Water-based release agent for die casting
By using layered silicate minerals of more than 0.005 wt% but less than 5 wt% in the aqueous release agent, especially smectite, the problem of decomposition and gasification of the aqueous release agent at high temperature is solved, and the low speed is achieved Excellent molten metal insulation and productivity improvement in high-speed die casting.
Patent Information
- Application Number
- CN202180027539.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-04-10
- Filing Date
- 2021-04-08
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-04-08
AI Technical Summary
The existing aqueous mold release agents tend to decompose and gasify at high temperatures, resulting in a decrease in the insulation of molten metals, and the productivity and operating environment are difficult to improve in low-speed/high-speed die casting.
Use layered silicate minerals with a height of more than 0.005 wt% but less than 5 wt%, especially smectite, as a dispersant, and the particle size is controlled below 0.1 μm to ensure stable dispersion in water, prevent settlement and accumulation, and at high temperatures Maintain stability underneath.
Excellent molten metal flowability and thermal insulation in low-speed/high-speed die casting are achieved, preventing sticking molds and bubbles, improving productivity and operating environment stability, and convenient redispersion after drying, reducing mechanical dirt accumulation.
Smart Images

Figure CN115485081B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an aqueous mold release agent for low-speed / high-speed die casting, and more particularly to an aqueous mold release agent having excellent molten metal heat retention and low accumulation properties and excellent operating environment maintenance. Background Art
[0002] In die casting such as aluminum die casting, in order to prevent the welding of the mold and the casting formed by solidification of the molten metal and to easily remove the casting from the mold without damaging it, a release agent is applied to the molding surface of the mold in each molding cycle. The release agent is roughly divided into water-based type (dispersion medium: water), oily type (dispersion medium: hydrocarbon liquid), and powder type (solvent-free) according to the presence or type of dispersion medium. In any type of release agent, waxes, esters, silicone oils, etc. with high heat resistance are contained as lubricating components. In addition, in order to impart higher heat resistance, inorganic lubricating materials such as graphite, talc, and mica are sometimes used as solid lubricants.
[0003] Among release agents, oil-based release agents are generally said to have excellent release properties, but they are limited in the cases where they can be used due to the risk of smoke or fire. Powder-based release agents reduce waste such as waste water and waste liquid, but they have problems such as not being able to cool the mold with the release agent, not being able to easily adjust the concentration of the release agent, and requiring special coating equipment. On the other hand, water-based release agents are currently the most commonly used die-casting release agents because they are easy to apply and can cool the mold while applying.
[0004] As for the aqueous mold release agent for die casting, Patent Document 1 discloses an aqueous mold release agent for low-speed injection mold casting, which is obtained by combining a specific clay mineral with thixotropy and a specific high molecular weight organic compound, and adding a dispersant with an ionic repulsive effect to the compound together with water. The above-mentioned specific clay mineral is generally expected to improve the heat retention of molten metal and is effective in ensuring the fluidity of molten metal. In addition, the generation of gas is also small, which is also effective in ensuring the internal quality.
[0005] However, clay minerals generally have low dispersibility in water and many disadvantages in terms of stability. Specifically, problems such as high sedimentation velocity, accumulation in pipes, or nozzle clogging, etc., are prone to occur in terms of maintenance or production efficiency. In addition, although the specific high molecular weight organic compounds or dispersants described in Patent Document 1 contribute to the stable dispersion of clay minerals in the stock solution state, their effect is significantly reduced after dilution with water as the actual form of use, and thus the above-mentioned problems cannot be solved. It is further believed that these high molecular weight organic compounds or dispersants are more likely to undergo thermal decomposition and gasification when in contact with high-temperature molten metal, which will become a cause of reduced internal quality.
[0006] Therefore, mold release agents containing clay minerals are generally used only in fields where heat retention of molten metal is primarily required, particularly in low-speed die casting and the like.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent No. 4464214 Summary of the invention
[0010] Technical problem to be solved by the invention
[0011] As described above, in order to utilize the characteristics of water-based mold release agents, in order to respond to new alloy types such as high-functional alloys that have been actively developed in recent years, to adapt to new manufacturing methods such as low-speed die casting methods for the purpose of improving the internal quality of products, or to respond to the requirements of precision casting manufacturing processes that require efficient molding of more complex shapes in recent years, water-based mold release agents that use a combination of inorganic lubricants or high molecular weight organic compounds have been proposed.
[0012] An object of the present invention is to provide a die casting release agent which has excellent molten metal heat retention and can improve productivity and operating environment and can be used in both low-speed and high-speed die casting.
[0013] Means for solving technical problems
[0014] In the aqueous die-casting release agent of the present invention, a specific layered silicate mineral is dispersed at a concentration of 0.005 wt% or more and less than 5 wt%, and the particle size of the layered silicate mineral when dispersed is 0.1 μm or less.
[0015] The layered silicate mineral is preferably a smectite-based mineral.
[0016] Effects of the Invention
[0017] The water-based release agent of the present invention is characterized in that it is formulated with a specific layered silicate mineral that can be stably and transparently dispersed in water, and can maintain a stable solution state in the original liquid state and the diluted liquid state without the use of a dispersant that may cause the internal quality to deteriorate due to gasification. Thus, the release agent film formed by applying the water-based release agent of the present invention to the mold can achieve more excellent molten metal fluidity due to the good molten metal heat retention from the specific layered silicate mineral, can prevent sticking due to its high heat resistance, and can prevent internal quality degradation such as bubbles or lumps due to the suppression of gas generation. At the same time, the water-based release agent of the present invention prevents sedimentation, accumulation, etc. from occurring in the piping by achieving a stable solution state, which helps to improve productivity / operability. Furthermore, the water-based release agent of the present invention can suppress the accumulation of dirt around the machine because it is also easily redispersed in water after drying.
[0018] Due to the above effects, the aqueous mold release agent of the present invention can simultaneously achieve high product quality and manufacturing efficiency, and can be preferably used in both high-speed and low-speed die casting. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 A schematic diagram illustrating the steps of evaluating thermal insulation properties.
[0020] Figure 2 This is a schematic diagram for explaining the steps of evaluating the releasability. DETAILED DESCRIPTION
[0021] Hereinafter, the aqueous mold release agent for die casting of the present invention will be described in detail.
[0022] In the aqueous die-casting release agent of the present invention (hereinafter simply referred to as "aqueous die-casting release agent"), a layered silicate mineral is dispersed at a concentration of 0.005 wt% or more and less than 5 wt%, and the particle size of the layered silicate mineral when dispersed is 0.1 μm or less.
[0023] Layered silicate minerals are the main component minerals of clay minerals and are formed of fine particles. Layered silicate minerals include kaolinite, pyrophyllite, smectite (saponite, hectorite, stevensite, beidellite, etc.), vermiculite, mica clay minerals (illite and sericite), talc, glauconite, and chlorite.
[0024] Clay minerals include, in addition to the above-mentioned layered silicate minerals, crystalline aluminosilicates having fine pores such as zeolite, and hydrous magnesium silicates having a chain structure such as sepiolite.
[0025] Table 1 shows the properties of 1% aqueous dispersions prepared by dispersing smectite and talc as layered silicate minerals and sepiolite as a chain clay mineral in water.
[0026] In a 1% aqueous dispersion of hectorite and stevensite, microparticles with a particle size of less than 0.05 μm obtained by MICROTRACK UPA were dispersed in water, showing a high transparency of 90% with a transmittance obtained by a haze meter (HGH-2DP). In soapstone, the particle size when dispersed in water was 0.05 to 0.1 μm, which was slightly larger than the particle size of hectorite and stevensite, and showed a high transparency of 90% with a transmittance.
[0027] On the other hand, when montmorillonite is dispersed in water, the particle size during dispersion exceeds 1 μm and the transmittance is less than 50%, which is worse than that of hectorite, stevensite and saponite. Even a 1% aqueous dispersion of sepiolite or talc with a particle size of more than 1 μm has a transmittance of less than 50% and poor transparency due to precipitation or turbidity.
[0028] Table 1
[0029]
[0030] Particle size at 1% dispersion: AA: less than 0.05 μm, A: 0.05 μm or more and less than 0.1 μm, B: 0.1 μm or more and less than 1 μm, C: 1 μm or more
[0031] Transmittance (%) AA: 90% or more, A: 70% or more and less than 90%, B: 50% or more and less than 70%, C: less than 50%
[0032] Thermal insulation AA: less than 140°C, A: 140°C or more and less than 160°C, B: 160°C or more and less than 180°C, C: 180°C or more
[0033] Stability (3 months at room temperature) A: no separation, B: turbidity, C: sedimentation / precipitation
[0034] As shown in Table 1, the layered silicate mineral of the present invention has a layered structure and a particle size of 0.1 μm or less when dispersed. Clay minerals with a layered structure have a large cation exchange capacity due to isomorphous substitution of metal ions and negative charge on the layer itself. When such layered clay minerals are dispersed in water, they swell due to changes in surface charge distribution, etc., and form a stable colloidal solution-like dispersion. The hectorite, saponite and stevensite in Table 1 show high transmittance and form a stable dispersion.
[0035] On the other hand, in the case of layered silicate compounds such as chain clay minerals or talc having low transmittance when dispersed in water and having a particle size exceeding 0.1 μm when dispersed, precipitation and settling over time are inevitable, and this precipitation and settling eventually occurs in piping, etc., causing accumulation or nozzle clogging.
[0036] The layered silicate mineral of the present invention is more preferably kaolinite, pyrophyllite, smectite (saponite, hectorite, stevensite and beidellite, etc.), vermiculite, mica clay minerals, glauconite and chlorite, and is further preferably smectite, and particularly preferably saponite, hectorite and stevensite among smectites.
[0037] The aqueous release agent contains the layered silicate mineral at a concentration of 0.005 wt % or more and less than 5 wt %, preferably 0.05 to 3 wt %.
[0038] When the layered silicate mineral of the present invention is dispersed in water, the particle size of the layered silicate mineral in the aqueous dispersion is 0.1 μm or less, preferably 0.05 μm or less. The finer the particles of the layered silicate mineral in water, the easier it is to disperse, and the better it is in preventing precipitation or sedimentation, and therefore it is suitable for the present invention.
[0039] For example, when hectorite is added to water, the hectorite becomes small particles to the extent that the particles are almost invisible and enters the water, and the aqueous dispersion presents a transparent solution. Even if the aqueous dispersion becomes a dry film by evaporation of water, it is dispersed again when water is injected, so it is advantageous in preventing nozzle clogging. Even if the aqueous dispersion is prepared for more than 2 months, the state does not change, and no precipitation or sedimentation is seen. In addition, since hectorite is an inorganic powder, it will not be thermally decomposed even at a temperature equivalent to 650 to 720°C of molten metal. Furthermore, since the film formed by the aqueous release agent formed on the entire contact surface between the mold and the molten metal contains hectorite that is difficult to thermally decompose, the film formed by the aqueous release agent is formed on the entire contact surface between the mold and the molten metal, and the mold and the molten metal will not directly contact, which has the effect of preventing sticking.
[0040] The aqueous release agent contains the layered silicate mineral and water. The water used may be tap water, distilled water, ion-exchanged water, pure water, or the like.
[0041] The aqueous release agent may contain, in addition to the above-mentioned layered silicate mineral, a release component, a dispersant component, and other additive components contained in a general aqueous release agent within a range not impairing the effects of the present invention.
[0042] Examples of mold release components include organosilicon compounds, waxes, mineral oils, fats and synthetic oils. Examples of the organosilicon compounds include organosilicon oils. Examples of waxes include petroleum waxes such as paraffin wax, olefin wax, polyethylene wax and polypropylene wax; oxidized waxes such as oxidized polyethylene wax and oxidized polypropylene; and natural waxes such as beeswax, carnauba wax and montan wax. Examples of fats and oils include animal oils and vegetable oils. Examples of synthetic oils include polybutene and polyester. The mold release components may be used alone or in combination of two or more.
[0043] As long as the above-mentioned dispersant component can emulsify and disperse the above-mentioned demoulding component in water, any of ionic surfactants (anionic, cationic and amphoteric surfactants) and nonionic surfactants can be used, but nonionic surfactants and anionic surfactants are preferred. The above-mentioned nonionic surfactants are, for example, polyoxyalkylene glycols, polyoxyalkylene alkyl ethers, polyoxyalkylene allyl ethers and polyoxyethylene sorbitan monooleate. The above-mentioned anionic surfactants are, for example, fatty acid soaps, alkyl / allyl sulfonates, etc. The above-mentioned dispersant components can be used alone or in combination of two or more.
[0044] The content of the dispersant component may be such that the release component can be emulsified and dispersed in water, and is, for example, 5 to 20 parts by mass, preferably 10 to 15 parts by mass, based on 100 parts by mass of the release agent component.
[0045] Other additive ingredients include defoamers, corrosion inhibitors, preservatives, rust inhibitors, viscosity enhancers and antioxidants.
[0046] The method for producing the aqueous release agent of the present invention is not particularly limited, and it can be preferably produced by, for example, adding a layered silicate mineral to a solution of a dispersant component dissolved in water and uniformly mixing the mixture, and further adding a release component such as an organosilicon compound and uniformly mixing the mixture.
[0047] The aqueous mold release agent of the present invention can be used for extrusion die casting, laminar flow (low speed) die casting, general die casting, and the like, and can be used in any of the above types.
[0048] The raw materials for die casting are non-ferrous metals such as aluminum, zinc, and magnesium, and their alloys. Die casting can be preferably used to manufacture automobile parts using, for example, aluminum alloys.
[0049] Example
[0050] Hereinafter, the present invention will be described in more detail based on Examples and Comparative Examples, but the present invention is not limited to these Examples and the like.
[0051] [Preparation of water-based release agent]
[0052] According to Examples 1 to 9 and Comparative Examples 1 to 7, water-based release agents were prepared.
[0053] [Evaluation of water-based release agents]
[0054] (1) Stability
[0055] After the aqueous mold release agent was left to stand at room temperature for 6 months, it was evaluated visually.
[0056] When no turbidity or sediment was observed, it was rated as good (A), when precipitates were observed, it was rated as fair (B), and when sedimentation or two-layer separation occurred, it was rated as bad (C). In addition, a relative evaluation was performed using the stability of the aqueous release agent of Comparative Example 7 prepared by diluting the silicone emulsion 5 times with water as the reference (A).
[0057] In addition, the stability of the diluted solution prepared by diluting the aqueous release agent as the stock solution by 50 times was visually evaluated in the same manner as above. In the case of dilution, the solution was left to stand for 3 days before evaluation.
[0058] (2) Thermal insulation
[0059] use Figure 1 The device shown evaluates the thermal insulation, i.e., the heat preservation of molten metal, as follows. A steel plate with a built-in thermocouple 2 mm below the surface is heated to 300°C and a water-based mold release agent is sprayed. Thereafter, 100 ml of molten metal of an aluminum alloy (ADC12 described in JIS K2219) at 680°C is supplied to the ring set on the steel plate. The temperature change shown by the thermocouple at this time is measured. The test conditions are shown in Table 2.
[0060] Table 2
[0061] Coating amount (ml) 0.2 Spray nozzle-steel plate distance (mm) 200 Steel plate material SKD61 Steel plate shape 200×200×30 Steel plate temperature (℃) 300 Alloy material ADC12 Molten metal temperature (℃) 680 Molten metal volume (ml) 100
[0062] The case where the temperature rise was less than 140°C was rated as excellent (AA), the case where it was 140°C or more and less than 160°C was rated as good (A), the case where it was 160°C or more and less than 180°C was rated as fair (B), and the case where it was 180°C or more was rated as poor (C).
[0063] (3) Mold release
[0064] When the mold temperature becomes high, the adhesion film is thermally decomposed and disappears, the adhesion efficiency is extremely reduced, and the molten metal comes into direct contact with the mold, causing mold sticking. Therefore, the Lub tester was used to test whether mold sticking occurred when the temperature of the steel plate coated with the water-based release agent was set to 350°C. Table 3 shows the test conditions, Figure 2 The test method is shown in .
[0065] Table 3
[0066] Coating amount (ml) 0.2 Spray nozzle-steel plate distance (mm) 200 Steel plate material SKD61 Steel plate shape 200×200×30 Steel plate temperature (℃) 350 Alloy material ADC12 Molten metal temperature (℃) 680 Molten metal volume (ml) 100
[0067] The case where no sticking was observed at 350° C. was rated as good (A), and the case where sticking was observed was rated as bad (C). Relative evaluation was performed using the releasability of the aqueous release agent of Comparative Example 7 as a reference (C).
[0068] [Example 1]
[0069] 0.05 parts by mass of hectorite, 20 parts by mass of a silicone emulsion (manufactured by Asahi Kasei Wacker Silicone Co., Ltd.; NR2707), and 79.95 parts by mass of water were mixed to prepare an aqueous release agent.
[0070] The obtained aqueous release agent was evaluated for stability, heat insulation, and release properties.
[0071] The results are shown in Table 4.
[0072] [Example 2]
[0073] An aqueous release agent was prepared in the same manner as in Example 1, except that saponite was used instead of hectorite.
[0074] The obtained aqueous release agent was evaluated in the same manner as in Example 1.
[0075] The results are shown in Table 4.
[0076] [Example 3]
[0077] A water-based release agent was prepared in the same manner as in Example 1, except that stevenstone was used instead of hectorite.
[0078] The aqueous release agent was evaluated in the same manner as in Example 1.
[0079] The results are shown in Table 4.
[0080] [Example 4]
[0081] 1 part by mass of hectorite, 20 parts by mass of silicone emulsion (NR2707 manufactured by Asahi Kasei Wacker Silicone Co., Ltd.), and 79 parts by mass of water were mixed to prepare an aqueous release agent.
[0082] The aqueous release agent was evaluated in the same manner as in Example 1.
[0083] The results are shown in Table 4.
[0084] [Example 5]
[0085] An aqueous release agent was prepared in the same manner as in Example 4, except that saponite was used instead of hectorite.
[0086] The aqueous release agent was evaluated in the same manner as in Example 1.
[0087] The results are shown in Table 4.
[0088] [Example 6]
[0089] An aqueous release agent was prepared in the same manner as in Example 4, except that stevenstone was used instead of hectorite.
[0090] The aqueous release agent was evaluated in the same manner as in Example 1.
[0091] The results are shown in Table 4.
[0092] [Example 7]
[0093] 3 parts by mass of hectorite, 20 parts by mass of a silicone emulsion (manufactured by Asahi Kasei Wacker Silicone Co., Ltd.; NR2707), and 77 parts by mass of water were mixed to prepare an aqueous release agent.
[0094] The aqueous release agent was evaluated in the same manner as in Example 1.
[0095] The results are shown in Table 4.
[0096] [Example 8]
[0097] An aqueous release agent was prepared in the same manner as in Example 7, except that saponite was used instead of hectorite.
[0098] The aqueous release agent was evaluated in the same manner as in Example 1.
[0099] The results are shown in Table 4.
[0100] [Example 9]
[0101] An aqueous release agent was prepared in the same manner as in Example 7, except that stevenstone was used instead of hectorite.
[0102] The aqueous release agent was evaluated in the same manner as in Example 1.
[0103] The results are shown in Table 4.
[0104] The stability, heat insulation and release properties of the aqueous release agents of Examples 1 to 9 were good. In particular, Examples 7 to 9 were excellent in heat insulation because the amount of layered silicate mineral added was large.
[0105] [Comparative Example 1]
[0106] An aqueous release agent was prepared by mixing 1 part by mass of montmorillonite, 20 parts by mass of a silicone emulsion (NR2707, manufactured by Asahi Kasei Wacker Silicone Co., Ltd.), 1 part by mass of a dispersant (CMC, manufactured by Nippon Paper Chemicals Co., Ltd.; F-20HC), 1 part by mass of a surfactant (XL70, manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.), and 77 parts by mass of water.
[0107] The obtained aqueous release agent was evaluated in the same manner as in Example 1.
[0108] The results are shown in Table 4. Since montmorillonite is swellable, when it comes into contact with water, the interlayer cations react with water molecules to increase the viscosity. However, the dispersed montmorillonite settles over time, so the stability is poor.
[0109] [Comparative Example 2]
[0110] A water-based mold release agent was prepared in the same manner as in Comparative Example 1, except that sepiolite (manufactured by Sepio Japan Co., Ltd.; Milcon SP2) was used instead of montmorillonite.
[0111] The aqueous release agent was evaluated in the same manner as in Example 1.
[0112] The results are shown in Table 4. When sepiolite having a unique chain-like fibrous morphology is dispersed in water, it exhibits thixotropy. However, since sepiolite settles over time, its stability is poor.
[0113] [Comparative Example 3]
[0114] An aqueous release agent was prepared in the same manner as in Comparative Example 1, except that talc (manufactured by Nippon Talc Co., Ltd.; Micro-ace P-4) was used instead of montmorillonite.
[0115] The aqueous release agent was evaluated in the same manner as in Example 1.
[0116] The results are shown in Table 4. Since talc has a particle size exceeding 0.1 μm when dispersed and is water-insoluble, the stability and transparency of its aqueous dispersion are poor.
[0117] [Comparative Example 4]
[0118] 5 parts by mass of hectorite, 20 parts by mass of a silicone emulsion (manufactured by Asahi Kasei Wacker Silicone Co., Ltd.; NR2707), and 75 parts by mass of water were mixed to prepare an aqueous release agent.
[0119] The aqueous release agent was evaluated in the same manner as in Example 1.
[0120] The results are shown in Table 4. Since the amount of hectorite, a layered silicate mineral, added was large, excellent heat insulation properties were exhibited, but significant gelation occurred, resulting in two-layer separation from the silicone emulsion.
[0121] [Comparative Example 5]
[0122] An aqueous release agent was prepared in the same manner as in Comparative Example 4, except that saponite was used instead of hectorite.
[0123] The aqueous release agent was evaluated in the same manner as in Example 1.
[0124] The results are shown in Table 4. Since the amount of soapstone added was large, excellent heat insulation properties were exhibited, but significant gelation occurred over time and stability was poor.
[0125] [Comparative Example 6]
[0126] An aqueous release agent was prepared in the same manner as in Comparative Example 4, except that stevenstone was used instead of hectorite.
[0127] The aqueous release agent was evaluated in the same manner as in Example 1.
[0128] The results are shown in Table 4. Since the amount of stevensite added was large, excellent heat insulation properties were exhibited, but significant gelation occurred over time and stability was poor.
[0129] [Comparative Example 7]
[0130] 20 parts by mass of a silicone emulsion (manufactured by Asahi Kasei Wacker Silicone Co., Ltd.; NR2707) and 80 parts by mass of water were mixed to prepare an aqueous release agent, and the obtained aqueous release agent was evaluated in the same manner as in Example 1.
[0131] The results are shown in Table 4.
[0132]
Claims
1. A water-based mold release agent for die casting, characterized in that: The montmorillonite-based layered silicate mineral is dispersed at a concentration of 0.005wt% or more and less than 5wt%, the particle size of the montmorillonite-based layered silicate mineral when dispersed is less than 0.1μm, the montmorillonite-based layered silicate mineral is saponite, hectorite or stevensite, and does not contain solid components other than the montmorillonite-based layered silicate mineral.