A calcium ion preparation and preparation method thereof

Through the combination of calcium-based solid porous carrier and calcium-source gel, the problem of low stability and absorption of calcium supplements is solved, and the sustained release and long-term storage of calcium ions in low-temperature environments is achieved, providing convenient calcium ion supplementation Way.

CN115531295BActive Publication Date: 2024-11-29SHANDONG DAODAO BIOENGINEERING CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211254364.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-13
Publication Date
2024-11-29
Estimated Expiration
2042-10-13

AI Technical Summary

Technical Problem

Existing calcium supplements have problems with poor stability, low absorption and bioavailability, especially the oral calcium gluconate solution is prone to precipitation and crystallization in low temperature environments, and solid calcium supplements need to be taken regularly, lacking sustained release type. Calcium ion supplement.

Method used

Using a combination of calcium-based solid porous carrier and calcium-containing gel doping/loading, the calcium-source gel network is prepared by porating and filling the calcium source gel network. , the cross-linking reaction of alginate and calcium lactate is used to form a stable gel structure, ensuring long-term storage and sustained release in a low-temperature environment.

Benefits of technology

The high content of calcium ions and sustained sustained release are achieved, ensuring the stability and long-term storage of the preparation in low temperature environments, overcoming the problems of poor stability and low absorption in the prior art, and providing convenient calcium ion supplementation methods. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115531295B_ABST
    Figure CN115531295B_ABST
Patent Text Reader

Abstract

The present invention relates to a loaded sustained-release calcium ion preparation, which is composed of a gel compound containing a calcium source and a calcium-based solid porous carrier, wherein the calcium-based solid porous carrier is prepared by molding and pore-forming steps using shellfish shell powder as the main raw material; the gel compound containing a calcium source is prepared by cross-linking reaction of alginate and a calcium source component. The calcium ion preparation of the present invention fills the gaps with a calcium source gel network, so that hydrogel particles with poor mechanical strength have high mechanical strength under the protection of the carrier, and after swelling in water, can not only continuously release calcium ion components for a long time, but also maintain good storage stability (especially when stored in a dry solid form).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of calcium supplement preparations, in particular to a loaded sustained-release calcium ion preparation and a preparation method thereof. Background Art

[0002] Calcium is one of the essential elements for mammals. There are various calcium supplement products on the market. For example, calcium gluconate oral solution is a common calcium ion supplement that can be used for purposes including osteoporosis, bone dysplasia, calcium supplementation, etc.

[0003] The formula of calcium gluconate oral solution on the market usually also includes auxiliary agents such as zinc gluconate, but the stability of the oral solution is a technical problem in this industry. This is because calcium gluconate solution is an unbalanced and unstable solution system, which is easy to precipitate crystals, especially in low temperature seasons or low temperature environments, and is difficult to redissolve. This phenomenon of calcium precipitation to form flocculent or granular precipitates under freezing or low temperatures not only affects the appearance but also the taste. For example, patent CN201811625872.1 discloses a calcium gluconate zinc oral solution, which increases the solubility of calcium gluconate by adding surfactants, etc., resulting in excessive and unnecessary use of additives.

[0004] Solid forms of calcium supplements, such as calcium carbonate particles, suffer from poor absorption and bioavailability.

[0005] However, whether solid or liquid calcium ion supplements are used in humans or other mammals, they need to be taken or fed regularly and quantitatively, which is too cumbersome. The prior art lacks a calcium ion supplement that can be used in a sustained-release manner.

[0006] Calcium lactate is a calcium ion source that is odorless and easily soluble in hot water. Because it has the characteristics of being easily soluble and easily absorbed, it is also a calcium supplement in the art. There are also related products on the market that use it as a calcium supplement for humans or other mammals. In addition, it can also be used as a food additive as a leavening agent due to its bulkiness. It is worth mentioning that due to the presence of divalent calcium cations in calcium lactate, it can undergo ion crosslinking reactions with alginates such as sodium alginate (replacing the Na ions blocked in the sodium alginate macromolecule), accumulating to form a stable gel structure that inhibits the flow of water, and the surface becomes a densely structured film with certain mechanical properties and selective permeability. This gel-like water ball can maintain the content liquid components and release slowly, and can also make the physical and chemical properties more stable and conducive to storage for a long time to a greater extent. However, this technology has not been used in the field of calcium ion supplementation.

[0007] In order to solve the defects of the prior art, it is necessary to provide an easily absorbed loaded sustained-release calcium ion preparation, which does not need to be taken directly orally (for example, it can be placed in a water dispenser and soaked in water to release the calcium ion component); while ensuring long-term (at least 24 hours) sustained release during use, it can also be stably stored for a long time even at lower ambient temperatures. Summary of the invention

[0008] In order to overcome the above defects in the prior art, the main purpose of the present invention is to provide a loaded sustained-release calcium ion preparation based on a solid porous carrier. Another purpose of the present invention is to provide a preparation method and application of the above loaded sustained-release calcium ion preparation.

[0009] To solve the technical problem, the present invention adopts a calcium-based solid porous carrier combined with calcium-containing gel doping / loading in the preparation of a loaded sustained-release calcium ion preparation, thereby ensuring high calcium ion content, easy absorption and sustained release.

[0010] At the same time, for the calcium-based carrier, a highly permeable porous carrier skeleton with high porosity is obtained through porosification treatment, and a calcium source gel network is filled inside the voids, so that the hydrogel particles with poor mechanical strength have high mechanical strength under the protection of the carrier. After expanding into balls in water, they can not only continuously release calcium ion components for a long time, but also maintain better storage stability under various lower temperature environments (especially when stored in a dry solid form).

[0011] The specific technical solutions of the present invention are as follows.

[0012] In the first aspect, the present invention provides a loaded sustained-release calcium ion preparation, which is composed of a gel complex containing a calcium source and a calcium-based solid porous carrier (specifically prepared by filling a calcium-based solid porous carrier with a gel complex containing a calcium source, that is, the carrier pores are filled with a calcium source gel component or a liquid-core hydrogel particle); wherein the gel complex is edible and is prepared by reacting alginate and a calcium source component containing at least calcium lactate. Optionally, the calcium-based solid porous carrier after the filling treatment is further impregnated (the impregnation liquid contains at least one additional calcium source such as calcium gluconate).

[0013] The calcium-based solid porous carrier is prepared from shellfish shell powder (preferably oyster shell powder), natural zeolite powder, low-melting point glass powder (preferably lead-free glass powder), chemical foaming agent, physical pore-forming additive (preferably sulfate) and binder as raw materials, and is prepared through molding treatment, sintering to form pores and secondary pore-forming steps.

[0014] Preferably, the preparation raw materials contain the following components in parts by weight:

[0015] 50-60 parts of shellfish shell powder, 20-30 parts of natural zeolite powder, 10-20 parts of low melting point glass powder, 0.5-5 parts of chemical foaming agent, 3-15 parts of sulfate, and an appropriate amount of binder solution.

[0016] Further preferably, the preparation raw materials contain the following components in parts by weight:

[0017] 50-60 parts of shellfish shell powder, 20-30 parts of natural zeolite powder, 10-20 parts of low melting point glass powder, 1-3 parts of chemical foaming agent, 5-15 parts of sulfate particles, and an appropriate amount of binder solution.

[0018] The low melting point glass powder is preferably one with a softening temperature below 600°C, or borosilicate glass with a melting point below 700°C (furthermore, other glass powders with a melting point not higher than the decomposition temperature of calcium carbonate may also be selected as high temperature binders). Preferably, the particle size of the glass powder is 1-10 microns (preferably 3-10 microns).

[0019] More preferably, the low melting point glass powder is a lead-free glass powder with a softening temperature of 400-600° C. and a particle size of 5-10 μm.

[0020] Among them, the shellfish shell powder is preferably clean and dry oyster shell powder, and is further preferably crushed into particles or powders not exceeding 0.2 mm (preferably not exceeding 0.1 mm).

[0021] The physical pore-forming additive is selected from sulfates, preferably potassium sulfate particles; it is highly water-soluble and can be removed by washing / dissolving after sintering as a physical temporary pore-forming material, thereby leaving corresponding gaps in the carrier and increasing the interconnected porosity. When used, it is preferably coated or coated (such as resin coating) to reduce dissolution loss during mixing.

[0022] The chemical foaming agent is selected from water-insoluble thermally decomposable chemical particles with a particle size of 0.1-10 microns and a decomposition gas production of not less than 100 ml / g, preferably sulfonyl hydrazide or azo solid particles.

[0023] Preferably, the chemical foaming agent is selected from sulfonyl hydrazides, such as at least one of trihydrazino triazine, p-toluenesulfonyl semicarbazide, 1,3-benzenedisulfonyl hydrazide, 4,4'-oxybisbenzenesulfonyl hydrazide, and p-toluenesulfonyl hydrazide. Further preferably, the sulfonyl hydrazide pore-forming agent is selected from trihydrazino triazine or p-toluenesulfonyl semicarbazide, and the decomposition gas thereof is substantially non-toxic nitrogen and carbon dioxide.

[0024] Wherein, the binder is selected from cellulose, preferably sodium carboxymethyl cellulose or ethyl cellulose, which is usually used in the form of an aqueous solution.

[0025] In the present invention, the edible gel complex containing a calcium source is prepared by cross-linking reaction between alginate and spheroids containing calcium lactate in the pores of a carrier.

[0026] Furthermore, the carrier after the cross-linking reaction is further impregnated in an impregnation solution. The impregnation solution contains at least one other form of calcium source, preferably calcium gluconate; or the impregnation solution is selected from a composite solution of calcium gluconate and zinc gluconate.

[0027] In the present invention, the cross-linking reaction comprises the following steps:

[0028] 1) In situ preparation of a filler containing calcium lactate in the internal pores of the carrier;

[0029] 2) preparing a 0.5-2 wt% alginate solution, allowing the solid porous carrier containing the calcium lactate filler to fully cross-link with the calcium lactate-containing spheres in the alginate solution, thereby obtaining a preform of a loaded sustained-release calcium ion preparation of a pore-filled gel, and freeze-drying to obtain a finished preparation;

[0030] 3) Optionally, the preformed product of the loaded sustained-release calcium ion preparation is freeze-dried, immersed in an impregnation solution containing an additional calcium source, and then freeze-dried again to obtain the loaded sustained-release calcium ion preparation.

[0031] The specific steps are as follows S1-S4:

[0032] S1: In situ preparation of a filler containing calcium lactate

[0033] Preferably, the calcium source solution is prepared at a mass ratio of calcium source: deionized water = 1:30-50. The calcium source includes at least calcium lactate; preferably, it also includes at least one of calcium chloride or calcium gluconate, and the mass ratio of calcium lactate to calcium gluconate is 3-10:1.

[0034] For example, a proper amount of calcium lactate powder is weighed at room temperature and added to deionized water, and stirred until completely dissolved; then the prepared calcium-based solid porous carrier particles (when spherical, the diameter is preferably 1-50 mm) are added to the solution, and shaken or ultrasonically treated for a period of time so that the pores of the carrier are completely filled with the solution; after pre-freezing treatment at -2°C to 0°C (or ice bath conditions), the carrier is taken out and continued to be frozen at -18°C for 6-8h to obtain a carrier whose pores are filled with an ice calcium source, which is set aside.

[0035] S2: In a water bath, add sodium alginate powder into deionized water at 50-70°C and stir continuously to completely dissolve it to obtain a sodium alginate solution with a mass fraction of 0.5-1.5wt%, add 0.05-0.1wt% glycerol dropwise, and perform ultrasonic treatment for 5-10 minutes to remove bubbles to obtain a colorless, transparent, viscous sodium alginate solution.

[0036] S3: Cool the sodium alginate solution to 25-35°C, add the carrier filled with ice calcium source, and immerse it completely in the sodium alginate solution, then shake it on a shaker for 5-15 minutes to allow the sodium alginate solution to fully cross-link with calcium sources such as calcium lactate. After the cross-linking is completed, take out the carrier to obtain a carrier with gel filled in the pores, that is, a preformed product of a loaded sustained-release calcium ion preparation. The gel (spherical or irregular) has a transparent surface film and is wrapped with a calcium source solution (or an ice-water-doped calcium source mixture) inside. Rinse the carrier with deionized water 1-3 times to remove excess sodium alginate solution on the surface, thereby obtaining a loaded sustained-release calcium ion preparation with a calcium source gel (liquid core hydrogel particles) filled in the pores. After ultraviolet disinfection, seal and package.

[0037] Furthermore, for long-term storage, the above-mentioned sustained-release calcium ion preparation can be fully frozen at -60°C and then freeze-dried to obtain a pure solid state sustained-release calcium ion preparation product, which can be sealed and packaged after disinfection.

[0038] S4: Optionally, the above-mentioned pure solid state sustained-release calcium ion preparation can be fully immersed in a solution containing other additional calcium sources, and then freeze-dried again to obtain a sustained-release calcium ion preparation doped with other calcium sources. After sterilization, the preparation is sealed and packaged.

[0039] In a second aspect, the present invention also provides a method for preparing the above-mentioned loaded sustained-release calcium ion preparation, comprising the following steps:

[0040] S1: Preparation of calcium-based solid porous carrier

[0041] 1) Weigh the following solid raw material powders of appropriate particle sizes by weight: shellfish shell powder (preferably oyster shell powder), natural zeolite powder, low melting point glass powder, chemical foaming agent, and sulfate particles, and mix them evenly in a mixer to obtain a solid mixed raw material;

[0042] Preferably, the weight proportions of the raw materials are as follows: 50-60 parts of shellfish shell powder, 20-30 parts of natural zeolite powder, 10-20 parts of low-melting point glass powder, 3-15 parts of sulfate particles; and 0.5-5 parts of sulfonylhydrazine powder.

[0043] The sulfonyl hydrazide powder is selected from trihydrazino triazine or p-toluenesulfonyl semicarbazide. The sulfate is selected from potassium sulfate.

[0044] 2) Dissolve a cellulose binder in deionized water to obtain a 0.5-3 wt% solution for use as a bonding slurry, wherein the binder is selected from sodium carboxymethyl cellulose or ethyl cellulose.

[0045] The above-mentioned adhesive slurry is evenly sprayed on the solid mixed raw materials to wet and bond them to obtain a wet material. After the wet material is fully stirred and mixed, it is pressed and formed by a ball press or a granulator to obtain a shaped wet material (based on the pressed product, it is preferred to control the amount of adhesive slurry to be within 50wt%).

[0046] The molded body may be a sphere or a cylinder or other appropriate shapes; preferably a sphere with a diameter of 5-50 mm (a sphere that is too large or too small is prone to breakage and has a low yield).

[0047] The forming operations such as spheres or round particles can be prepared by general methods in the art, for example, by granulators such as disc granulators (including but not limited to drum granulators, spherical shot blasting machines, etc.) or extrusion spheronization (extrude into a cylindrical shape and then cut into pellets and rounded).

[0048] Exemplarily, the mass dosage of the adhesive slurry can be 30-100% of the solid mixed raw material; those skilled in the art can select a suitable amount of adhesive slurry to be added according to the specific equipment used and the shape and size of the granules.

[0049] 3) The formed wet material is directly heated and pore-forming in a heating device (such as a heating kiln or a muffle furnace), and the steps are as follows:

[0050] First, perform pore-forming treatment: preheat the wet material at 150-180°C for 10-15 minutes, then heat it to 260-280°C at a rate of 5-6°C / min, and keep it warm for 30-60 minutes, so that the chemical foaming agent is fully decomposed to perform pore-forming treatment;

[0051] Secondly, a high-temperature bonding treatment is carried out: after the pore-forming treatment, the heating device is heated to 500-650°C and calcined for 0.5-1h (this temperature will not cause thermal decomposition of calcium carbonate in the oyster shell), so that the low-melting point glass powder is fully melted, and then the temperature is reduced and the product is taken out of the furnace and naturally cooled to room temperature. The broken products are removed (the broken products can be used as raw materials to replace part of the oyster shells after crushing), and the complete molded product is fully washed or soaked in water to dissolve and remove the potassium sulfate particles doped therein, and the calcium-based solid porous carrier product is obtained after being fully dried.

[0052] Among them, the chemical foaming agent can be a single substance or a mixture of multiple substances with different particle sizes to form pores of different sizes. At the same time, the particle size of the potassium sulfate physical pore-forming agent can also be different particle sizes to increase the porosity of the connected pores and reduce the number of closed pores (the closed pores inside the carrier cannot effectively fill the sustained-release gel and are invalid pores).

[0053] The calcination temperature can be selected according to the melting temperature of the molten binder, i.e., the glass powder, and the calcination temperature is preferably below 800° C. to avoid thermal decomposition of the calcium carbonate in the oyster powder.

[0054] S2: Filling a calcium source containing calcium lactate into a calcium-based solid porous carrier to prepare a carrier with pores filled with the calcium source; the specific steps are as follows:

[0055] A calcium source containing at least calcium lactate is added to deionized water, and after stirring to dissolve, calcium-based solid porous carrier particles are added to fully fill the pores inside the carrier with the calcium source solution; after freezing treatment, the carrier filled with the calcium source (solid form) is obtained and set aside.

[0056] S3: placing the carrier with pores filled with calcium source in alginate solution to carry out gelation and cross-linking reaction; the specific steps are as follows:

[0057] 1) Under water bath conditions, prepare a 0.5-1.5 wt% sodium alginate solution; add a carrier filled with a calcium source to the solution for cross-linking reaction for 5-15 minutes, wash with deionized water, and obtain a loaded sustained-release calcium ion preparation with a calcium source gel (i.e., a liquid core hydrogel) filled in the pores. After disinfection, seal and package.

[0058] 2) Optionally, the sustained-release calcium ion preparation loaded with the liquid core hydrogel body in the pores is freeze-dried to obtain a solid sustained-release calcium ion preparation finished product, which is then sealed and packaged after sterilization.

[0059] S4: Optionally, the solid-state sustained-release calcium ion preparation product can be further subjected to the following impregnation treatment steps:

[0060] The obtained solid state loaded sustained-release calcium ion preparation is immersed in an additional calcium source solution (such as calcium gluconate solution, or zinc gluconate / calcium gluconate composite solution) to carry out surface loading of the carrier material (preferably under shaking or ultrasonic conditions), and after sufficient immersion, the surface solution is removed to obtain a composite surface calcium source loaded sustained-release calcium ion preparation; optionally, it can be further freeze-dried and sealed for storage, and placed in water for subsequent use.

[0061] In a third aspect, the present invention also provides the use of the above-mentioned loaded sustained-release calcium ion preparation as a calcium supplement for mammals, including humans.

[0062] Wherein, illustratively, the application includes placing the loaded sustained-release calcium ion preparation in drinking water or other drinking liquids. Preferably, when used, the amount of water is 5-500 times the mass of the loaded sustained-release calcium ion preparation, preferably 10-200 times, and more preferably 20-100 times (those skilled in the art can select a suitable amount according to the actual use environment and the solid / liquid gel in the preparation).

[0063] For example, an appropriate amount of the loaded sustained-release calcium ion preparation of the present invention can be placed in a mammal drinking water container (trough) as a calcium ion source, and its sustained-release property is suitable for long-term use (for example, 1-15 days or even longer), such as 24h, 48h, 100h, etc., and regular replenishment of clean water is sufficient. Regeneration treatment can also be performed regularly (for example, one week, half a month, one month or two months, etc., according to the measured calcium ion concentration).

[0064] Preferably, after sufficient soaking, regeneration treatment is performed when the calcium ion concentration in the water is lower than 50 μmol / L.

[0065] Exemplarily, the regeneration method comprises the following steps:

[0066] 1) The old sustained-release calcium ion preparation is dried, calcined at 500-600°C, washed, the residual gel component is removed, and filled with a new calcium source, and then cross-linked with alginate to obtain a new pore-filled calcium source gel-loaded sustained-release calcium ion preparation.

[0067] 2) Optionally, the novel sustained-release calcium ion preparation is immersed in an additional calcium source solution and then dried. The specific operation can be carried out according to the above-mentioned relevant steps of the present invention.

[0068] Compared with the prior art, the present invention has the following beneficial technical effects:

[0069] 1) Compared with directly using calcium-based solids (such as oyster shell powder) or low-strength hydrogel balls (in the prior art, calcium ions and sodium alginate are cross-linked to form hydrogel balls with edible films), the present invention innovatively uses a calcium-based porous carrier-filled type high mechanical strength loaded sustained-release calcium ion preparation based on the characteristic requirements of long-term use in the field of calcium supplementation. The pores of the calcium source liquid core hydrogel are filled, and the preparation can also be freeze-dried and stored for a long time.

[0070] Therefore, the preparation of the present invention generates gel spheres in situ and seals them inside the carrier voids. The presence of the carrier skeleton overcomes the inherent shortcomings of hydrogel sphere preparations in the prior art, such as poor mechanical strength, difficulty in preservation, poor support, easy breakage and difficulty in storage and carrying (even the freeze-dried form is prone to fragmentation or breakage, and the gel sphere form cannot be restored after swelling).

[0071] 2) The present invention adopts a method of combining a calcium-based porous carrier with internal pore filling and surface loading of a calcium source in the preparation of a loaded sustained-release calcium ion preparation, thereby ensuring a high calcium ion loading amount and sustained sustained release (when a higher calcium ion concentration is required, more calcium source can be loaded by immersion); at the same time, for the carrier, a chemical foaming pore-forming agent and a physical pore-forming treatment are used to obtain a higher through pore, and the high permeability of the pores ensures that the cross-linking reaction in the preparation of the calcium source liquid core hydrogel body proceeds smoothly and has a high filling rate.

[0072] 2) The construction of a permeable porous carrier is one of the key technical means of the present invention. Oyster shell powder, a calcium-based material with low porosity, is used, and a specific pore-forming process is adopted. The chemical foaming agent can be thermally decomposed at a relatively low temperature to produce a large number of pores; and the high-temperature resistant potassium sulfate particles can be dissolved and removed after the carrier is formed to form a secondary pore, overcoming the disadvantage of partially closed pores produced by chemical foaming agents (although the closed pores are also ion-permeable, they are not conducive to the production reaction of the gel, that is, the permeability of sodium alginate is poor, so it cannot be quickly cross-linked in a short time to form a hydrogel to seal the calcium source solution).

[0073] At the same time, the presence of potassium sulfate can also prevent the closed-pore effect caused by the melting of the binder glass powder (melting of the glass phase) to a certain extent, which is beneficial to improving the porosity of the through holes.

[0074] In addition, the zeolite powder and oyster shell powder that are not fully bonded in the carrier are lost during the water washing process and combined with the pores formed after the potassium sulfate is dissolved, further increasing the proportion of through holes and reducing the closed hole phenomenon. The combination of the above means allows the carrier to expose more effective reactive pores, thereby providing more reaction interfaces for the cross-linking reaction (the porosity can reach more than 85% by volume). This is one of the main innovations of the present invention.

[0075] 3) The present invention adopts the method of oyster shell powder crushing-mixing-bonding sintering instead of directly using zeolite or oyster shell powder, which not only utilizes the microporous characteristics of zeolite itself and the high calcium-based characteristics of oyster shell powder (the small amount of oyster shell powder released during its use is also one of the beneficial calcium supplement ingredients), but also the co-blending and doping pore-forming method realizes a high dispersion of through holes inside the carrier, increases the exposed area of ​​the internal pores connected to the surface (favorable to the anti-spheroidization cross-linking reaction), so that it can accommodate more calcium source hydrogel.

[0076] 4) The carrier provided by the present invention has high support strength and good stability, low fragmentation rate during use, and the carrier compressive strength can be as high as 10MPa or more. Under long-term water immersion conditions, the calcium ion supplement demand can be maintained for more than 72 hours or even longer.

[0077] Exemplarily, the freeze-dried solid calcium ion preparation is continuously immersed in 30-80 times its weight of deionized water for one week, during which the deionized water is replaced every 24 hours. After one week, the calcium ion concentration in the immersed water (after immersion for 24 hours) is measured to be not less than 50 μM (depending on the concentration of the calcium source). BRIEF DESCRIPTION OF THE DRAWINGS

[0078] Figure 1 The figure shows the electron microscope surface microscopic morphology (×8000) of the freeze-dried gel in Example 4 of the present invention.

[0079] Figure 2 Shown is the microscopic morphology (×500) of the carrier skeleton composition structure in Example 4 of the present invention.

[0080] Figure 3 The figure shows the overall appearance of the carrier in Effect Example 2 of the present invention after undergoing a 72-hour flushing test. DETAILED DESCRIPTION

[0081] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.

[0082] It should be noted that, in this article, terms such as "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of more restrictions, an element defined by the sentence "comprises a ..." does not exclude the existence of other identical elements in the process, method, article or device including the element.

[0083] Example 1

[0084] Preparation of calcium-based solid porous carrier 1

[0085] 1) Weigh the following solid raw material powders by weight: 60 parts of clean oyster shell powder (passed through a 200-mesh sieve), 20 parts of natural zeolite powder (passed through a 200-mesh sieve), 15 parts of low-melting-point glass powder (Guangdong Geliner Materials Company, melting point 585-600°C), 3 parts of foaming agent trihydrazinotriazine particles (particle size 1-3 microns), and 12 parts of potassium sulfate particles (sieved, particle size range 0.2-0.6 mm), and mix them evenly in a mixer to obtain about 2.16 kg of solid mixed raw materials;

[0086] 2) Sodium carboxymethyl cellulose is dissolved in deionized water to obtain a 1.5 wt% solution as a bonding slurry. The bonding slurry is evenly sprayed on the above solid mixed raw materials to wet and bond to obtain a wet material, and the wet material is fully stirred and mixed to form spherical particles through a ball making machine to obtain a spherical wet material with a diameter of about 25 mm and a moisture content of about 32 wt%.

[0087] 3) The obtained wet molded material is directly subjected to heating and pore-forming treatment in a muffle furnace: first, the wet molded material is preheated at 150°C for 15 minutes, and then the heating device is heated to 280°C at a rate of 5°C / min and kept warm for 30 minutes; secondly, after the pore-forming treatment, the heating device is heated to 620°C and calcined for 1 hour to fully melt the low-temperature glass powder, and then the temperature is reduced and the material is taken out of the furnace and naturally cooled to room temperature to remove the broken products. The complete molded product is fully soaked and washed with water to dissolve and remove the potassium sulfate particles doped therein, and then fully dried to obtain a complete calcium-based solid porous carrier product of about 1.55g.

[0088] Example 2

[0089] Preparation of calcium-based solid porous carrier 2

[0090] 1) Weigh the following solid raw material powders by weight: 55 parts of clean oyster shell powder (passed through a 200-mesh sieve), 25 parts of natural zeolite powder (passed through a 200-mesh sieve), 12 parts of glass powder (same as above), 2.5 parts of p-toluenesulfonyl semicarbazide particles (particle size 1-5 microns) of a foaming agent, and 10 parts of potassium sulfate particles (sieved, particle size range 0.2-0.6 mm), and mix them evenly in a mixer to obtain about 2.05 kg of a solid mixed raw material;

[0091] 2) Sodium carboxymethyl cellulose is dissolved in deionized water to obtain a 1.8 wt% solution as a bonding slurry. The bonding slurry is evenly sprayed on the solid mixed raw materials to wet and bond to obtain a wet material, and the wet material is fully stirred and mixed to form spherical particles through a ball making machine to obtain a spherical wet material with a diameter of about 30 mm.

[0092] 3) The obtained wet molded material is directly subjected to heating and pore-forming treatment in a muffle furnace: first, the wet molded material is preheated at 180°C for 12 minutes, and then the heating device is heated to 260°C at a rate of 6°C / min and kept warm for 45 minutes; after the pore-forming treatment, the temperature is raised to 600°C and calcined for 1 hour to fully melt the low-temperature glass powder, and then the temperature is lowered and taken out of the furnace, and naturally cooled to room temperature, the broken products are removed, and the intact molded product is fully soaked and washed with water to dissolve and remove the potassium sulfate particles doped therein, and then fully dried to obtain a finished calcium-based solid porous carrier of about 1.46 kg.

[0093] Example 3

[0094] 1) Calcium lactate and calcium chloride powders (mass ratio of 6:1, both food grade) were weighed and added to deionized water at room temperature, and stirred until completely dissolved to prepare about 2 L of a calcium source solution, wherein the mass fraction of calcium lactate was 2.4 wt%; then about 1 kg of the calcium-based solid porous carrier 1 prepared in Example 1 was added to the solution and immersed, and then ultrasonicated for 3 min so that the pores of the carrier were completely filled with the solution; after pre-freezing treatment at -2°C, the carrier was separated and continued to be frozen at -18°C for 6 h to obtain a carrier whose pores were filled with an ice-like calcium source, which was set aside.

[0095] 2) In a water bath, add sodium alginate powder to deionized water at 60°C and continue stirring to completely dissolve it to obtain about 2 L of sodium alginate solution with a mass fraction of 1.2 wt%, add 1 ml of glycerol dropwise, and perform ultrasonic treatment for 5 min to remove bubbles to obtain a colorless and transparent sodium alginate solution.

[0096] 3) Cool the sodium alginate solution to about 30°C, add the frozen carrier with pores filled with ice calcium source, immerse it completely in the sodium alginate solution, and then shake it on a shaker at 150rpm for 6min to allow the sodium alginate solution to fully crosslink with the surface of the calcium source ice ball in the carrier pores to form a gel. After crosslinking, take out the carrier to obtain a carrier with gel filled in the pores, i.e., a preform of a loaded sustained-release calcium ion preparation. The formed gel has a transparent surface film, and the calcium source solution (part of which contains a small amount of ice water-doped calcium source mixture) is wrapped inside. Rinse the carrier with deionized water to remove excess sodium alginate solution on the surface. After the surface is dried, a loaded sustained-release calcium ion preparation with calcium source gel (i.e., liquid core hydrogel particles) filled in the pores is obtained. Sealed package.

[0097] Example 4

[0098] 1) Weigh calcium lactate and calcium gluconate powders (mass ratio of 10:1) at room temperature, add them to deionized water, and stir until completely dissolved to prepare about 2L of calcium source solution, wherein the mass fraction of calcium lactate is 2.0wt%; then take about 0.8kg of the calcium-based solid porous carrier 2 prepared in Example 2 above, add it to the solution and immerse it, ultrasonicate it for 3min so that the pores of the carrier are completely filled with the solution, continue to immerse it for 10min, and then freeze it at -2°C, then take out the carrier and continue to freeze it at -18°C for 6h to obtain a carrier with pores filled with ice-like calcium source, which is set aside.

[0099] 2) In a water bath, add sodium alginate powder to deionized water at 60°C and continue stirring to completely dissolve it to obtain about 2 L of sodium alginate solution with a mass fraction of 1.5 wt%, add 1 ml of glycerol dropwise, and perform ultrasonic treatment for 5 min to remove bubbles to obtain a colorless and transparent sodium alginate solution.

[0100] 3) Cool the sodium alginate solution to room temperature, add the frozen carrier with pores filled with ice calcium source, immerse it completely in the sodium alginate solution, and then shake it on a shaker at 140rpm for 8 minutes to allow the sodium alginate solution to fully cross-link with the surface of the calcium source ice ball in the carrier pores to form a gel. Take out the carrier to obtain a carrier with gel filled in the pores, i.e., a preform of a loaded sustained-release calcium ion preparation. The formed gel has a transparent surface film and is wrapped with a calcium source solution (or ice water doped with a calcium source) inside. Rinse the carrier with deionized water to remove excess sodium alginate solution on the surface, thereby obtaining a loaded sustained-release calcium ion preparation with liquid core hydrogel particles filled in the pores.

[0101] 4) The loaded sustained-release calcium ion preparation is fully frozen at -60°C and then freeze-dried to obtain a loaded sustained-release calcium ion preparation with a solid gel skeleton filled in the pores. The pure solid finished product is suitable for long-term storage and sealed packaging.

[0102] According to the attached Figure 1 It can be seen that the surface film layer of the gel has a pore channel structure that allows the ions wrapped inside to pass through; Figure 2 It can be seen that the carrier skeleton composition also has a porous structure, which can further accommodate calcium source substances.

[0103] Example 5

[0104] About 300 g of the solid state sustained-release calcium ion preparation obtained in Example 4 was taken for immersion treatment: it was immersed in 1 L of immersion solution at room temperature, and the immersion solution was composed of 30 g of calcium gluconate, 5 g of zinc gluconate, 10 g of gluconic acid, and the pH value was adjusted to 4. After sufficient immersion until the gel was completely swollen, the sustained-release calcium ion preparation loaded with an additional calcium source was obtained; it can be further freeze-dried and sealed for storage.

[0105] Comparative Example

[0106] 1) Prepare a 2 wt % aqueous solution of calcium lactate, add calcium chloride to make its concentration 0.35 wt %, then pour the solution into a spherical silica gel mold (with a diameter of 30 mm) and freeze it for 6 hours to form an ice ball.

[0107] 2) Prepare a 1.5wt% sodium alginate solution, immerse the prepared calcium lactate ice ball in the sodium alginate solution, and shake it on a shaker for 5-6 minutes at room temperature for cross-linking reaction. After the reaction is completed, take out the gel ball, rinse the excess sodium alginate solution on the surface, and use filter paper to absorb the attached water to obtain a hydrogel ball. The compressive strength of the gel ball is less than 0.5MPa, which is easy to break. The calcium ion preparation in Example 3 of the present invention has a compressive strength of 12MPa, which well protects the gel filled inside.

[0108] Effect Example 1

[0109] Sustained release test:

[0110] After soaking the single spherical calcium ion preparation (liquid core hydrogel filled in the pores) in 50 times the weight of deionized water for 24 hours, the calcium ion concentration in the water after equilibrium was measured to be 0.62 mM; the deionized water of equal weight was replaced every 24 hours, and the calcium ion concentration in the water (after soaking for 24 hours) was measured one week later to be 158 μM. When the same weight of the carrier without gel (carrier 1 prepared in Example 1) was used alone, the calcium ion concentration after soaking in 50 times the weight of deionized water for 24 hours was less than 10 μM.

[0111] It should be noted that when using freeze-dried solid calcium ion preparations, solid calcium ion preparations of equal weight usually need to add more water because they contain a higher content of calcium source. The adjustment of the appropriate amount can be selected by those skilled in the art according to actual conditions.

[0112] Effect Example 2

[0113] Durability test: The carriers in Example 1 above were filled into a fixed PE plastic tube with a length of 10 cm (the tube diameter was basically the same as the carrier diameter), and circulating water was continuously circulated through the plastic tube at a flow rate of 1 cm / s to simulate the flushing situation, and the time for the appearance to remain intact was observed. The experiment was repeated for 5 groups, and it was found that after 72 hours of continuous flushing, 4 groups of carriers were still able to maintain their intact shape without breaking, proving that the 72-hour flushing durability of the carriers was about 80%, and they had high water resistance and mechanical strength. According to the attached Figure 3 It can be seen that after 72 hours of flushing, the appearance of the carrier is still basically intact (among which, some loosely bound particles such as oyster shell powder and zeolite powder are lost, resulting in a certain amount of quality loss which is inevitable) without any breakage.

[0114] The embodiments of the present invention are described above, but the present invention is not limited to the above-mentioned specific implementation modes, and the above-mentioned implementation modes are not restrictive. Under the enlightenment of the present invention, ordinary technicians in this field can make many changes without departing from the scope of protection of the purpose of the present invention and the claims, which are all within the protection of the present invention.

Claims

1. A loaded sustained-release calcium ion preparation, comprising a gel complex containing a calcium source and a calcium-based solid porous carrier, characterized in that: The calcium ion preparation is prepared by the following method: S1) Preparation of calcium-based solid porous carrier: S1.1) Weigh raw material powders by weight: 50-60 parts of shellfish shell powder, 20-30 parts of natural zeolite powder, 10-20 parts of low melting point glass powder, 3-15 parts of sulfate particles, and 0.5-5 parts of sulfonylhydrazine compound powder, and mix them evenly to obtain a solid mixed raw material; the sulfonylhydrazine compound is selected from at least one of trihydrazinotriazine and p-toluenesulfonylsemicarbazide; the sulfate particles are selected from potassium sulfate; S1.2) dissolving a cellulose binder in deionized water to obtain a 0.5-3 wt% solution as a binder slurry for standby use; wherein the binder is selected from sodium carboxymethyl cellulose; spraying the binder slurry uniformly on the solid mixed raw material to wet and bond to obtain a wet material, stirring and mixing the wet material thoroughly, and then pressing and molding to obtain a molded wet material; S1.3) The wet molded material is heated in a heating device; first, the wet molded material is preheated at 150-180°C for 10-15 minutes, and then the heating device is heated to 260-280°C at a rate of 5-6°C / min, and the temperature is kept for 30-60 minutes to fully decompose the sulfonylhydrazine compound; then, the heating device is heated to 500-650°C and calcined for 0.5-1h, and the temperature is lowered and taken out of the furnace, cooled to room temperature, and the broken products are removed, and the intact molded product is fully washed with water or fully soaked with water to dissolve and remove sulfate, so as to obtain a calcium-based solid porous carrier finished product; S2) Preparation of a carrier with pores filled with a calcium source: A calcium source solution is prepared, wherein the calcium source includes at least calcium lactate; the prepared calcium-based solid porous carrier is added to the calcium source solution, and shaken or ultrasonically treated so that the carrier pores are completely filled with the solution; the carrier is taken out after pre-freezing treatment at -2°C to 0°C, and is further frozen at -18°C for 6-8h to obtain a carrier whose pores are filled with the ice calcium source; S3) Cross-linking reaction: S3.1) In a water bath, add sodium alginate powder to deionized water at 50-70°C and stir continuously to completely dissolve it to obtain a sodium alginate solution with a mass fraction of 0.5-1.5wt%, then dropwise add an appropriate amount of glycerol, and ultrasonically treat for 5-10 minutes to remove bubbles to obtain a sodium alginate solution; S3.2) Cool the sodium alginate solution to 25-35°C, add a carrier filled with an ice calcium source, and immerse it completely in the sodium alginate solution, then shake it on a shaker for 5-15 minutes to allow the sodium alginate solution and the calcium source to cross-link. After the cross-linking is completed, remove the carrier and rinse it with deionized water to obtain a loaded sustained-release calcium ion preparation with the calcium source gel filled in the pores of the carrier.

2. A method for preparing the loaded sustained-release calcium ion preparation according to claim 1, characterized in that: The following steps are involved: S1) Preparation of calcium-based solid porous carrier: S1.1) Weigh raw material powders by weight: 50-60 parts of shellfish shell powder, 20-30 parts of natural zeolite powder, 10-20 parts of low melting point glass powder, 3-15 parts of sulfate particles, and 0.5-5 parts of sulfonylhydrazine compound powder, and mix them evenly to obtain a solid mixed raw material; the sulfonylhydrazine compound is selected from at least one of trihydrazinotriazine and p-toluenesulfonylsemicarbazide; the sulfate particles are selected from potassium sulfate; S1.2) dissolving a cellulose binder in deionized water to obtain a 0.5-3 wt% solution as a binder slurry for standby use; wherein the binder is selected from sodium carboxymethyl cellulose; spraying the binder slurry uniformly on the solid mixed raw material to wet and bond to obtain a wet material, stirring and mixing the wet material thoroughly, and then pressing and molding to obtain a molded wet material; S1.3) The wet molded material is heated in a heating device: first, the wet molded material is preheated at 150-180°C for 10-15 minutes, and then the heating device is heated to 260-280°C at a rate of 5-6°C / min, and the temperature is kept for 30-60 minutes to fully decompose the sulfonylhydrazine compound; then, the heating device is heated to 500-650°C and calcined for 0.5-1h, and the temperature is lowered and taken out of the furnace, and cooled to room temperature, and the broken products are removed, and the intact molded product is fully washed with water or fully soaked with water to dissolve and remove sulfate, so as to obtain a calcium-based solid porous carrier finished product; S2) Preparation of a carrier with pores filled with a calcium source: A calcium source solution is prepared, wherein the calcium source includes at least calcium lactate; the prepared calcium-based solid porous carrier is added to the calcium source solution, and shaken or ultrasonically treated so that the carrier pores are completely filled with the solution; the carrier is taken out after pre-freezing treatment at -2°C to 0°C, and is further frozen at -18°C for 6-8h to obtain a carrier whose pores are filled with the ice calcium source; S3) Cross-linking reaction: S3.1) In a water bath, add sodium alginate powder to deionized water at 50-70°C and stir continuously to completely dissolve it to obtain a sodium alginate solution with a mass fraction of 0.5-1.5wt%, then dropwise add an appropriate amount of glycerol, and ultrasonically treat for 5-10 minutes to remove bubbles to obtain a sodium alginate solution; S3.2) Cool the sodium alginate solution to 25-35°C, add a carrier filled with an ice calcium source, and immerse it completely in the sodium alginate solution, then shake it on a shaker for 5-15 minutes to allow the sodium alginate solution and the calcium source to cross-link. After the cross-linking is completed, remove the carrier and rinse it with deionized water to obtain a loaded sustained-release calcium ion preparation with the calcium source gel filled in the pores of the carrier.

3. The preparation method according to claim 2, characterized in that: The method further comprises the following steps: subjecting the loaded sustained-release calcium ion preparation filled with the calcium source gel to a sufficient freezing treatment at -60°C and then freeze-drying the frozen calcium ion preparation to obtain a finished product of the loaded sustained-release calcium ion preparation in a pure solid state.

4. The preparation method according to claim 3, characterized in that: The obtained pure solid state loaded sustained-release calcium ion preparation finished product is further subjected to the following immersion treatment step: the obtained pure solid state loaded sustained-release calcium ion preparation finished product is immersed in an additional calcium source solution, and after sufficient immersion, the surface solution is removed to obtain a composite calcium source loaded sustained-release calcium ion preparation.

5. Use of the loaded sustained-release calcium ion preparation according to claim 1 in the preparation of a calcium supplement for mammals.

Citation Information

Patent Citations

  • Calcium-zinc gluconate oral solution and preparation method thereof

    CN109528644A

  • Calcium-zinc-ion-composite bacteriostatic alginate delivery material and preparation method thereof

    CN106994133A

  • Fenton catalyst for water treatment and preparation method thereof

    CN114643059A