Electrochemical preparation method of porous spherical nano-silicon material

The electrochemical method directly converts silicon carbide to porous spherical silicon nanospheres, addressing inefficiencies and costs in existing methods, enabling efficient and cost-effective production of high-value porous silicon nanospheres.

CN115505944BActive Publication Date: 2024-12-03GUIZHOU INST OF TECH +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211158710.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-22
Publication Date
2024-12-03
Estimated Expiration
2042-09-22

AI Technical Summary

Technical Problem

Current methods for preparing nano-silicon materials with porous spherical structures are inefficient, energy-intensive, and costly, limiting their industrial application.

Method used

An electrochemical method using silicon carbide as a cathode and metal titanium as an anode to etch carbon from silicon carbide precursors, forming a porous spherical silicon material through in-situ etching in a molten salt electrolytic cell.

Benefits of technology

This method allows for the direct, efficient, and cost-effective production of high-specific surface area, high-value porous silicon nanospheres with controlled morphology, overcoming the limitations of existing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115505944B_ABST
    Figure CN115505944B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing a porous spherical nano-silicon material. It is the first time that the molten salt electrochemical etching technology is used in the preparation of silicon materials, and the new silicon material with a dual structure of porous and spherical is directly prepared. Silicon carbide is used as the initial raw material. First, silicon carbide is pressed into a porous electrode as the cathode, a metal titanium sheet with a size of 20*20*2mm is used as the anode, and an analytically pure anhydrous CaCl 2 The electrolyte is molten salt, and the corundum crucible is the electrolytic cell. The new silicon material with a porous + spherical dual structure is directly prepared by an electrochemical etching method. The method can directly prepare porous spherical silicon materials from silicon carbide, with low cost, simple process, easy control of the morphology and order of the product, low requirements on raw materials, simple preparation process, low cost, low preparation process temperature, and is conducive to industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of silicon material preparation technology, and in particular to an electrochemical preparation method of porous spherical nano silicon material. Background Art

[0002] In recent years, with the rapid development of emerging technology industries such as electric vehicles, the demand for high-performance secondary lithium-ion batteries has become more and more urgent. Lithium-ion batteries are composed of positive and negative electrode materials, electrolytes, separators, current collectors, binders, conductive agents, battery shells, etc., among which positive and negative electrode materials are the key. Lithium battery negative electrode materials include carbon materials, metal oxide materials, metal and alloy materials, lithium metal nitride materials, and the current research hotspot-silicon negative electrode materials. The theoretical lithium storage capacity of silicon is 4200 mAh / g. Among all elements that can be alloyed to store lithium, silicon has the highest specific capacity. At room temperature, each silicon atom can combine with up to 3.75 lithium atoms to obtain Li 15 Si4 alloy phase, the corresponding actual lithium storage capacity is up to 3579mAh / g, which is about 10 times the actual specific capacity of graphite. The voltage platform of silicon is slightly higher than that of graphite (about 0.4 V), and the possibility of causing surface lithium precipitation during low-temperature charging or fast charging (lithium insertion) is small. The safety performance is better than graphite, the resources are abundant, and the environment is friendly.

[0003] However, silicon negative electrodes also have some disadvantages. In the process of electrochemical lithium extraction and insertion, the silicon negative electrode is accompanied by a huge volume change of up to 300%. The resulting mechanical force will cause the silicon particles to break and pulverize, resulting in the loss of electrical contact between the silicon particles and the current collector, causing a sharp attenuation of the capacity of the silicon negative electrode material, which manifests as extremely poor cycle stability. In order to solve the above problems, scientists have done a lot of exploration and research on reducing the volume effect of silicon negative electrodes in the past decade. Among them, the volume effect modification of silicon negative electrode materials can be summarized into two aspects: one is zero-dimensional nano-ization, that is, preparing spherical silicon particles and reducing the size of silicon materials to the nanoscale. Studies have shown that spherical submicron and nanoscale materials can effectively alleviate the volume expansion effect of silicon; the second is to prepare porous silicon materials and use the pore structure inside the silicon particles to alleviate the volume effect of silicon in electrochemical reactions. This pore structure can be microporous, mesoporous, macroporous, hollow or a composite of multiple pore structures.

[0004] However, the preparation of nano-silicon materials with porous spherical structures has always been a difficult problem. How to prepare them efficiently and with low consumption is the focus of current research. The current main silane method, metallurgical method, fluidized bed method and other methods are limited by complexity, high energy consumption, and high raw material requirements. Therefore, in order to make the new porous silicon nanosphere material widely used in industrial production, the most critical thing is how to produce the new porous silicon nanosphere material on a large scale, efficiently, with low consumption, and in a precisely controllable manner. It is of particular significance to develop a short-process, efficient, low-consumption, green and controllable technology for preparing new spherical silicon materials with porous structures. Summary of the invention

[0005] The purpose of the present invention is to address the difficulties of existing zero-dimensional porous new silicon materials and their preparation processes, and to propose a method for preparing a nano silicon material with a porous + spherical dual structure, which can directly and controllably prepare a porous spherical new silicon material from a silicon carbide precursor. This method can directly prepare a porous, high specific surface area, high value-added porous silicon nanosphere material from relatively common and relatively inexpensive silicon carbide, simplifying the process flow, improving preparation efficiency, and not requiring high initial materials, thereby reducing manufacturing costs.

[0006] In order to achieve the above invention purpose, the present invention adopts the following technical solutions:

[0007] An electrochemical preparation method for a porous spherical novel nano-silicon material comprises the following steps: using silicon carbide powder as a cathode and a metal titanium sheet as an anode, obtaining an electrolysis product by an electrochemical in-situ etching method, and cleaning the electrolysis product to obtain a porous spherical nano-silicon material.

[0008] The electrochemical preparation method of the spherical nano-silicon material comprises the following steps:

[0009] (1) Preparing a precursor: adding a binder to nano-spherical silicon carbide powder and ball milling to obtain an initial powder;

[0010] (2) Preparation of cathode: The initial powder is pressed into a circular sheet, and then the circular sheet is wrapped up and down with a nickel foam mesh in a sandwich manner to obtain a sandwich-wrapped electrode;

[0011] (3) Preparation of anode: preparation of metal titanium sheet electrode;

[0012] (4) preparing an electrolytic cell system: using a corundum crucible or a stainless steel crucible as a reaction electrolytic cell, using analytically pure anhydrous calcium chloride as an electrolyte, and using an inert atmosphere as a protective gas; then assembling it with a sandwich-wrapped electrode and a metal titanium sheet electrode, and then connecting it to an external power supply device to form an electrolytic cell system;

[0013] (5) Preparing electrolysis products: After slowly heating the electrolytic cell system to a preset temperature under the protection of an inert atmosphere, a voltage is applied between the cathode and the anode of the electrolytic cell, and the sandwich-wrapped electrodes are electrolytically removed from the metal cations in the carbide to obtain electrolysis products from the cathode. When the current drops to a preset current, the electrolysis ends and the electrolysis products are obtained;

[0014] (6) Preparation of porous spherical nano-silicon materials: The electrolysis product is taken out, the nickel foam mesh is peeled off and soaked in deionized water for several times to completely remove the molten salt components remaining in the product. The product is then washed with deionized water and dried to obtain a porous spherical nano-silicon material.

[0015] In the aforementioned electrochemical preparation method of spherical nano-silicon material, in step (1), the binder is polyvinyl butyral or liquid paraffin; the amount of the binder added is 10-25% of the weight of the nano-spherical silicon carbide powder;

[0016] In the aforementioned electrochemical preparation method of spherical nano-silicon materials, the ball milling is for 10 to 24 hours.

[0017] In the aforementioned electrochemical preparation method of spherical nano-silicon materials, in step (2), the pressing pressure is 20-40 MPa.

[0018] In the aforementioned electrochemical preparation method of spherical nano-silicon material, in step (3), the size of the metal titanium sheet electrode is 20*20*2 mm.

[0019] In the aforementioned electrochemical preparation method of spherical nano-silicon material, in step (5), the preset temperature is 900-1200°C.

[0020] In the aforementioned electrochemical preparation method of spherical nano-silicon material, the applied voltage is 2.5~4.0V.

[0021] In the aforementioned electrochemical preparation method of spherical nano-silicon material, the predetermined current is 0.2-0.3A.

[0022] Beneficial Effects

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. The advantage of the present invention is that a new type of spherical silicon material with a porous structure can be directly prepared from a common nano-spherical silicon carbide precursor through molten salt electrochemical conversion. The principle of the method of the present invention is to use spherical micron or nano silicon carbide as a cathode and a metal titanium sheet as an anode to remove carbon from the silicon carbide precursor through electrochemical in-situ etching conversion to form a spherical silicon material with a porous structure. This synthesis process does not require additional process flow, that is, the preparation of a new type of spherical silicon material with a porous structure can be finally achieved in one step. The present invention provides a new green synthesis method for a new type of spherical silicon material with a porous structure.

[0025] 2. The present invention can directly prepare relatively common and inexpensive silicon carbide into porous, high specific surface area, high value-added porous silicon nanosphere materials, simplifying the process flow, improving preparation efficiency, and not requiring high initial materials, thereby reducing manufacturing costs; it has the characteristics of low cost, wide sources, simple process and continuous operation, easy control, green and pollution-free, and the ability to accurately control the morphology and order of the product.

[0026] 3. In the present invention, when preparing the cathode, the initial powder is pressed into a circular sheet, and then the circular sheet is wrapped up and down with a foam nickel mesh in a sandwich manner to obtain a sandwich-wrapped electrode. The advantages of preparing the sandwich electrode by the present invention are: 1. Better coating and protection of the cathode sheet, further preventing the cathode sheet from dispersing during the electrolysis process, resulting in the inability to collect samples; 2. Increasing the effective electrolysis area of ​​the cathode sheet and improving the electrolysis efficiency.

[0027] 4. The present invention uses metal titanium sheets as electrodes because titanium sheets are more stable in molten salts than other metals and can easily react with migrated carbon atoms to form titanium carbide, thereby achieving the purpose of recovering carbon.

[0028] 5. Anhydrous calcium chloride is used as the electrolyte in the present invention because anhydrous calcium chloride has a higher melting point and is more stable than other molten salts. At high temperatures, ion migration will be faster and the electrolysis efficiency will be higher.

[0029] 6. The purpose of the ball milling in the present invention is to grind the large-particle binder into finer particles. During this process, the raw materials and the binder will be fully mixed together. According to experimental results, the ball milling time of 10h~24h can achieve the desired effect. If the ball milling time is too short or too long, the expected effect cannot be achieved.

[0030] 7. The pressing pressure in the present invention is 20-40 MPa because it can be pressed into a sheet shape and maintain a stable structure during the electrolysis process under this pressure.

[0031] 8. The present invention sets the size of the titanium sheet to 20*20*2 mm. Under this size, 1.0-2.0 g of cathode sheet can be completely electrolyzed in combination with the voltage and electrolysis time proposed in the present invention.

[0032] 9. In the preset temperature of the present invention, voltage and temperature affect each other. After experiments, the melting point of calcium chloride is 772°C, but in order to make calcium chloride fully melt and minimize the resistance to ion migration, the preset temperature is set to 900°C at the lowest. The upper limit of the decomposition voltage of calcium chloride at this temperature is 4.0V. Above this voltage, calcium chloride will decompose under the electric field, making the experiment impossible to carry out; and the preset temperature is higher than 1200°C, which will affect the stability of the entire system, and will produce problems such as the hardness of nickel foam and titanium sheet decreasing, affecting the stability of the electrolysis system, and reducing the electrolysis efficiency. At this temperature, the upper limit of the decomposition voltage of calcium chloride is 2.5V. Among them, the current of 0.2~0.3A means that when the current value drops to this interval after a period of electrolysis, it means that the electrolysis is completed. This is a conclusion drawn based on the results of repeated experiments.

[0033] 10. The product obtained by the present invention can be analyzed to find that only silicon exists in the product, and the carbon element has been completely etched and stripped. It is a very typical spherical particle morphology with a very obvious pore structure distribution, and the pore size is mainly concentrated between 2-4nm, and it also has obvious mesoporous material curve characteristics. Therefore, the present invention has prepared a new type of nano-silicon material with a porous spherical structure, which makes up for the defects of the existing lithium battery silicon negative electrode material and has a very good application prospect. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is a schematic diagram of a short process for directly preparing a novel porous silicon nanosphere material from a silicon carbide precursor in Examples 1 and 2 of the method of the present invention.

[0035] Figure 2 The schematic diagram of the electrolytic cell structure used for synthesizing the novel porous silicon nanosphere material by the method of the present invention is shown.

[0036] The digital codes in the figure represent the following: 1-corundum or stainless steel crucible, 2-nickel foam, 3-metal titanium anode, 4-calcium chloride molten salt electrolyte, 5-iron chromium aluminum electrode wire, 6-sandwich wrapped electrode.

[0037] Figure 3 The XRD spectrum of the electrolysis product obtained in Example 1 of the present invention.

[0038] Figure 4 This is a SEM morphology image of the electrolysis product obtained in Example 1 of the present invention.

[0039] Figure 5 This is a TEM morphology image of the electrolysis product obtained in Example 1 of the present invention.

[0040] Figure 6 This is a morphology diagram of the nitrogen adsorption-desorption curve of the electrolysis product obtained in Example 1 of the present invention.

[0041] Figure 7This is a pore size distribution diagram of the electrolysis product obtained in Example 1 of the present invention.

[0042] Figure 8 This is a SEM morphology of the electrolysis product obtained in Example 2 of the present invention.

[0043] Fig. 9 This is a TEM morphology image of the electrolysis product obtained in Example 2 of the present invention. DETAILED DESCRIPTION

[0044] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present application.

[0045] Example 1. An electrochemical preparation method for porous spherical nano-silicon materials. Figure 1 The simple process shown in the figure is carried out to prepare a new type of porous silicon nanosphere material. The specific steps are as follows:

[0046] (1) Weigh 1.0 g of spherical micro-nano silicon carbide raw material fine powder to which 15% by weight of polyvinyl butyral binder has been added and ball-milled to form a uniform powder.

[0047] (2) The fine powder is pressed into a circular sheet under 25 MPa. The upper and lower sheets are wrapped with nickel foam and then clamped with iron-chromium-aluminum wire to form a silicon carbide cathode.

[0048] (3) Place the prepared silicon carbide cathode as Figure 2 The placement method shown is placed in a molten salt electrolytic cell. Analytical pure anhydrous CaCl2 is used as the molten salt electrolyte, a corundum crucible is used as the reaction container, and high-purity argon is used as the protective gas for electrolysis in a sealed resistance furnace. The electrolysis temperature is selected to be 900℃, the voltage is 2.5 V, and the 20*20*2mm metal titanium sheet assembly electrode is used as the anode system. After electrochemical etching for 12 hours, the electrolysis is completed (the current range is within the predetermined 0.2-0.3A), and then the synthesis experiment of the new porous silicon nanosphere material is completed.

[0049] (4) After the reaction is completed, the obtained product is washed with deionized water and dried in air at 100°C to obtain a new type of porous silicon nanosphere material.

[0050] The XRD spectrum of the prepared product is as follows: Figure 3 As shown, it can be seen that only silicon exists in the product, and the carbon element has been completely etched and stripped off.

[0051] The microscopic morphology of the product is Figure 4 As shown, it is a very typical spherical particle morphology.

[0052] The TEM morphology of the product is as follows Figure 5 As shown, it has a very obvious pore structure distribution.

[0053] The nitrogen adsorption-desorption curve of the product is as follows: Figure 6 As shown, it is found that it has obvious curvilinear characteristics of mesoporous materials.

[0054] Figure 7 The pore size distribution diagram of the electrolysis product obtained in this embodiment shows that the pore size of the product is mainly concentrated between 2-4 nanometers, proving that the pores of the product are mainly in the form of mesopores, thus proving that the synthesized nano-silicon material has a porous spherical structure. It can be seen that when the electrolysis voltage is 2.5 V, the new nano-silicon material with a porous spherical structure that can be prepared by this method has very good application prospects.

[0055] Example 2. An electrochemical preparation method of porous spherical nano-silicon material. The steps are as follows:

[0056] (1) Weigh 1.5 g of spherical micro-nano silicon carbide raw material fine powder to which 20% by weight of polyvinyl butyral binder has been added and ball-milled to form a uniform powder.

[0057] (2) The fine powder is pressed into a circular sheet under 30 MPa. The pressed sheet is wrapped with nickel foam and is clamped and led out with iron-chromium-aluminum wire to make a silicon carbide cathode.

[0058] (3) Place the prepared silicon carbide cathode as Figure 2 The placement method shown is placed in a molten salt electrolytic cell. Analytical pure anhydrous CaCl2 is used as the molten salt electrolyte, a corundum crucible is used as the reaction container, and high-purity argon is used as the protective gas for electrolysis in a sealed resistance furnace. The temperature is selected to be 1000℃, the voltage is 3.0 V, and the electrode assembled with a 20*20*2mm metal titanium sheet is used as the anode system. After electrochemical etching for 10 hours, the electrolysis ends (the current range is within the predetermined 0.2-0.3A), and the synthesis experiment of the new porous silicon nanosphere material is completed.

[0059] (4) After the reaction is completed, the obtained product is washed with deionized water and dried in air at 100°C to obtain a new type of porous silicon nanosphere material.

[0060] The microscopic morphology of the product is Figure 8 As shown, it is a very typical spherical particle morphology. The TEM morphology of the product is as follows Fig. 9 As shown, it has a very obvious pore structure distribution.

[0061] When the electrolysis voltage is 3.0 V, the novel nano-silicon material with a porous spherical structure prepared by this method makes up for the defects of the existing silicon negative electrode materials for lithium batteries and has very good application prospects.

[0062] Example 3. An electrochemical preparation method of porous spherical nano-silicon material. The steps are as follows:

[0063] (1) Preparing a precursor: Add 10% of the weight of the nano-spherical silicon carbide powder as a liquid paraffin binder to 1.2 g of nano-spherical silicon carbide powder and ball-mill for 24 hours to obtain an initial powder;

[0064] (2) Preparation of cathode: The initial powder is pressed into a circular sheet at 20 MPa, and then the circular sheet is wrapped up and down with a nickel foam mesh in a sandwich manner to obtain a sandwich-wrapped electrode;

[0065] (3) Preparation of anode: Prepare a titanium sheet electrode with a size of 20*20*2 mm;

[0066] (4) preparing an electrolytic cell system: using a corundum crucible or a stainless steel crucible as a reaction electrolytic cell, using analytically pure anhydrous CaCl2 as an electrolyte, and using an inert atmosphere as a protective gas; then assembling it with a sandwich-wrapped electrode and a metal titanium sheet electrode, and then connecting it to an external power supply device to form an electrolytic cell system;

[0067] (5) Preparation of electrolysis products: After slowly heating the electrolytic cell system to a preset temperature of 900°C under the protection of high-purity argon gas in an inert atmosphere, a voltage of 4.0 V is applied between the cathode and the anode of the electrolytic cell, and the sandwich-wrapped electrodes are electrolytically removed from the metal cations in the carbides to obtain electrolysis products from the cathode. When the current drops to a preset current of 0.3 A, the electrolysis ends and the electrolysis products are obtained;

[0068] (6) Preparation of porous spherical nano-silicon materials: The electrolysis product is taken out, the nickel foam mesh is peeled off and soaked in deionized water for several times to completely remove the molten salt components remaining in the product. The product is then washed with deionized water and dried to obtain a porous spherical nano-silicon material.

[0069] Example 4. An electrochemical preparation method of porous spherical nano-silicon material. The steps are as follows:

[0070] (1) Preparing a precursor: Add 25% of the weight of the nano-spherical silicon carbide powder as a liquid paraffin binder to 2.0 g of nano-spherical silicon carbide powder and ball-mill for 10 h to obtain an initial powder;

[0071] (2) Preparation of cathode: The initial powder is pressed into a circular sheet at 40 MPa, and then the circular sheet is wrapped up and down with a nickel foam mesh in a sandwich manner to obtain a sandwich-wrapped electrode;

[0072] (3) Preparation of anode: Prepare a titanium sheet electrode with a size of 20*20*2 mm;

[0073] (4) preparing an electrolytic cell system: using a corundum crucible or a stainless steel crucible as a reaction electrolytic cell, using analytically pure anhydrous CaCl2 as an electrolyte, and using an inert atmosphere as a protective gas; then assembling it with a sandwich-wrapped electrode and a metal titanium sheet electrode, and then connecting it to an external power supply device to form an electrolytic cell system;

[0074] (5) Preparation of electrolysis products: After slowly heating the electrolytic cell system to a preset temperature of 1200°C under the protection of high-purity argon gas in an inert atmosphere, a voltage of 2.5 V is applied between the cathode and the cathode of the electrolytic cell, and the sandwich-wrapped electrodes are electrolytically removed from the metal cations in the carbides to obtain electrolysis products from the cathode. When the current drops to a preset current of 0.2 A, the electrolysis ends and the electrolysis products are obtained;

[0075] (6) Preparation of porous spherical nano-silicon materials: The electrolysis product is taken out, the nickel foam mesh is peeled off and soaked in deionized water for several times to completely remove the molten salt components remaining in the product. The product is then washed with deionized water and dried to obtain a porous spherical nano-silicon material.

[0076] The above is only a preferred specific implementation manner of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can make equivalent substitutions or changes according to the technical solution and concept of the present application within the technical scope disclosed in the present application, which should be covered by the protection scope of the present application.

Claims

1. An electrochemical preparation method of porous spherical nano-silicon material, characterized in that: The following steps are involved: Using silicon carbide powder as cathode and titanium sheet as anode, electrolysis products are obtained by electrochemical in-situ etching, and the electrolysis products are cleaned to obtain porous spherical nano-silicon materials; The following steps are involved: (1) Preparing a precursor: adding a binder to nano-spherical silicon carbide powder and ball milling to obtain an initial powder; (2) Preparation of cathode: The initial powder is pressed into a circular sheet, and then the circular sheet is wrapped up and down with a nickel foam mesh in a sandwich manner to obtain a sandwich-wrapped electrode; (3) Preparation of anode: preparation of metal titanium sheet electrode; (4) preparing an electrolytic cell system: using a corundum crucible or a stainless steel crucible as a reaction electrolytic cell, using analytically pure anhydrous calcium chloride as an electrolyte, and using an inert atmosphere as a protective gas; then assembling it with a sandwich-wrapped electrode and a metal titanium sheet electrode, and then connecting it to an external power supply device to form an electrolytic cell system; (5) Preparation of electrolysis products: After slowly heating the electrolytic cell system to a preset temperature of 900-1200°C under the protection of an inert atmosphere, a voltage of 2.5-4.0V is applied between the cathode and the anode of the electrolytic cell, and the sandwich-wrapped electrodes are electrolytically removed from the metal cations in the carbides to obtain electrolysis products from the cathode. When the current drops to a preset current of 0.2-0.3A, the electrolysis ends and the electrolysis products are obtained; (6) Preparation of porous spherical nano-silicon materials: The electrolysis product is taken out, the nickel foam mesh is peeled off and soaked in deionized water for several times to completely remove the molten salt components remaining in the product. The product is then washed with deionized water and dried to obtain a porous spherical nano-silicon material.

2. The electrochemical preparation method of a porous spherical nano-silicon material according to claim 1, characterized in that: In step (1), the binder is polyvinyl butyral or liquid paraffin; the amount of the binder added is 10-25% of the weight of the nano-spherical silicon carbide powder.

3. The electrochemical preparation method of a porous spherical nano-silicon material according to claim 2, characterized in that: In step (1), the ball milling is performed for 10 to 24 hours.

4. The electrochemical preparation method of porous spherical nano-silicon material according to claim 1, characterized in that: In step (2), the pressing pressure is 20-40 MPa.

5. The electrochemical preparation method of porous spherical nano-silicon material according to claim 1, characterized in that: In step (3), the size of the metal titanium sheet electrode is 20*20*2 mm.