A spiral hole transport material and its preparation method and application
By designing and developing spiral hole transport materials, we have solved the problems of difficult synthesis, high cost and low efficiency of Spiro-OMeTAD in perovskite solar cells, achieved efficient and stable hole transport performance, and improved the perovskite solar energy Battery efficiency and stability.
Patent Information
- Application Number
- CN202211249768.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-12
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-10-12
AI Technical Summary
The hole transport material Spiro-OMeTAD used in existing perovskite solar cells is difficult to synthesize, has high cost, and has low intrinsic hole mobility. Dopants are needed to improve conductivity, but dopants will reduce device life and affect Efficiency and stability.
Design and develop a spiral hole transport material with excellent solubility, controllable energy levels and high hole mobility. It is prepared through the coupling reaction of compound A and compound B to form a spiral hole transport material with excellent hole transport performance and interface characteristics. Materials used in perovskite solar cells.
It improves the efficiency and stability of perovskite solar cells, provides superior hole transport performance and interface characteristics compared with traditional hole transport materials, reduces production costs, and extends device life.
Smart Images

Figure CN115490632B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solar cells, and in particular relates to a hole transport material and a preparation method and application thereof. Background Art
[0002] In recent years, perovskite solar cells with organic-inorganic hybrid perovskite materials as "light absorbers" have achieved rapid development, and their recently verified efficiency has exceeded 25%, comparable to traditional silicon-based solar cells. In addition to the active layer perovskite, the hole transport material in perovskite solar cells also has a crucial impact on its efficiency and stability. Its energy level structure, hole mobility, film morphology and interface properties all have an important impact on the extraction, transfer, transmission and recombination of holes, thereby affecting the performance of the final device.
[0003] At present, the most widely used and universal hole transport material in normal perovskite cells is Spiro-OMeTAD. However, its synthesis and purification are relatively difficult, the cost is high, and the intrinsic hole mobility is low. Dopants are required to improve the conductivity of the hole transport layer, and the introduction of dopants will reduce the life of the device. Therefore, the design and development of hole transport materials with energy level matching and high hole mobility are of great significance to improving the efficiency and stability of perovskite solar cells. Summary of the invention
[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a hole transport material and a preparation method and application thereof. The hole transport material has excellent solubility, adjustable energy level, hole mobility and film morphology, and more superior hole transport performance and interface characteristics than the traditional hole transport material Spiro-OMeTAD, and can be applied to perovskite solar cells.
[0005] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0006] In a first aspect, the present invention provides a spiro-type hole transport material having a structure as shown in Formula I:
[0007]
[0008] Formula I;
[0009] Wherein, the D1 group and the D2 group are donor unit groups.
[0010] Preferably, the donor unit group D1 is selected from any one of the donor unit groups shown in the following structure:
[0011]
[0012] ;
[0013] Wherein, the R groups are independently selected from hydrogen, methyl, methoxy, 2-methoxyethoxy, methylthio, tert-butyl or vinyl, and the dotted line on N indicates the group connection position.
[0014] Preferably, the donor unit group D2 is selected from any one of the donor unit groups shown in the following structures and is not the same as the D1 group:
[0015]
[0016]
[0017] ;
[0018] Wherein, the R groups are independently selected from hydrogen, methyl, methoxy, 2-methoxyethoxy, methylthio, tert-butyl or vinyl, and the dotted line on N indicates the group connection position.
[0019] Preferably, the hole transport material is selected from any one of the following compounds:
[0020]
[0021]
[0022] In a second aspect, the present invention provides a method for preparing the hole interface material according to the first aspect, the preparation method comprising the following steps:
[0023] (1) Compound A and compound B undergo coupling reaction to obtain compound C. The reaction formula is as follows:
[0024] ;
[0025] (2) Compound C and compound E undergo a coupling reaction to obtain a compound represented by formula I. The reaction formula is as follows:
[0026] ;
[0027] Wherein, the donor unit group D1 is selected from any one of the donor unit groups shown in the following structure:
[0028]
[0029] ;
[0030] Wherein, the donor unit group D2 is selected from any one of the donor unit groups shown in the following structures and is not the same as D1:
[0031]
[0032] Preferably, the palladium catalyst in step (1) is Pd(OAc)2;
[0033] Preferably, in step (1), the molar mass ratio of compound A to compound B is 1:2;
[0034] Preferably, the solvent for the coupling reaction in step (1) is toluene;
[0035] Preferably, the temperature of the coupling reaction in step (1) is 90-100°C, for example, 90°C or 100°C;
[0036] Preferably, the coupling reaction time in step (1) is 20-24 h, for example, 20 h, 21 h, 22 h, 23 h, 24 h;
[0037] Preferably, the catalyst for the coupling reaction in step (2) is Pd(OAc)2;
[0038] Preferably, in step (2), the molar mass ratio of compound C to compound E is 1:(2.1-2.4), for example, 1:2.1, 1:2.2, 1:2.3, 1:2.4;
[0039] Preferably, the solvent for the coupling reaction in step (2) is toluene;
[0040] Preferably, the temperature of the coupling reaction in step (2) is 100-120°C, for example, 100°C, 110°C, 120°C;
[0041] Preferably, the coupling reaction time in step (2) is 20-24 h, for example, 20 h, 21 h, 22 h, 23 h, or 24 h.
[0042] In a third aspect, the present invention provides a use of the hole transport material as described in the first aspect in preparing solar cell materials;
[0043] Preferably, the solar cell is a perovskite solar cell.
[0044] In a fourth aspect, the present invention provides a hole transport layer, wherein the hole transport layer comprises the hole transport material as described in the first aspect.
[0045] In a fifth aspect, the present invention provides a perovskite solar cell, wherein the perovskite solar cell comprises a hole transport layer as described in the fourth aspect.
[0046] Preferably, the perovskite solar cell comprises, from top to bottom, an anode electrode layer, a hole transport layer, a perovskite active layer, an electron transport layer and a cathode electrode layer.
[0047] Preferably, the anode electrode layer is a silver electrode.
[0048] Preferably, the thickness of the anode motor layer is 100-150 nm, for example, 100 nm, 110 nm, 120 nm, 130 nm, 140 nm, or 150 nm.
[0049] Preferably, the thickness of the hole transport layer is 80-120 nm, for example, 80 nm, 90 nm, 100 nm, 110 nm, or 120 nm.
[0050] Preferably, the perovskite active layer is CH3NH3PbI3, and its thickness is 400-600 nm, for example, it can be 400 nm, 420 nm, 440 nm, 460 nm, 480 nm, 500 nm, 520 nm, 540 nm, 560 nm, 580 nm, 600 nm.
[0051] Preferably, the electron transport layer is a TiO2 electron transport layer.
[0052] Preferably, the thickness of the electron transport layer is 40-60 nm, for example, 40 nm, 50 nm, or 60 nm.
[0053] Preferably, the cathode electrode is ITO conductive glass.
[0054] Preferably, the cathode electrode has a thickness of 150-180 nm, for example, 150 nm, 160 nm, 170 nm, or 180 nm.
[0055] Compared with the prior art, the present invention has the following beneficial effects:
[0056] The hole transport material of the present invention has excellent solubility, adjustable energy level, hole mobility and film morphology, and more superior hole transport performance and interface characteristics than the traditional hole transport material Spiro-OMeTAD, and can be applied to perovskite solar cells. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] Figure 1 It is a comparison chart of the electrochemical performance tests of the hole transport materials provided in Examples 1-5.
[0058] Figure 2 This is a comparison chart of the ultraviolet-visible absorption spectra of the hole transport materials provided in Examples 1-5. DETAILED DESCRIPTION
[0059] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0060] Example 1
[0061] This embodiment provides a hole transport material having a structure as shown in Formula I-1:
[0062]
[0063] Formula Ⅰ-1
[0064] Synthesis route of hole transport material Ⅰ-1:
[0065] (1) Synthesis of intermediate compound 1:
[0066] 2,7-Dibromo-2',7'-diiodospirobifluorene (150 mg, 0.2 mmol), bis(4-methoxyphenyl)amine (92 mg, 0.4 mmol), Pd(OAc)2 (1 mg, 0.004 mmol), tri-tert-butylphosphine (20 μL, 0.008 mmol), sodium tert-butoxide (58 mg, 0.6 mmol) were placed in a double-necked flask; after purging with argon three times, 5 mL of toluene was added; the reaction was carried out under argon protection; after reacting at 90°C for 24 h, the reaction system was cooled to room temperature after the reaction was completed, the solvent was spun off, and the crude product was purified by column to obtain the intermediate compound 1 with a mass of 101 mg and a yield of 55%.
[0067] 1 H NMR (400 MHz, CDCl3): δ 7.83 (d, J = 8.1 Hz, 2H), 7.64 (d, J = 8.0Hz, 2H), 7.56 (d, J = 8.1 Hz, 2H), 6.85-6.83 (m, 10H), 6.76-6.74 (m, 10H), 3.67 (s, 12H);
[0068] High resolution mass spectrometry: C 53 H 40Br2N2O4 Calculated value: 926.1355, Found: 926.1359 [M + ].
[0069] (2) Synthesis of hole transport material I-1:
[0070] The intermediate compound 1 (60 mg, 0.064 mmol) obtained in step (1), 3,6-dimethoxycarbazole (36 mg, 0.1536 mmol), Pd(OAc)2 (0.32 mg, 0.00128 mmol), tri-tert-butylphosphine (6.4 μL, 0.00256 mmol), and sodium tert-butoxide (18 mg, 0.192 mmol) were placed in a double-necked flask; after purging with argon three times, 4 mL of toluene was added; the reaction was carried out under argon protection; after reflux reaction for 24 h, the reaction system was cooled to room temperature after the reaction was completed, the solvent was spun off, and the crude product was purified by column to obtain hole transport material I-1 with a mass of 60 mg and a yield of 77%.
[0071] 1 H NMR (400 MHz, DMSO- d 6): δ 8.16 (d, J = 8.1 Hz, 2H), 7.83 (d, J =2.4 Hz, 4H), 7.63-7.60 (m, 4H), 7.13 (d, J = 8.9 Hz, 4H), 7.01 (dd, J = 8.9,2.4 Hz, 4H), 6.89-6.85 (m, 10H), 6.79 (dd, J = 8.4, 2.1 Hz, 2H), 6.73 (d, J =9.0 Hz, 8H), 6.32 (d, J = 2.1 Hz, 2H), 3.88 (s, 12H), 3.65 (s, 12H);
[0072] Elemental analysis calculated: C, 79.65; H, 5.28; N, 4.59, found: C, 79.95; H, 5.16;N, 4.78.
[0073] Example 2
[0074] This embodiment provides a hole transport material having a structure as shown in Formula I-2:
[0075]
[0076] Formula I-2
[0077] Synthesis route of hole interface material Ⅰ-2:
[0078]
[0079] Synthesis of hole transport material Ⅰ-2
[0080] The synthesis method of steps (1) and (2) is the same as that of the hole transport material I-1, except that the reactant in step (2) is changed from 3,6-dimethoxycarbazole to , yield 80%.
[0081] 1 H NMR (400 MHz, THF- d 8) δ 8.03 (dd, J = 8.1, 1.2 Hz, 2H), 6.85 (d, J= 1.9 Hz, 2H), 6.82 – 6.70 (m, 12H), 6.68 – 6.61 (m, 10H), 6.57 (dq, J = 6.9,3.1 Hz, 14H), 5.89 – 5.79 (m, 4H), 3.64 (d, J = 1.2 Hz, 12H);
[0082] Elemental analysis calculated values: C, 81.61; H, 4.98; N, 4.94, found values: C, 81.88; H, 4.77;N, 4.70.
[0083] MALDI-TOF mass spectrometry: C 77 H 56 N4O6 analysis value: 1132.4, measured value: 1132.4 [M + ].
[0084] Example 3
[0085] This embodiment provides a hole transport material having a structure as shown in Formula I-3:
[0086]
[0087] Formula I-3
[0088] Synthesis route of hole interface material I-3:
[0089]
[0090] Synthesis of hole transport material Ⅰ-3
[0091] The synthesis method of steps (1) and (2) is the same as that of the hole transport material I-1, except that the reactant in step (2) is changed from 3,6-dimethoxycarbazole to , yield 80%.
[0092] 1 H NMR (400MHz, CD2Cl2): δ 8.05 (d, J = 8.0 Hz, 2H), 7.43 (d, J = 9.4Hz, 4H), 7.05-6.99 (m, 10H), 6.92-6.85 (m, 14H), 6.72 (br, 10H), 6.20 (d, J =8.0 Hz, 4H), 3.77 (s, 12H);
[0093] Elemental analysis calculated: C, 79.36; H, 4.84; N, 4.81; S, 5.50 Found: C, 79.27;H, 4.95; N, 4.61; S, 5.32.
[0094] MALDI-TOF mass spectrometry: C 77 H 56 N4O4S2 analytical value: 1164.3, measured value: 1164.4 [M + ].
[0095] Example 4
[0096] This embodiment provides a hole transport material having a structure as shown in Formula I-4:
[0097]
[0098] Formula I-4
[0099] Synthesis route of hole interface material I-4:
[0100]
[0101] Synthesis of hole transport material Ⅰ-4
[0102] The synthesis method of steps (1) and (2) is the same as that of the hole transport material I-1, except that the reactant in step (2) is changed from 3,6-dimethoxycarbazole to , yield 65%.
[0103] 1 H NMR (400 MHz, THF- d8) δ 7.97 (d, J = 8.0 Hz, 2H), 6.93 – 6.85 (m,7H), 6.83 – 6.69 (m, 18H), 6.60 (dd, J = 13.3, 8.7 Hz, 10H), 6.54 – 6.48 (m,3H), 6.38 (d, J = 8.2 Hz, 5H), 3.64 (s, 12H);
[0104] Elemental analysis calculated: C, 73.44; H, 4.48; N, 4.45, Found: C, 73.72; H, 4.69;N, 4.23.
[0105] MALDI-TOF mass spectrometry: C 77 H 56 N4O4Se2 analysis value: 1260.2, measured value: 1260.3 [M + ].
[0106] Example 5
[0107] This embodiment provides a hole transport material having a structure as shown in Formula I-5:
[0108]
[0109] Formula I-5
[0110] Synthesis route of hole interface material I-5:
[0111]
[0112] Synthesis of hole transport material Ⅰ-5
[0113] The synthesis method of steps (1) and (2) is the same as that of the hole transport material I-1, except that the reactant in step (2) is changed from 3,6-dimethoxycarbazole to , yield 44%.
[0114] 1 H NMR (400 MHz, THF- d8) δ 8.22 (d, J = 8.0 Hz, 2H), 8.03 (dd, J =7.8, 1.6 Hz, 4H), 7.44 (dd, J = 8.1, 1.7 Hz, 4H), 7.37 (ddd, J = 8.7, 7.2,1.7 Hz, 4H), 7.27 – 7.18 (m, 4H), 7.02 (d, J = 1.9 Hz, 2H), 6.84 – 6.76 (m,8H), 6.74 (dd, J = 8.3, 2.1 Hz, 2H), 6.70 – 6.62 (m, 8H), 6.61 – 6.52 (m,6H), 3.67 (s, 12H);
[0115] Elemental analysis calculated: C, 75.23 H, 4.59; N, 4.56; S, 5.22 Found: C, 75.17; H,4.50; N, 4.48; S, 5.16.
[0116] MALDI-TOF mass spectrometry: C 77 H 56 N4O8S2 analytical value: 1228.3, measured value: 1228.4 [M + ].
[0117] Example 6
[0118] This embodiment provides a hole transport material having a structure as shown in Formula I-6:
[0119]
[0120] Formula I-6
[0121] Synthesis route of hole interface material I-6:
[0122]
[0123] Synthesis of hole transport material Ⅰ-6
[0124] The synthesis method of steps (1) and (2) is the same as that of the hole transport material I-1, except that the reactant in step (2) is changed from 3,6-dimethoxycarbazole to , yield 56%.
[0125] 1 H NMR (400 MHz, THF- d8) δ 7.78 (d, J = 8.5 Hz, 4H), 7.64 (d, J = 8.2Hz, 2H), 7.39 – 7.24 (m, 8H), 7.23 – 7.16 (m, 2H), 7.11 (dd, J = 7.4, 1.2 Hz, 2H), 6.88 – 6.81 (m, 8H), 6.80 – 6.60 (m, 18H), 6.60 – 6.44 (m, 7H), 3.68 (s,12H), 3.62 (d, J = 1.1 Hz, 6H);
[0126] MALDI-TOF mass spectrometry: C 87 H 68 N4O6 analysis value: 1264.5, measured value: 1264.5 [M + ].
[0127] Example 7
[0128] This embodiment provides a hole transport material having a structure as shown in Formula I-7:
[0129]
[0130] Formula I-7
[0131] Synthesis route of hole interface material I-7:
[0132]
[0133] (1) Synthesis of intermediate compound 2
[0134] 2,7-Dibromo-2',7'-diiodospirobifluorene (150 mg, 0.2 mmol), 3,6-dimethoxy-9H-carbazole (91 mg, 0.4 mmol), Pd(OAc)2 (1 mg, 0.004 mmol), tri-tert-butylphosphine (20 μL, 0.008 mmol), sodium tert-butoxide (58 mg, 0.6 mmol) were placed in a double-necked flask; after purging with argon three times, 5 mL of toluene was added; the reaction was carried out under argon protection; after reacting at 90°C for 24 h, the reaction system was cooled to room temperature after the reaction was completed, the solvent was spun off, and the crude product was purified by column to obtain the intermediate compound 2 with a mass of 140 mg and a yield of 77%.
[0135] 1 H NMR (400 MHz, CDCl3) δ 8.06 (d, J = 8.1 Hz, 2H), 7.64 (dd,J = 8.1,1.9 Hz, 2H), 7.59 (d, J = 8.2 Hz, 2H), 7.50-7.47 (m, 6H), 7.17 (s, 2H), 7.15(s, 2H), 7.08 (d, J = 1.8 Hz, 2H), 6.97 (d, J = 2.5 Hz, 2H), 6.95 (d, J = 2.5Hz, 2H), 6.92 (d, J = 1.9 Hz, 2H), 3.90 (s, 12H);
[0136] (2) Synthesis of hole transport material I-7
[0137] The synthesis method of hole transport material I-7 step (2) is the same as the synthesis of hole transport material I-1, and the yield of hole transport material I-7 is 42%.
[0138] 1 H NMR (400 MHz, THF- d 8) δ 7.92 (dd, J = 9.3, 4.5 Hz, 2H), 7.72 (dd, J= 16.5, 8.4 Hz, 5H), 7.63 – 7.55 (m, 6H), 7.52 – 7.46 (m, 2H), 7.41 (d, J =8.3 Hz, 2H), 7.26 (t, J = 7.8 Hz, 2H), 7.19 (d, J = 9.0 Hz, 6H), 7.12 – 7.07(m, 2H), 7.06 – 6.95 (m, 9H), 6.81 – 6.74 (m, 4H), 6.66 (dd, J = 8.3, 2.2 Hz,2H), 6.58 (dd, J = 8.5, 1.8 Hz, 6H), 3.86 (s, 12H), 3.59 (d, J = 1.5 Hz, 6H);
[0139] MALDI-TOF mass spectrometry: C 87 H 64 N4O6 analysis value: 1260.4, measured value: 1260.5[M + ].
[0140] The electrochemical performance of the hole transport materials provided in Examples 1 to 5 was tested as follows:
[0141] Its electrochemical performance was tested by CHI760 electrochemical workstation;
[0142] Figure 1 The electrochemical performance test comparison diagram of the hole transport materials provided in Examples 1-5 shows that the hole transport materials described in the present invention all show obvious redox peaks. The HOMO energy level of each hole transport material is calculated from the redox starting peak position. The specific test results are shown in Table 1:
[0143] Table 1
[0144]
[0145] It can be seen from the above test data that the HOMO energy level of the hole transport material provided in Examples 1-5 is -5.11~-5.16eV, indicating that the hole transport material of the present invention has an energy level that is relatively matched with the perovskite valence band, which is beneficial to the extraction and transfer of holes in the perovskite battery device.
[0146] The hole transport materials provided in Examples 1 to 5 were subjected to UV-visible absorption spectrum testing in the following manner:
[0147] Its performance was tested by Shimadzu UV-3600 UV-visible absorption spectrometer;
[0148] Figure 2 The ultraviolet-visible absorption spectrum comparison diagram of the hole transport material provided in Examples 1-5 shows that the hole transport material of the present invention mainly shows obvious absorption peaks around 320nm and 380nm. No absorption peak appears at the visible light wavelength, indicating that no absorption peak appears in the visible light range, indicating that the hole transport material of the present invention can avoid the absorption of visible light, which is beneficial to improve the light absorption of the perovskite active layer, thereby improving the short-circuit current.
[0149] The applicant declares that the present invention uses the above-mentioned embodiments to illustrate the hole transport material and its preparation method and application described in the present invention, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention and the addition of auxiliary components, the selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A hole transport material having a structure as shown in Formula I-1: Formula Ⅰ-1.