects. DETAILED DESCRIPTION

[0025] The present invention is further described below in conjunction with embodiments, but the protection scope of the present invention is not limited thereto:

[0026] Comparative Example:

[0027] On the polyester production line, purified terephthalic acid and ethylene glycol are used as raw materials, ethylene glycol antimony is used as a polymerization catalyst, red and blue toners, and phosphoric acid heat stabilizers are mixed into a slurry and put into the esterification kettle. The molar ratio of purified terephthalic acid to ethylene glycol is 1:1.2; the amount of ethylene glycol antimony added is 180μg / g of the total amount of polyester; the amount of redness agent and blueness agent added is 0.6μg / g and 1.4μg / g of the total amount of polyester respectively; the amount of phosphoric acid heat stabilizer added is 15μg / g of the total amount of polyester. The esterification reaction temperature is 220-260℃. After the esterification reaction, it enters the final reduction kettle for polycondensation reaction. The polycondensation temperature is 275-285℃. After the polymerization reaction is completed, it enters the granulation system for granulation and packaging. After drying and pre-crystallization at 180℃ for 4h, medical polyester chips are obtained. The relevant index data measured with reference to the polyester test standard (GB / T14190-2009) are as shown in the following table.

[0028] Embodiment 1:

[0029] (1) Using hexadecanol and trimellitic anhydride in a molar ratio of 3:1 as raw material b, heating to 120° C. in the presence of a concentrated sulfuric acid catalyst in an amount of 0.05 wt % of raw material b, and reflux for 1.2 h to obtain a flow promoter monomer, hexadecanol trimellitate;

[0030] (2) On a polyester production line, purified terephthalic acid and ethylene glycol are used as raw materials, ethylene glycol antimony is used as a polymerization catalyst, red and blue toners, and phosphoric acid heat stabilizer are mixed into a slurry and fed into an esterification kettle, wherein the molar ratio of purified terephthalic acid to ethylene glycol is 1:1.2; the amount of ethylene glycol antimony added is 180 μg / g of the total amount of polyester; the amounts of redness agent and blueness agent added are 0.6 μg / g and 1.4 μg / g of the total amount of polyester, respectively; and the amount of phosphoric acid heat stabilizer added is 15 μg / g of the total amount of polyester. The esterification reaction temperature is 220-260°C. After the esterification reaction, it enters the final reduction kettle for condensation polymerization at a temperature of 275-285°C. The flow promoter monomer hexadecyl trimellitate is added to the melt line side of the final reduction kettle outlet using an online addition technology - screw plasticization method. The screw plasticization temperature is 120°C. The amount of flow promoter monomer added is 0.4% of the total amount of polyester. It is fully stirred with the polymer and then enters the granulation system for granulation and packaging. After drying and pre-crystallization at 180°C for 4 hours, medical polyester chips are obtained. The measured relevant index data are shown in the following table.

[0031] Embodiment 2:

[0032] (1) Using octadecyl alcohol and citric acid in a molar ratio of 3:1 as raw material b, heating to 155° C. in the presence of a concentrated sulfuric acid catalyst in an amount of 0.02 wt % of raw material b, and refluxing for 1.5 h to obtain a flow promoter monomer, octadecyl citrate;

[0033] (2) On a polyester production line, purified terephthalic acid and ethylene glycol are used as raw materials, ethylene glycol antimony is used as a polymerization catalyst, red and blue toners, and phosphoric acid heat stabilizer are mixed into a slurry and fed into an esterification kettle, wherein the molar ratio of purified terephthalic acid to ethylene glycol is 1:1.2; the amount of ethylene glycol antimony added is 180 μg / g of the total amount of polyester; the amounts of redness agent and blueness agent added are 0.6 μg / g and 1.4 μg / g of the total amount of polyester, respectively; and the amount of phosphoric acid heat stabilizer added is 15 μg / g of the total amount of polyester. The esterification reaction temperature is 220-260°C. After the esterification reaction, it enters the final reduction kettle for condensation polymerization at a temperature of 275-285°C. The flow promoter monomer octadecyl citrate is added to the melt line side of the final reduction kettle outlet using an online addition technology - screw plasticization method. The screw plasticization temperature is 160°C. The amount of flow promoter monomer added is 0.30% of the total amount of polyester. It is fully stirred and mixed with the polymer, and then enters the granulation system for granulation and packaging. After drying and pre-crystallization at 180°C for 4 hours, medical polyester chips are obtained. The measured relevant index data are shown in the following table.

[0034] Embodiment 3:

[0035] (1) using tetracosanol and trimellitic anhydride in a molar ratio of 3:1 as raw material b, heating to 125° C. under the condition that the amount of concentrated sulfuric acid catalyst is 0.01wt% of raw material b, and reflux for 2h to obtain a flow promoter monomer, tetracosanol trimellitic acid ester;

[0036] (2) On a polyester production line, purified terephthalic acid and ethylene glycol are used as raw materials, ethylene glycol antimony is used as a polymerization catalyst, red and blue toners, and phosphoric acid heat stabilizer are mixed into a slurry and fed into an esterification kettle, wherein the molar ratio of purified terephthalic acid to ethylene glycol is 1:1.2; the amount of ethylene glycol antimony added is 180 μg / g of the total amount of polyester; the amounts of redness agent and blueness agent added are 0.6 μg / g and 1.4 μg / g of the total amount of polyester, respectively; and the amount of phosphoric acid heat stabilizer added is 15 μg / g of the total amount of polyester. The esterification reaction temperature is 220-260°C. After the esterification reaction, it enters the final reduction kettle for condensation polymerization at a temperature of 275-285°C. The flow promoter monomer tetradecyl trimellitate is added to the melt line side of the final reduction kettle outlet using an online addition technology - screw plasticization method. The screw plasticization temperature is 120°C. The amount of flow promoter monomer added is 0.12% of the total amount of polyester. It is fully mixed with the polymer and then enters the granulation system for granulation and packaging. After drying and pre-crystallization at 180°C for 4 hours, medical polyester chips are obtained. The measured relevant index data are shown in the following table.

[0037] Embodiment 4:

[0038] (1) Using C16-18 alcohol and phosphoric acid in a molar ratio of 3:1 as raw material b, heating to 90° C. in the presence of a concentrated sulfuric acid catalyst in an amount of 0.1 wt % of raw material b, and refluxing for 30 min to prepare a flow promoter monomer, cetostearyl alcohol phosphate C16-18P;

[0039] (2) On a polyester production line, purified terephthalic acid and ethylene glycol are used as raw materials, ethylene glycol antimony is used as a polymerization catalyst, red and blue toners, and phosphoric acid heat stabilizer are mixed into a slurry and fed into an esterification kettle, wherein the molar ratio of purified terephthalic acid to ethylene glycol is 1:1.2; the amount of ethylene glycol antimony added is 180 μg / g of the total amount of polyester; the amounts of redness agent and blueness agent added are 0.6 μg / g and 1.4 μg / g of the total amount of polyester, respectively; and the amount of phosphoric acid heat stabilizer added is 15 μg / g of the total amount of polyester. The esterification reaction temperature is 220-260°C. After the esterification reaction, it enters the final reduction kettle for polycondensation reaction at a polycondensation temperature of 275-285°C. The flow promoter C16-18P is added to the melt line side of the final reduction kettle outlet using an online addition technology - screw plasticization method. The screw plasticization temperature is 70°C, and the amount of flow promoter monomer added is 0.2% of the total amount of polyester. It is fully stirred with the polymer and then enters the granulation system for granulation and packaging. After drying and pre-crystallization at 180°C for 4 hours, medical polyester chips are obtained. The measured relevant index data are as shown in the following table.

[0040] Embodiment 5:

[0041] (1) Using C20-22 alcohol and phosphoric acid in a molar ratio of 3:1 as raw material b, heating to 80° C. in the presence of a concentrated sulfuric acid catalyst in an amount of 0.06 wt % of raw material b, and refluxing for 1 h to obtain a flow promoter monomer C20-22 alcohol phosphate C20-22P;

[0042] (2) On a polyester production line, purified terephthalic acid and ethylene glycol are used as raw materials, ethylene glycol antimony is used as a polymerization catalyst, red and blue toners, and phosphoric acid heat stabilizer are mixed into a slurry and fed into an esterification kettle, wherein the molar ratio of purified terephthalic acid to ethylene glycol is 1:1.2; the amount of ethylene glycol antimony added is 180 μg / g of the total amount of polyester; the amounts of redness agent and blueness agent added are 0.6 μg / g and 1.4 μg / g of the total amount of polyester, respectively; and the amount of phosphoric acid heat stabilizer added is 15 μg / g of the total amount of polyester. The esterification reaction temperature is 220-260°C. After the esterification reaction, it enters the final reduction kettle for condensation polymerization, and the condensation polymerization temperature is 275-285°C. The flow promoter C20-22 alcohol phosphate C20-22P is added at the side end of the melt pipeline at the outlet of the final reduction kettle by using the online addition technology-screw plasticization method. The screw plasticization temperature is 70°C, and the amount of flow promoter monomer added is 0.02% of the total amount of polyester. It is fully stirred with the polymer and then enters the granulation system for granulation and packaging. After drying and pre-crystallization at 180°C for 4 hours, medical polyester chips are obtained. The measured relevant index data are as shown in the following table.

[0043] Embodiment 6:

[0044] On the polyester production line, purified terephthalic acid and ethylene glycol are used as raw materials, ethylene glycol antimony is used as a polymerization catalyst, red and blue colorants, and phosphoric acid heat stabilizer are mixed into a slurry and fed into an esterification kettle, and the molar ratio of purified terephthalic acid to ethylene glycol is 1:1.2; the added amount of ethylene glycol antimony is 180μg / g of the total amount of polyester; the added amounts of redness agent and blueness agent account for 0.6μg / g and 1.4μg / g of the total amount of polyester respectively; the added amount of phosphoric acid heat stabilizer is 15μg / g of the total amount of polyester. The esterification reaction temperature is 220-260°C. After the esterification reaction, the product enters the final reduction kettle for polycondensation reaction at a temperature of 275-285°C. The flow promoter monomer cetostearyl alcohol is added to the melt line side of the final reduction kettle outlet using an online addition technology - screw plasticization method. The screw plasticization temperature is 70°C. The amount of flow promoter monomer added is 0.15% of the total amount of polyester. The product is fully stirred with the polymer and then enters the granulation system for granulation and packaging. After drying and pre-crystallization at 180°C for 4 hours, medical polyester chips are obtained. The measured relevant index data are as shown in the following table.

[0045]

[0046] Note: The relevant index data test refers to the polyester test standard (GB / T14190-2009) and the disposable human venous blood sample collection container standard (YY0314-2007), where the melt index test conditions are 280℃ and the load is 2.16Kg.

Claims

1. A method for preparing medical polyester, characterized in that: The method uses dibasic acid and diol as raw materials b, mixes raw materials b, polymerization catalyst, toner and phosphorus stabilizer into slurry, puts into esterification kettle, after esterification reaction, enters final reduction kettle for polycondensation reaction, adds flow promoter at the side end of melt pipeline at the outlet of final reduction kettle and mixes with polymer thoroughly and evenly, and obtains polyester chips with characteristic viscosity of 0.55-0.70dL / g; The flow promoter is prepared by the following method: using fatty alcohol and tricarboxylic acid as raw materials a, carrying out esterification reaction under the condition of acidic catalyst to obtain the flow promoter; the fatty alcohol is at least one of octadecyl alcohol, hexadecanol, tetracosanol, C16-18 alcohol and C20-22 alcohol; The tricarboxylic acid is trimellitic anhydride, phosphoric acid or citric acid, and the molar ratio of the fatty alcohol to the tricarboxylic acid is 1-8:

1.

2. The preparation method according to claim 1, characterized in that: The molar ratio of fatty alcohol to tricarboxylic acid is 2-5:

1.

3. The preparation method according to claim 1, characterized in that: The acidic catalyst is concentrated sulfuric acid, and the amount of the catalyst used is 0.01%-3% of the raw material a.

4. The preparation method according to claim 1, characterized in that: The added amount of the flow promoter monomer is 0.02%-0.4% by weight of the medical polyester material.

5. A medical polyester according to claim 1, characterized in that: The medical polyester is prepared by the following method: With dibasic acid and diol as raw material b, raw material b, polymerization catalyst, colorant and phosphorus stabilizer are prepared into slurry and put into esterification kettle. After esterification reaction, it enters into final reduction kettle for polycondensation reaction. Flow promoter is added to the side end of melt pipeline at the outlet of final reduction kettle and mixed with polymer thoroughly and evenly, and polyester chips with characteristic viscosity of 0.55-0.70dL / g are obtained.

Citation Information

Patent Citations

  • Polyester slices for manufacturing vacuum blood collection tube and preparation method of polyester slices

    CN104017338A

  • Medical modified polyester masterbatch and preparation method thereof

    CN104448720A

  • Production technology of novel medical section

    CN105860038A

  • Polyester chip masterbatch for blood sampling tube, preparation method and application

    CN106589857A

  • Method for preparing titanium catalyst polyester

    CN101104678A