A hollow rhodium nanostructure and preparation method thereof

By depositing and etching rhodium on gold nanostructures, hollow rhodium nanostructures with large specific surface areas are prepared, which solves the problems of single structure and high synthesis cost in the existing technology, and realizes the preparation and application potential of multifunctional nanostructures.

CN115533090BActive Publication Date: 2024-10-01NANJING UNIV OF AERONAUTICS & ASTRONAUTICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211190362.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-28
Publication Date
2024-10-01
Estimated Expiration
2042-09-28

AI Technical Summary

Technical Problem

Existing hollow rhodium nanostructures are limited to nanosphere structures, and the etching template used in the synthesis process has harsh conditions, resulting in high costs and limiting the scope of rhodium nanostructures in practical applications.

Method used

Hollow rhodium nanostructures are obtained by depositing rhodium on gold nanostructures and etching. The specific steps include adding rhodium trichloride and ascorbic acid solutions to cetyltrimethylammonium bromide solution to form solid gold-rhodium nanostructures. The structure is then etched in an acidic solution to remove the gold core, resulting in a hollow rhodium nanostructure with a large specific surface area.

Benefits of technology

The preparation of anisotropic hollow rhodium nanostructures has been achieved, with a large specific surface area. The etchant can be low-concentration hydrochloric acid. The conditions are mild and simple, and it is suitable for photocatalysis, electrocatalysis and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115533090B_ABST
    Figure CN115533090B_ABST
Patent Text Reader

Abstract

The invention relates to a hollow rhodium nanostructure and a preparation method thereof. The structure is formed by a discontinuous rhodium thin layer and discrete rhodium nanoclusters. The preparation method of the structure comprises the following steps: rhodium is deposited on a gold nanostructure, and then the gold is etched to obtain the hollow rhodium nanostructure. The preparation conditions of the invention are mild, the hollow rhodium nanostructure is obtained by combining template growth with an etching process, and in particular, a hollow rhodium nanostructure can be obtained, the steps are simple, and the operability is strong.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a noble metal nanostructure and a preparation method thereof, and in particular to a hollow rhodium nanostructure and a preparation method thereof. Background Art

[0002] Precious metal nanomaterials have unique optical, electric, and magnetic properties due to their different compositions, sizes, and morphologies. In recent years, they have received extensive attention in the fields of catalysis, photonics, electronics, and biomedicine. As a member of the precious metals, rhodium can be used in various catalytic reactions due to its excellent catalytic properties. However, limited by its rising price and extremely low abundance in the earth's crust, the large-scale application of rhodium faces huge obstacles. In recent years, researchers have developed many strategies to improve the utilization rate of rhodium and reduce its loading to achieve the purpose of controlling costs. The hollow rhodium nanostructure combines the advantages of rich porous channels and large specific surface area, which can greatly improve the utilization efficiency of rhodium and solve the clogging problem of nanocatalysts. It is a particularly excellent one among many structures currently available. Among the existing rhodium nanocatalysts, except for thin film catalysts, hollow rhodium nanocluster catalysts have not been reported.

[0003] However, the hollow rhodium nanostructures that have been developed so far are limited to one type of isotropic structure, namely nanospheres, which will greatly limit the scope of application of rhodium nanostructures in practical applications. In addition, the strategies for synthesizing hollow rhodium nanostructures are mostly obtained through etching templates. The conditions such as aqua regia and iodide used in the etching process are too harsh, which greatly increases the synthesis cost of hollow rhodium nanostructures. Summary of the invention

[0004] Purpose of the invention: The purpose of the present invention is to provide a hollow rhodium nanostructure with anisotropy and large specific surface area;

[0005] The second object of the present invention is to provide a method for preparing a hollow rhodium nanostructure with a large specific surface area.

[0006] Technical solution: The hollow rhodium nanostructure described in the present invention is formed by discontinuous rhodium thin layers and discrete rhodium nanoclusters.

[0007] Wherein, the diameter of the rhodium nanoclusters is 6-10nm.

[0008] Wherein, the hollow rhodium nanostructure is a hollow rhodium nano-burdock structure, a hollow rhodium nano-rod structure, a hollow rhodium nano-cube, a hollow rhodium nano-wire or a hollow rhodium nano-star.

[0009] The method for preparing the hollow rhodium nanostructure is as follows: rhodium is deposited on the gold nanostructure, and then the gold is etched to obtain the hollow rhodium nanostructure.

[0010] Specifically, the following steps are included:

[0011] (1) adding the gold nanostructure solution to a hexadecyltrimethylammonium bromide solution, then adding a rhodium trichloride aqueous solution and an ascorbic acid solution, and placing the obtained mixed solution in an oven to obtain a solid gold-rhodium nanostructure;

[0012] (2) adding the solid gold-rhodium nanostructure to a hexadecyltrimethylammonium bromide solution after centrifugation, adding an acidic solution at room temperature, and drying the obtained mixed solution;

[0013] (3) The sample obtained in step (2) is centrifuged and then placed in a hexadecyltrimethylammonium bromide solution for dispersion to obtain a hollow rhodium nanostructure.

[0014] The method for preparing the hollow rhodium nanostructure of the present invention is universal. To obtain the hollow rhodium nanostructure of the target shape, it is only necessary to use a gold nanometal structure of the corresponding shape. Preferably, the gold nanostructure in step (1) is a gold nanobipyramid, and the obtained hollow rhodium nanostructure is a hollow rhodium nano-Xanthium structure.

[0015] Preferably, the gold nanostructure in step (1) is a gold nanorod, and the obtained hollow rhodium nanostructure is a hollow rhodium nanorod structure.

[0016] Wherein, in the step (1), the concentration of the hexadecyltrimethylammonium bromide solution is 0.001-0.1 mol / L, the concentration of the rhodium chloride aqueous solution is 0.001-0.01 mol / L, and the concentration of the ascorbic acid solution is 0.01-0.1 mol / L; the volume ratio of the gold nanostructure, hexadecyltrimethylammonium bromide, rhodium chloride, and ascorbic acid is 10-40:6-9:4-8:4-8. When the concentration of the reaction reagent is lower than the aforementioned range, the reaction rate will be too slow, the rhodium deposition will be incomplete, and the like; when the concentration of the reaction reagent is higher than the aforementioned range, the reaction rate will be too fast, the morphology will be uncontrollable, and in addition, it may cause excessive rhodium deposition, which is not conducive to the subsequent removal of the gold core.

[0017] Wherein, the reaction temperature in step (1) is 40-80°C and the reaction time is 1-8h. If the reaction temperature is too low or the reaction time is too short, the rhodium deposition is incomplete and the reaction rate is too slow. If the reaction temperature is too high or the reaction time is too long, the diffusion effect of the rhodium nanoshell on the surface of the gold core is significantly increased, the morphology is uncontrollable and it is not conducive to the subsequent removal of the gold core.

[0018] Wherein, in the step (2), the concentration of hexadecyltrimethylammonium bromide is 0.01-2 mol / L, the concentration of the acidic solution is 1-5 mol / L, and the volume ratio of the solid gold-rhodium nanostructure solution, the hexadecyltrimethylammonium bromide solution, and the acidic solution is 1:1:1. When the concentration of the reaction reagent is lower than the aforementioned range, a series of problems such as poor dispersion of the solid gold-rhodium nanostructure and uneven and incomplete etching of the gold core will result; when the concentration of the reaction reagent is higher than the aforementioned range, problems such as too fast etching rate, uncontrollable morphology, and excessive use of the reaction reagent and increased cost will result.

[0019] Wherein, the reaction temperature in step (2) is 60-80°C and the reaction time is 4-8h. If the reaction temperature is too low or the reaction time is too short, the rate of removing the gold core will be significantly slowed down or the gold core will not be completely removed.

[0020] Wherein, the acidic solution in step (2) is preferably hydrochloric acid.

[0021] Wherein, the concentration of the hexadecyl trimethyl ammonium bromide solution in step (3) is 0.001-0.01 mol / L. The role of hexadecyl trimethyl ammonium bromide is to act as a surfactant and stabilize the surface of the hollow rhodium structure. When the concentration is lower than the above range, the nanostructure will not be well dispersed and agglomeration will occur, which is not conducive to subsequent applications. When the concentration is higher than the above range, the concentration of bromide ions on the surface of the hollow rhodium nanostructure is too high, which is not conducive to exposing its surface catalytic sites and resulting in reduced performance.

[0022] The heating conditions in steps (2) and (3) are: heating in an oven, heating in a water bath, or heating in an oil bath.

[0023] In step (3), the dispersing process is: dispersing after oscillating in an oscillator at room temperature.

[0024] Reaction principle: Under the action of ascorbic acid, the rhodium metal precursor undergoes a reduction reaction on the surface of the gold nanostructure, forming a rhodium nanoshell on the surface of the gold nanostructure, forming a solid gold-rhodium nanobimetallic structure; in the presence of hexadecyltrimethylammonium bromide, the acidic solution can etch away the core structure of the gold nanostructure, thereby obtaining a hollow rhodium nanostructure. Furthermore, the present invention is based on a route of template growth followed by etching, using gold nanobipyramids as templates, growing a rhodium nanocluster shell, and then etching with hydrochloric acid to obtain an anisotropic hollow rhodium nanostructure. This preparation method can also be extended to the preparation of hollow rhodium nanostructures of various other shapes, by simply replacing the gold nanobipyramids with corresponding gold nanostructures, such as gold nanorods, nanocubes, nanowires, nanostars, etc.

[0025] Beneficial effects: Compared with the prior art, the present invention achieves the following significant effects: (1) In the presence of ascorbic acid and hexadecyltrimethylammonium bromide, a gold nanostructure is used as a template, and a hollow rhodium nanostructure is prepared by a process of template growth and then etching, which has various anisotropies and a large specific surface area; (2) The etchant can be low-concentration hydrochloric acid, the preparation conditions are mild and simple, and the operability is strong; (3) The obtained hollow rhodium nano-Xanthium structure is anisotropic, which is not available in the prior art; (4) The obtained hollow rhodium nano-Xanthium structure has uniform morphology and good dispersibility, and has potential applications in the fields of photocatalysis, electrocatalysis, and three-way catalysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is the preparation principle diagram of the present invention;

[0027] Figure 2 is a transmission electron microscope image of the hollow rhodium nano-Xanthium structure of Example 1;

[0028] Figure 3 is the energy spectrum of the hollow rhodium nano-Xanthium structure of Example 1;

[0029] Figure 4 is the UV-visible light absorption spectrum of the hollow rhodium nano-Xanthium structure of Example 1;

[0030] Figure 5 is a transmission electron microscope image of a solid gold-rhodium nanostructure and a hollow gold-rhodium nanostructure grown based on gold nanorods in Example 12;

[0031] Figure 6 It is the transmission electron microscope image of the structure obtained in comparative examples 1 and 2. DETAILED DESCRIPTION

[0032] The present invention is described in further detail below.

[0033] Example 1

[0034] Step 1, adding 1 mL of the gold nanobipyramid solution to 9 mL of 0.001 mol / L hexadecyltrimethylammonium bromide solution, then adding 400 μL of 0.01 mol / L rhodium trichloride aqueous solution and 400 μL of 0.1 mol / L ascorbic acid solution, shaking the obtained mixed solution and placing it in an oven at 80° C. to react for 8 hours to obtain a solid gold-rhodium nano-Xanthium structure;

[0035] Step 2, after the solid gold-rhodium nano-Xanthium structure is centrifuged at 8000rpm for 15min, the supernatant is discarded, and the lower precipitate is dispersed into 5mL, 0.01mol / L hexadecyltrimethylammonium bromide solution, and then 5mL, 2mol / L hexadecyltrimethylammonium bromide solution and 5mL, 1mol / L hydrochloric acid solution are added respectively, and the obtained mixed solution is shaken and placed in an 80°C oven for reaction for 8h;

[0036] Step 3, after the sample in step 2 is centrifuged at 8000rpm for 10min, the supernatant is discarded, the lower precipitate is dispersed in 5mL, 0.001mol / L hexadecyltrimethylammonium bromide solution, and oscillated at 100rpm in an oscillator at room temperature for 1h to obtain a hollow rhodium nano-Xanthium structure.

[0037] The morphology of the prepared hollow rhodium nanostructures was analyzed, see Figures 1 to 3 , respectively are the transmission electron microscope image, high-resolution transmission electron microscope image and energy spectrum image of the hollow rhodium nano-Xanthium structure. It can be seen from the figures that the structure is composed only of rhodium elements, with abundant porous channels on the surface. The rhodium nanostructure layer is composed of discontinuous thin layers and discrete rhodium nanoclusters with a diameter of 6-10nm. This morphology gives the hollow rhodium nano-Xanthium structure a larger specific surface area.

[0038] Figure 4 It is the UV-visible absorption spectra corresponding to the synthesized hollow rhodium nano-Xanthium structure and the solid gold-rhodium nano-Xanthium structure. It can be clearly seen that the SPR resonance peak belonging to the gold nanobipyramid almost disappeared after the etching treatment, confirming the successful preparation of the hollow rhodium nano-Xanthium structure.

[0039] Example 2

[0040] Step 1, adding 1 mL of the gold nanobipyramid solution to 9 mL of 0.001 mol / L hexadecyltrimethylammonium bromide solution, then adding 500 μL of 0.01 mol / L rhodium trichloride aqueous solution and 500 μL of 0.1 mol / L ascorbic acid solution, shaking the obtained mixed solution and placing it in an oven at 80° C. for reaction for 8 hours to obtain a solid gold-rhodium nano-Xanthium structure;

[0041] Step 2, after the solid gold-rhodium nano-Xanthium structure is centrifuged at 8000rpm for 15min, the supernatant is discarded, and the lower precipitate is dispersed into 5mL, 0.01mol / L hexadecyltrimethylammonium bromide solution, and then 5mL, 2mol / L hexadecyltrimethylammonium bromide solution and 5mL, 2mol / L hydrochloric acid solution are added respectively, and the obtained mixed solution is shaken and placed in an 80°C oven for reaction for 8h;

[0042] Step 3, after the sample in step 2 is centrifuged at 8000rpm for 10min, the supernatant is discarded, the lower precipitate is dispersed in 5mL, 0.001mol / L hexadecyltrimethylammonium bromide solution, and oscillated at 100rpm in an oscillator at room temperature for 1h to obtain a hollow rhodium nano-Xanthium structure.

[0043] Example 3

[0044] Step 1, add 1mL of gold nanobipyramid solution to 9mL of 0.001mol / L hexadecyltrimethylammonium bromide solution, then add 600μL of 0.01mol / L rhodium trichloride aqueous solution and 600μL of 0.1mol / L ascorbic acid solution, shake the obtained mixed solution and place it in an 80°C oven for reaction for 8h to obtain a solid gold-rhodium nano-Xanthium structure;

[0045] Step 2, after the solid gold-rhodium nano-Xanthium structure is centrifuged at 8000rpm for 15min, the supernatant is discarded, and the lower precipitate is dispersed into 5mL, 0.01mol / L hexadecyltrimethylammonium bromide solution, and then 5mL, 2mol / L hexadecyltrimethylammonium bromide solution and 5mL, 3mol / L hydrochloric acid solution are added respectively, and the obtained mixed solution is shaken and placed in an 80°C oven for reaction for 8h;

[0046] Step 3, after the sample in step 2 is centrifuged at 8000rpm for 10min, the supernatant is discarded, the lower precipitate is dispersed in 5mL, 0.001mol / L hexadecyltrimethylammonium bromide solution, and oscillated at 100rpm in an oscillator at room temperature for 1h to obtain a hollow rhodium nano-Xanthium structure.

[0047] Example 4

[0048] Step 1, adding 1 mL of the gold nanobipyramid solution to 9 mL of 0.001 mol / L hexadecyltrimethylammonium bromide solution, then adding 700 μL of 0.01 mol / L rhodium trichloride aqueous solution and 700 μL of 0.1 mol / L ascorbic acid solution, shaking the obtained mixed solution and placing it in an oven at 80° C. to react for 8 hours to obtain a solid gold-rhodium nano-Xanthium structure;

[0049] Step 2, after the solid gold-rhodium nano-Xanthium structure is centrifuged at 8000rpm for 15min, the supernatant is discarded, and the lower precipitate is dispersed into 5mL, 0.01mol / L hexadecyltrimethylammonium bromide solution, and then 5mL, 2mol / L hexadecyltrimethylammonium bromide solution and 5mL, 4mol / L hydrochloric acid solution are added respectively, and the obtained mixed solution is shaken and placed in an 80°C oven for reaction for 8h;

[0050] Step 3, after the sample in step 2 is centrifuged at 8000rpm for 10min, the supernatant is discarded, the lower precipitate is dispersed in 5mL, 0.001mol / L hexadecyltrimethylammonium bromide solution, and oscillated at 100rpm in an oscillator at room temperature for 1h to obtain a hollow rhodium nano-Xanthium structure.

[0051] Example 5

[0052] Step 1, adding 1 mL of the gold nanobipyramid solution to 9 mL of 0.001 mol / L hexadecyltrimethylammonium bromide solution, then adding 800 μL of 0.01 mol / L rhodium trichloride aqueous solution and 800 μL of 0.1 mol / L ascorbic acid solution, shaking the obtained mixed solution and placing it in an oven at 80° C. to react for 8 hours to obtain a solid gold-rhodium nano-Xanthium structure;

[0053] Step 2, after the solid gold-rhodium nano-Xanthium structure is centrifuged at 8000rpm for 15min, the supernatant is discarded, and the lower precipitate is dispersed into 5mL, 0.01mol / L hexadecyltrimethylammonium bromide solution, and then 5mL, 2mol / L hexadecyltrimethylammonium bromide solution and 5mL, 5mol / L hydrochloric acid solution are added respectively, and the obtained mixed solution is shaken and placed in an 80°C oven for reaction for 8h;

[0054] Step 3, after the sample in step 2 is centrifuged at 8000rpm for 10min, the supernatant is discarded, the lower precipitate is dispersed in 5mL, 0.001mol / L hexadecyltrimethylammonium bromide solution, and oscillated at 100rpm in an oscillator at room temperature for 1h to obtain a hollow rhodium nano-Xanthium structure.

[0055] Example 6

[0056] Step 1, adding 2 mL of gold nanobipyramid solution to 8 mL of 0.001 mol / L hexadecyltrimethylammonium bromide solution, then adding 400 μL of 0.01 mol / L rhodium trichloride aqueous solution and 400 μL of 0.1 mol / L ascorbic acid solution, shaking the obtained mixed solution and placing it in an 80° C. oven for reaction for 8 hours to obtain a solid gold-rhodium nano-Xanthium structure;

[0057] Step 2, after the solid gold-rhodium nano-Xanthium structure is centrifuged at 8000rpm for 15min, the supernatant is discarded, and the lower precipitate is dispersed into 5mL, 0.10mol / L hexadecyltrimethylammonium bromide solution, and then 5mL, 2mol / L hexadecyltrimethylammonium bromide solution and 5mL, 3mol / L hydrochloric acid solution are added respectively, and the obtained mixed solution is shaken and placed in an 80°C oven for reaction for 8h;

[0058] Step 3, after the sample in step 2 is centrifuged at 8000rpm for 10min, the supernatant is discarded, the lower precipitate is dispersed in 5mL, 0.001mol / L hexadecyltrimethylammonium bromide solution, and oscillated at 200rpm in an oscillator at room temperature for 1h to obtain a hollow rhodium nano-Xanthium structure.

[0059] Example 7

[0060] Step 1, add 3mL of gold nanobipyramid solution to 7mL of 0.001mol / L hexadecyltrimethylammonium bromide solution, then add 400μL of 0.01mol / L rhodium trichloride aqueous solution and 400μL of 0.1mol / L ascorbic acid solution, shake the obtained mixed solution and place it in an 80°C oven for reaction for 8h to obtain a solid gold-rhodium nano-Xanthium structure;

[0061] Step 2, after the solid gold-rhodium nano-Xanthium structure is centrifuged at 8000rpm for 15min, the supernatant is discarded, and the lower precipitate is dispersed into 5mL, 0.10mol / L hexadecyltrimethylammonium bromide solution, and then 5mL, 2mol / L hexadecyltrimethylammonium bromide solution and 5mL, 4mol / L hydrochloric acid solution are added respectively, and the obtained mixed solution is shaken and placed in an 80°C oven for reaction for 8h;

[0062] Step 3, after the sample in step 2 is centrifuged at 8000rpm for 10min, the supernatant is discarded, the lower precipitate is dispersed in 5mL, 0.001mol / L hexadecyltrimethylammonium bromide solution, and oscillated at 200rpm in an oscillator at room temperature for 1h to obtain a hollow rhodium nano-Xanthium structure.

[0063] Example 8

[0064] Step 1, add 4 mL of gold nanobipyramid solution to 6 mL of 0.001 mol / L hexadecyltrimethylammonium bromide solution, then add 400 μL of 0.01 mol / L rhodium trichloride aqueous solution and 400 μL of 0.1 mol / L ascorbic acid solution, shake the obtained mixed solution and place it in an 80° C. oven for reaction for 8 hours to obtain a solid gold-rhodium nano-Xanthium structure;

[0065] Step 2, after the solid gold-rhodium nano-Xanthium structure is centrifuged at 8000rpm for 15min, the supernatant is discarded, and the lower precipitate is dispersed into 5mL, 0.10mol / L hexadecyltrimethylammonium bromide solution, and then 5mL, 2mol / L hexadecyltrimethylammonium bromide solution and 5mL, 5mol / L hydrochloric acid solution are added respectively, and the obtained mixed solution is shaken and placed in an 80°C oven for reaction for 8h;

[0066] Step 3, after the sample in step 2 is centrifuged at 8000rpm for 10min, the supernatant is discarded, the lower precipitate is dispersed in 5mL, 0.001mol / L hexadecyltrimethylammonium bromide solution, and oscillated at 200rpm in an oscillator at room temperature for 1h to obtain a hollow rhodium nano-Xanthium structure.

[0067] Example 9

[0068] Step 1, adding 1 mL of the gold nanobipyramid solution to 9 mL of 0.001 mol / L hexadecyltrimethylammonium bromide solution, then adding 400 μL of 0.01 mol / L rhodium trichloride aqueous solution and 400 μL of 0.1 mol / L ascorbic acid solution, shaking the obtained mixed solution and placing it in an oven at 80° C. to react for 8 hours to obtain a solid gold-rhodium nano-Xanthium structure;

[0069] Step 2, after the solid gold-rhodium nano-Xanthium structure is centrifuged at 12000rpm for 15min, the supernatant is discarded, and the lower precipitate is dispersed into 5mL, 0.1mol / L hexadecyltrimethylammonium bromide solution, and then 5mL, 2mol / L hexadecyltrimethylammonium bromide solution and 5mL, 1mol / L hydrochloric acid solution are added respectively, and the obtained mixed solution is shaken and placed in an 80°C oven for reaction for 8h;

[0070] Step 3, after the sample in step 2 is centrifuged at 12000rpm for 10min, the supernatant is discarded, the lower precipitate is dispersed in 5mL, 0.01mol / L hexadecyltrimethylammonium bromide solution, and oscillated at 200rpm in an oscillator at room temperature for 1h to obtain a hollow rhodium nano-Xanthium structure.

[0071] Example 10

[0072] Step 1, add 1mL of gold nanobipyramid solution to 9mL of 0.001mol / L hexadecyltrimethylammonium bromide solution, then add 400μL of 0.001mol / L rhodium trichloride aqueous solution and 400μL of 0.1mol / L ascorbic acid solution, shake the obtained mixed solution and place it in a 40°C oven for reaction for 1h to obtain a solid gold-rhodium nano-Xanthium structure;

[0073] Step 2, after the solid gold-rhodium nano-Xanthium structure is centrifuged at 8000rpm for 10min, the supernatant is discarded, and the lower precipitate is dispersed into 5mL, 0.001mol / L hexadecyltrimethylammonium bromide solution, and then 5mL, 2mol / L hexadecyltrimethylammonium bromide solution and 5mL, 1mol / L hydrochloric acid solution are added respectively, and the obtained mixed solution is shaken and placed in a 60°C oven for reaction for 4h;

[0074] Step 3, after the sample in step 2 is centrifuged at 8000rpm for 10min, the supernatant is discarded, the lower precipitate is dispersed in 5mL, 0.001mol / L hexadecyltrimethylammonium bromide solution, and oscillated at 100rpm in an oscillator at room temperature for 1h to obtain a hollow rhodium nano-Xanthium structure.

[0075] Embodiment 11

[0076] Step 1, adding 1 mL of gold nanobipyramid solution to 9 mL of 0.1 mol / L hexadecyltrimethylammonium bromide solution, then adding 400 μL of 0.01 mol / L rhodium trichloride aqueous solution and 400 μL of 1 mol / L ascorbic acid solution, shaking the obtained mixed solution and placing it in an 80° C. oven for reaction for 8 hours to obtain a solid gold-rhodium nano-Xanthium structure;

[0077] Step 2, after the solid gold-rhodium nano-Xanthium structure is centrifuged at 12000rpm for 15min, the supernatant is discarded, and the lower precipitate is dispersed into 5mL, 0.01mol / L hexadecyltrimethylammonium bromide solution, and then 5mL, 2mol / L hexadecyltrimethylammonium bromide solution and 5mL, 5mol / L hydrochloric acid solution are added respectively, and the obtained mixed solution is shaken and placed in an 80°C oven for reaction for 8h;

[0078] Step 3, after the sample in step 2 is centrifuged at 12000rpm for 15min, the supernatant is discarded, the lower precipitate is dispersed in 5mL, 0.01mol / L hexadecyltrimethylammonium bromide solution, and oscillated at 200rpm in an oscillator at room temperature for 3h to obtain a hollow rhodium nano-Xanthium structure.

[0079] Example 12

[0080] On the basis of Example 1, the difference from Example 1 is that the gold nanobipyramids are replaced by a gold nanorod solution.

[0081] Depend on Figure 5 It can be seen that the present invention uses a low-purity gold nanorod sample as a template for the gold hollow rhodium nanostructure, which includes gold nanorods, gold nanospheres, and gold nanocubes, and the corresponding shapes are marked in the figure. The solid gold-rhodium nanostructure and the hollow rhodium nanostructure both faithfully replicate the shape of the corresponding gold nanostructure core, and the obtained hollow rhodium nanostructures include hollow rhodium nanorod structures, hollow rhodium nanocubes, hollow rhodium nanospheres, and other structures. This example illustrates the universality of the preparation method of the present invention.

[0082] Comparative Example 1

[0083] On the basis of Example 1, different from Example 1, the concentration of the rhodium chloride solution in step 1 is 0.0008 mol / L.

[0084] Comparative Example 2

[0085] Based on Example 1, different from Example 1, the temperature in step 2 is 50°C.

[0086] Depend on Figure 6 It can be seen that the synthesis of hollow rhodium Xanthium nanostructures is significantly affected by the temperature and concentration of the reaction reagents. If the concentration of the reaction reagents is too low or the reaction temperature is too low, problems such as incomplete rhodium deposition and incomplete gold core etching will occur.

Claims

1. A method for preparing a hollow rhodium nanostructure, characterized in that: Depositing rhodium on the gold nanostructures and then etching the gold to obtain hollow rhodium nanostructures; The method for preparing the hollow rhodium nanostructure specifically comprises the following steps: (1) Adding a gold nanostructure solution to a hexadecyltrimethylammonium bromide solution, and then adding a rhodium trichloride aqueous solution and an ascorbic acid solution, and reacting the obtained mixed solution under heating conditions to obtain a solid gold-rhodium nanostructure; the concentration of the hexadecyltrimethylammonium bromide solution is 0.001~0.1 mol / L, the concentration of the rhodium trichloride aqueous solution is 0.001~0.01 mol / L, and the concentration of the ascorbic acid solution is 0.01~0.1 mol / L; the reaction temperature is 40~80°C, and the reaction time is 1~8 h; (2) adding the solid gold-rhodium nanostructure to a hexadecyltrimethylammonium bromide solution after centrifugation, adding an acidic solution at room temperature, and reacting the obtained mixed solution under heating conditions; the concentration of hexadecyltrimethylammonium bromide is 0.01~2 mol / L, the concentration of the acidic solution is 1~5 mol / L; the reaction temperature is 60~80 °C, and the reaction time is 4~8h; (3) The sample obtained in step (2) is centrifuged and placed in a hexadecyltrimethylammonium bromide solution to obtain a hollow rhodium nanostructure after dispersion; the concentration of the hexadecyltrimethylammonium bromide solution is 0.001-0.01 mol / L.

2. A hollow rhodium nanostructure prepared by the preparation method according to claim 1, characterized in that: The nanostructured material is composed of discontinuous rhodium thin layers and discrete rhodium nanoclusters; the diameter of the rhodium nanoclusters is 6-10 nm.

3. The hollow rhodium nanostructure according to claim 2, characterized in that The hollow rhodium nanostructure is a hollow rhodium nano-burdock structure, a hollow rhodium nano-rod structure, a hollow rhodium nano-cube, a hollow rhodium nano-wire or a hollow rhodium nano-star.