A membrane capacitor deionization and desalination module and its preparation method and a membrane capacitor deionization and desalination device

By using ordered carbon materials and electrodeposition doped conductive polymer technology in the capacitive deionization desalination module, the problems of low adsorption capacity and poor stability of conductive polymer electrode materials are solved, and efficient and stable salt ion adsorption and Desalination effect.

CN115536114BActive Publication Date: 2024-11-29QINGHAI INST OF SALT LAKES OF CHINESE ACAD OF SCI +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211014518.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-23
Publication Date
2024-11-29
Estimated Expiration
2042-08-23

AI Technical Summary

Technical Problem

In the existing capacitive deionization technology, the ion saturation adsorption capacity of the conductive polymer electrode material is low, and there are problems such as low desalination amount, slow desalination rate and poor cycle stability during the desalination process.

Method used

Using ordered carbon materials as the matrix, redox doped conductive polymers with ion vacancies of different sizes and ion radii are electrodeposited to form an asymmetric doped electrode to improve the adsorption amount and stability during the desalination process.

Benefits of technology

It realizes the "coordinated and efficient" adsorption of specific anion and cation pairs in the salt solution during the desalination process, improves the adsorption capacity and electrode cycle stability, and reduces energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115536114B_ABST
    Figure CN115536114B_ABST
Patent Text Reader

Abstract

The present invention provides a membrane capacitor deionization and desalination module, a preparation method thereof, and a membrane capacitor deionization and desalination device. The membrane capacitor deionization and desalination module comprises an anode, a cathode, and an ion exchange membrane; the anode comprises a carbon material matrix and a conductive polymer doped with anions A deposited in the carbon material matrix; the cathode comprises a carbon material matrix and a conductive polymer doped with anions B deposited in the carbon material matrix. The present invention uses an ordered carbon material as a matrix, and electrodeposit redox-doped conductive polymers of ion vacancies of different ionic radii, thereby being able to "synergistically and efficiently" adsorb specific anion and cation pairs in a salt solution during the desalination process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of capacitor deionization and desalination materials, and in particular relates to a membrane capacitor deionization and desalination module and a preparation method thereof, and a membrane capacitor deionization and desalination device. Background Art

[0002] Capacitive deionization (CDI) is a green and efficient water treatment technology developed in recent years for low-salinity saltwater and seawater desalination. The capacitive deionization device contains a pair of porous electrodes, allowing the salt solution to flow between the electrodes. When a certain voltage (usually 1.0-1.6V) is applied to the porous electrodes, the anions and cations in the salt solution will migrate to the surface of the porous electrodes with opposite charges under the action of the electric field to form a double layer structure, thereby removing ions in the solution (electroadsorption or charging process).

[0003] Membrane Capacitive Deionization (MCDI) technology is a further improvement of CDI technology. It adds ion exchange membranes on both sides of the electrode. By applying voltage to the positive and negative electrodes, cations can freely penetrate into the negative electrode through the cation exchange membrane (CEM), and anions can also penetrate into the positive electrode through the anion exchange membrane (AEM) to prevent the common ion effect during the regeneration process, thereby improving the overall desalination efficiency of the module and reducing energy consumption.

[0004] Regardless of the form of the capacitive deionization module, the active electrode plays the most critical role. In traditional technology, carbon electrodes based on electric double layer (EDL) capacitors, such as activated carbon (AC), carbon nanotubes (CNTs), graphene or carbon aerogel, have been widely used in the MCDI field. However, the ion saturation adsorption capacity (SAC) of these electrode materials based on the ion double layer electrical adsorption / desorption process is usually low (generally 15-25 mg / g), because the salt ions with opposite charges are only adsorbed on the surface of the corresponding carbon electrode material.

[0005] Pseudocapacitor materials that store ions through Faradaic reactions rather than double-layer adsorption have attracted special attention due to their huge adsorption capacity, low energy loss, and selective separation properties. Conducting polymers (CPs) can store high-density charges and generate Faradaic pseudocapacitors, and are a class of pseudocapacitor electrode materials with great application potential.

[0006] Common conductive polymers mainly include polypyrrole (PPy), polyaniline (PANI) and polythiophene (PEDOT). However, the intrinsic mechanical properties of conductive polymers are often poor, and they will induce volume swelling effect during frequent oxidation / reduction processes, which is not conducive to the precise regulation of ion transfer channels in polymers. Moreover, conductive polymers are prone to peroxidation reactions at high potentials, resulting in decreased electrical activity and increased ion transfer resistance. They are easy to fall off from the current collector or supporting substrate, resulting in low desalination capacity, slow desalination rate and poor cycle stability during MCDI desalination.

[0007] In addition, when assembling electrode materials into MCDI modules, due to the material itself or the design, people often only study a single electrode material as a part of the MCDI desalination process, while the other electrode usually uses the traditional double-layer electrode material as mentioned above, and this type of MCDI module is called an "asymmetric" or "hybrid" MCDI module. However, in fact, this electrode design cannot provide more active adsorption sites for inorganic salt ion pairs in the solution, so the adsorption amount in the desalination process still needs to be further improved.

[0008] Therefore, in this field, there is an urgent need to develop a symmetrical membrane capacitor deionization and desalination module, which not only has high desalination efficiency and adsorption capacity, but also has a stable structure, is not easy to fall off, and has a simple and easy preparation method. Summary of the invention

[0009] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a membrane capacitor deionization and desalination module and a preparation method thereof and a membrane capacitor deionization and desalination device. The present invention uses an ordered carbon material as a matrix to electrodeposit redox-doped conductive polymers of ion vacancies of different ionic radii, thereby being able to "synergistically and efficiently" adsorb specific anion and cation pairs in a salt solution during the desalination process.

[0010] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0011] In a first aspect, the present invention provides a membrane capacitor deionization and desalination module, the membrane capacitor deionization and desalination module comprising an anode, a cathode and an ion exchange membrane;

[0012] The anode includes a carbon material matrix and a conductive polymer doped with anions A deposited in the carbon material matrix;

[0013] The cathode includes a carbon material matrix and a conductive polymer doped with anions B and deposited in the carbon material matrix.

[0014] The present invention provides an ordered three-dimensional continuous network structure by using carbon material as a substrate, enhances the conductivity of the electrode, and solves the problem that traditional conductive polymer materials are prone to agglomeration and poor cyclic stability when used alone. In addition, by electrodeposition of asymmetric coordination doping and activation of conductive polymers with anions of different ionic radii, in the p-doping process, the doped anion A is easily dedoped during the synthesis process, leaving many positive vacancies on the polymer chain. When a positive voltage is applied to the anode, the anions in the salt solution are attracted to the positive vacancies and enter the electrode. On the contrary, when the anion B is doped with the polymer, since it is not easy to dedope, these undesorbed anions B can achieve ion adsorption with the cations in the solution through electrostatic action.

[0015] Preferably, the ionic radius of the anion A is smaller than that of the anion B.

[0016] In the present invention, by controlling the ionic radius of anion A to be smaller than that of anion B, the conductive polymer electrode film doped with anion A having a small ionic radius is easy to dedope, so that it contains corresponding anion vacancies and is positively charged; at the same time, due to its large ionic radius and long molecular chain structure, the conductive polymer electrode film doped with anion B having a large ionic radius is difficult to dedope and is negatively charged, so there are cation vacancies.

[0017] Preferably, the anion A comprises Cl - ,I - 、ClO4 - or NO3 - Any one or a combination of at least two of - ,I - 、ClO4 - or NO3 - For the sake of brevity, the combinations within the above range will not be listed one by one.

[0018] Preferably, the anion B comprises a dodecylbenzenesulfonate anion (DBS - ), p-toluenesulfonate anion (TsO - ), m-nitrobenzenesulfonate anion, 3-carboxybenzenesulfonate anion or polystyrenesulfonate anion (PSS - ) or a combination of at least two thereof, for example, DBS - , TsO - , m-nitrobenzenesulfonate anion, 3-carboxybenzenesulfonate anion or PSS - For the sake of brevity, the combinations within the above range will not be listed one by one.

[0019] Preferably, the carbon material matrix includes any one of carbon nanofibers, activated carbon or carbon aerogel, or a combination of at least two of them.

[0020] Preferably, the conductive polymer includes any one of polypyrrole, polyaniline or polythiophene or a combination of at least two thereof, for example, polypyrrole and polyaniline, polyaniline or polythiophene. For the sake of brevity, the combinations within the above range are not listed one by one.

[0021] In the present invention, the carbon material matrix electrode coated with a conductive polymer provides a continuous and stable framework and sufficient ion adsorption centers, thereby enhancing the stability, conductivity and ion selectivity of the electrode material.

[0022] In the present invention, the membrane capacitor deionization and desalination module further comprises a partition, which is arranged between the anion exchange membrane and the cation exchange membrane and is used for storing water and separating electrodes to prevent short circuit.

[0023] In a second aspect, the present invention provides a method for preparing the membrane capacitor deionization and desalination module according to the first aspect, the method comprising the following steps:

[0024] (1) mixing a precursor containing anion A and an optional solvent, and adding a monomer to form an electrolyte solution A, and then immersing a carbon material substrate in the electrolyte solution A for electrodeposition and activation, and drying to obtain the anode;

[0025] (2) mixing a precursor containing anions B and an optional solvent, and adding a monomer to form an electrolyte solution B, and then immersing the carbon material substrate in the electrolyte solution B for electrodeposition, and drying to obtain the cathode;

[0026] (3) Assembling the anode obtained in step (1), the cathode obtained in step (2) and the ion exchange membrane to obtain the membrane capacitor deionization and desalination module.

[0027] In the present invention, the ion selective electrode prepared by the present invention avoids the use of a binder and increases more adsorption active sites. In addition, the electrode has a relatively simple manufacturing process, a long service life, and is easy to achieve large-scale production, providing an industrial application basis for the selective removal and enrichment of specific ions.

[0028] Preferably, the precursor containing anion A in step (1) comprises at least two of a coordination acid solution containing anion A, a coordination salt solution containing anion A, or a single substance.

[0029] Preferably, the coordination acid solution containing anion A includes any one of hydrochloric acid solution, hydroiodic acid solution, perchloric acid solution or nitric acid solution, or a combination of at least two thereof, for example, it can be hydrochloric acid solution, hydroiodic acid solution, perchloric acid solution or nitric acid solution. For the sake of space brevity, the combinations within the above range are no longer listed one by one.

[0030] Preferably, the concentration of the coordination acid solution containing anion A is 0.05-0.2 mol / L, for example, 0.05 mol / L, 0.08 mol / L, 0.1 mol / L, 0.12 mol / L, 0.15 mol / L, 0.18 mol / L, or 0.2 mol / L.

[0031] In the present invention, the concentration of the coordination acid solution containing anion A is adjusted so that the pH of the solution is in the range of 2 to 3.5; if the concentration is too low, ie pH>4, polymerization will not be possible, and vice versa, the electroactivity will be lost.

[0032] Preferably, the coordination salt solution containing anion A includes a sodium salt solution or a potassium salt solution.

[0033] Preferably, the concentration of the coordination salt solution containing anion A is 0.01-0.1 mol / L, for example, 0.01 mol / L, 0.03 mol / L, 0.05 mol / L, 0.08 mol / L, or 0.1 mol / L.

[0034] In the present invention, the concentration of the coordination salt solution containing anion A is adjusted to a concentration range of 0.01-0.1 mol / L; if the concentration is too low, polymerization will not occur, and vice versa, the electroactivity will be lost.

[0035] Preferably, the solvent in step (1) is deionized water.

[0036] Preferably, the temperature of the addition in step (1) is -2-0°C, for example, -2°C, -1°C, or 0°C.

[0037] Preferably, the monomer in step (1) includes any one of pyrrole, aniline or thiophene or a combination of at least two thereof, for example, pyrrole, aniline or thiophene. For the sake of brevity, the combinations within the above range are not listed one by one.

[0038] Preferably, the concentration of the monomer in step (1) is 0.1-1.0 mol / L, for example, 0.1 mol / L, 0.2 mol / L, 0.5 mol / L, 0.8 mol / L, or 1.0 mol / L.

[0039] In the present invention, the concentration of the monomer in step (1) is adjusted to be 0.1-1.0 mol / L. If the concentration is too low, polymerization will not occur, and if the concentration is too high, the electroactivity will be lost.

[0040] Preferably, the voltage of the electrodeposition in step (1) is -0.8-2.5V, for example, it can be -0.8V, -0.5V, -0.3V, 0V, 0.5V, 0.8V, 1V, 1.2V, 1.5V, 1.8V, 2V, 2.2V, 2.5V.

[0041] Preferably, the scanning rate of the electrodeposition in step (1) is 5-50 mV / s, for example, it can be 5 mV / s, 8 mV / s, 10 mV / s, 15 mV / s, 20 mV / s, 25 mV / s, 30 mV / s, 35 mV / s, 40 mV / s, 45 mV / s, 50 mV / s.

[0042] Preferably, the electrodeposition time in step (1) is 17-50 min, for example, 17 min, 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, or 50 min.

[0043] Preferably, the activation in step (1) includes soaking in a coordination acid solution containing anion A.

[0044] In the present invention, the soaking time is 12-24 hours, for example, it can be 12 hours, 16 hours, 18 hours, 20 hours, 22 hours, or 24 hours.

[0045] Preferably, the activation in step (1) is carried out in deionized water.

[0046] Preferably, the activation time in step (1) is 500-3600 s, for example, 500 s, 800 s, 1000 s, 1200 s, 1500 s, 1800 s, 2000 s, 2200 s, 2500 s, 2800 s, 3000 s, 3200 s, 3400 s, or 3600 s.

[0047] Preferably, the precursor containing anion B in step (2) comprises at least two of a coordination acid solution containing anion B, a coordination salt solution containing anion B, or a single substance.

[0048] Preferably, the coordination acid solution containing the anion B comprises any one of dodecylbenzenesulfonic acid solution, p-toluenesulfonic acid solution, m-nitrobenzenesulfonic acid solution, 3-carboxybenzenesulfonic acid solution or polystyrenesulfonic acid solution, or a combination of at least two thereof. For example, it may be dodecylbenzenesulfonic acid solution, p-toluenesulfonic acid solution, m-nitrobenzenesulfonic acid solution, 3-carboxybenzenesulfonic acid solution or polystyrenesulfonic acid solution. For the sake of brevity, the combinations within the above range are no longer listed one by one.

[0049] Preferably, the concentration of the coordination acid solution containing anion B is 0.05-0.2 mol / L, for example, 0.05 mol / L, 0.08 mol / L, 0.1 mol / L, 0.12 mol / L, 0.15 mol / L, 0.18 mol / L, 0.2 mol / L.

[0050] In the present invention, the concentration of the coordination acid solution containing anions B is adjusted so that the pH of the solution is in the range of 2 to 3.5; if the concentration is too low, ie, pH>4, polymerization will not be possible, and vice versa, the electroactivity will be lost.

[0051] Preferably, the coordination salt solution containing anion B includes a sodium salt solution or a potassium salt solution.

[0052] Preferably, the concentration of the coordination salt solution containing anion B is 0.01-0.1 mol / L, for example, 0.01 mol / L, 0.03 mol / L, 0.05 mol / L, 0.08 mol / L, or 0.1 mol / L.

[0053] In the present invention, the concentration of the coordination salt solution containing the anion B is adjusted to a concentration range of 0.01-0.1 mol / L. If the concentration is too low, polymerization will not occur, and if the concentration is too high, the electroactivity will be lost.

[0054] Preferably, the solvent in step (2) is deionized water.

[0055] Preferably, the temperature of the addition in step (2) is -2-0°C, for example, -2°C, -1°C, or 0°C.

[0056] Preferably, the monomer in step (2) includes any one of pyrrole, aniline or thiophene or a combination of at least two thereof, for example, pyrrole, aniline or thiophene. For the sake of brevity, the combinations within the above range are not listed one by one.

[0057] Preferably, the concentration of the monomer in step (2) is 0.1-1.0 mol / L, for example, 0.1 mol / L, 0.2 mol / L, 0.5 mol / L, 0.8 mol / L, or 1.0 mol / L.

[0058] In the present invention, the concentration of the monomer in step (2) is adjusted to be 0.1-1.0 mol / L. If the concentration is too low, polymerization will not occur, and if the concentration is too high, the electroactivity will be lost.

[0059] Preferably, the voltage of the electrodeposition in step (2) is -0.8-2.5V, for example, it can be -0.8V, -0.5V, -0.3V, 0V, 0.5V, 0.8V, 1V, 1.2V, 1.5V, 1.8V, 2V, 2.2V, 2.5V.

[0060] Preferably, the scanning rate of the electrodeposition in step (2) is 5-50 mV / s, for example, it can be 5 mV / s, 8 mV / s, 10 mV / s, 15 mV / s, 20 mV / s, 25 mV / s, 30 mV / s, 35 mV / s, 40 mV / s, 45 mV / s, 50 mV / s.

[0061] Preferably, the electrodeposition time in step (2) is 17-50 min, for example, 17 min, 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, or 50 min.

[0062] Preferably, the activation in step (2) includes soaking in a coordination acid solution containing anion B.

[0063] In the present invention, the soaking time is 12-24 hours, for example, it can be 12 hours, 16 hours, 18 hours, 20 hours, 22 hours, or 24 hours.

[0064] Preferably, the activation in step (2) is carried out in deionized water.

[0065] Preferably, the activation time in step (2) is 500-3600 s, for example, 500 s, 800 s, 1000 s, 1200 s, 1500 s, 1800 s, 2000 s, 2200 s, 2500 s, 2800 s, 3000 s, 3200 s, 3400 s, or 3600 s.

[0066] In a third aspect, the present invention provides a membrane capacitor deionization and desalination device, comprising an end plate and the membrane capacitor deionization and desalination module according to the first aspect.

[0067] Preferably, the end plates are arranged on both sides of the membrane capacitor deionization and desalination module.

[0068] In the present invention, the edges of the end plates are sealed and fixed to each other by sealing materials; the electrode is located between the end plate and the ion exchange membrane; the two oppositely arranged ion exchange membranes, the anion and cation exchange membranes are respectively arranged between the electrode and the partition, and are respectively in contact with the anode and cathode electrodes.

[0069] Compared with the prior art, the present invention has the following beneficial effects:

[0070] The present invention uses an ordered carbon material as a matrix, and electrodeposits a redox-doped conductive polymer with ion vacancies of different ionic radii, thereby being able to "synergistically and efficiently" adsorb specific anion and cation pairs in a salt solution during the desalination process. On the one hand, the present invention uses a carbon material as a matrix, which enhances the conductivity of the electrode and solves the problem that traditional conductive polymer materials are prone to agglomeration and poor cycle stability when used alone. On the other hand, the present invention can increase active adsorption sites and improve the adsorption amount during the desalination process by asymmetric doping, so that it has the advantages of high adsorption capacity, high electrode cycle stability, and high charge efficiency during the adsorption process. Therefore, the membrane capacitor deionization and desalination module provided by the present invention has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0071] Figure 1 is a schematic diagram of the preparation process of the electrode in Example 1, wherein the enlarged image is a SEM image of the carbon nanofiber membrane and the electrode;

[0072] Figure 2 is a photograph of the anode prepared in Example 1;

[0073] Figure 3 is a photograph of the cathode prepared in Example 1;

[0074] Figure 4 This is a SEM image of the anode prepared in Example 1, with a scale of 5 μm;

[0075] Figure 5 This is a SEM image of the cathode prepared in Example 1, with a scale of 5 μm;

[0076] Figure 6 The cyclic voltammetry spectrum of the electrode prepared in Example 1 at a scan rate of 1 mV / s;

[0077] Figure 7 is the AC impedance spectrum of the electrode prepared in Example 1;

[0078] Figure 8 This is a cycle performance diagram of the electrode prepared in Example 1 at a current density of 1 A / g;

[0079] Fig. 9A bar graph of the electrosorption capacity of the membrane capacitor deionization and desalination device provided in Application Example 1 under 50 membrane capacitor deionization and desalination cycles in a salt water desalination experimental test;

[0080] Fig.10 This is a SEM image of the electrode prepared in Comparative Example 1, with a scale of 5 μm;

[0081] Fig.11 This is a cycle performance diagram of the electrode prepared in Comparative Example 1 at a current density of 1 A / g. DETAILED DESCRIPTION

[0082] The technical solution of the present invention is further described below by combining the accompanying drawings and specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0083] Example 1

[0084] The present embodiment provides a membrane capacitor deionization and desalination module, which comprises an anode, a cathode and an ion exchange membrane; the anode comprises a carbon nanofiber membrane and Cl deposited in the carbon nanofiber membrane. - doped polypyrrole; the cathode comprises a carbon nanofiber membrane and DBS deposited in the carbon nanofiber membrane - Doped polypyrrole.

[0085] The preparation method of the membrane capacitor deionization and desalination module is as follows: Figure 1 As shown:

[0086] (1) Electrospinning polyacrylonitrile (PAN) nanofiber membrane: PAN was dissolved in N,N-dimethylformamide to obtain a spinning solution in which the mass fraction of PAN was 8 wt.%, and stirred at 60 °C overnight. A high-voltage power supply of 14-20 kV was connected to an 18G stainless steel needle, and a grounded graphite paper was used as a receiver for the electrospinning process. A PAN membrane was obtained at an injection rate of 0.4-1 mL / h. In addition, the conductivity of the electrode significantly affects the electron transfer rate during the desalination process. In order to increase the conductivity of carbon nanofibers, 10 wt.% Ti3C2T x As a conductive enhancement phase;

[0087] (2) Preparation of PAN-based carbon nanofiber membrane: The electrospun PAN nanofiber membrane was pre-oxidized in air at a heating rate of 3°C / min, calcined at 90°C and 180°C for 30 min, and stored at 270°C for 60 min. Then it was naturally cooled in the furnace and transferred to a gas phase tube furnace for carbonization at 800°C in a nitrogen atmosphere at a heating rate of 3°C / min. After keeping the temperature for 90 min, a carbon nanofiber membrane (MCNF) was prepared.

[0088] (3) Preparation of anode: 0.07 mol / L sodium chloride solution and 0.1 mol / L hydrochloric acid solution were mixed, and 0.1 mol / L pyrrole monomer was added in an ice bath to form electrolyte solution A, and then the carbon nanofiber membrane was immersed in electrolyte solution A for electrodeposition and activation. The specific process is: electrochemical polymerization was carried out at a constant potential of 0.8 V in a three-electrode system, and the electrodeposition time was 3000 s. After immersing in 1 mol / L hydrochloric acid solution for 24 h, the electrode was reduced and activated in deionized water at a constant potential of -0.2 V for 1000 s to remove the doped Cl - Finally, the product with Cl was dried under vacuum at 80 °C for 12 h. - Vacancy anode (MCNF@PPy + Cl - );

[0089] (4) Preparation of cathode: 0.07 mol / L DBSNa solution and 0.1 mol / L HDBS solution were mixed, and 0.1 mol / L pyrrole monomer was added in an ice bath to form electrolyte solution B, and then the carbon nanofiber membrane was immersed in electrolyte solution B for electrodeposition and activation. The specific process is: electrochemical polymerization was carried out at a constant potential of 0.8 V under a three-electrode system, and the electrodeposition time was 3000 s. After immersion in 1 mol / L HDBS solution for 24 h, the electrode was reduced and activated in deionized water at a constant potential of -0.2 V for 1000 s to remove the doped DBS. - Finally, the cathode (MCNF@PPy + DBS - );

[0090] (3) Assembling the anode obtained in step (1), the cathode obtained in step (2) and the ion exchange membrane to obtain a membrane capacitor deionization and desalination module.

[0091] Figure 2-Figure 3 This shows that the electrode material prepared in Example 1 has self-supporting properties. Figure 4-Figure 5 This indicates that the electrode material prepared in Example 1 has a fibrous structure.

[0092] Example 2

[0093] The difference between this embodiment and embodiment 1 is that the preparation process of the anode is as follows: I2 and KI with a molar ratio of 1:1 are added to deionized water and stirred and mixed, and 0.3 mol / L pyrrole monomer is added in an ice bath to form electrolyte solution A, and then the carbon nanofiber membrane is immersed in electrolyte solution A for electrodeposition and activation. The specific process is: electrochemical polymerization is carried out at a constant potential of 0.85V in a three-electrode system, and the electrodeposition time is 90min. After soaking in a 1mol / L hydroiodic acid solution for 24h, the electrode is reduced and activated in deionized water at a constant potential of -0.8V for 3600s to remove the doped I3 - Finally, vacuum drying was performed at 80 °C for 12 h to obtain I3 - The anode is vacant, and the rest is the same as in Example 1.

[0094] Example 3

[0095] The difference between this embodiment and embodiment 1 is that the preparation process of the cathode is as follows: 0.1mol / L p-toluenesulfonic acid (TsOH) solution and 0.3mol / L sodium p-toluenesulfonate (TsONa) solution are mixed, and 0.3mol / L pyrrole monomer is added in an ice bath to form electrolyte solution B, and then the carbon nanofiber membrane is immersed in electrolyte solution B for electrodeposition and activation. The specific process is: electrochemical polymerization is carried out at a constant potential of 0.8V under a three-electrode system, and the electrodeposition time is 3000s. After soaking in 1mol / L TsOH solution for 24h, the electrode is reduced and activated in deionized water at a constant potential of -0.2V for 1000s to remove the doped TSO - Finally, vacuum drying was performed at 80° C. for 12 h to obtain a cathode with cation vacancies. The other steps were the same as those in Example 1.

[0096] Example 4

[0097] The difference between this embodiment and embodiment 1 is that the preparation process of the anode is as follows: 0.07mol / L sodium chloride solution and 0.1mol / L hydrochloric acid solution are mixed, and 0.1mol / L aniline monomer is added in an ice bath to form electrolyte solution A, and then the carbon nanofiber membrane is immersed in electrolyte solution A for electrodeposition and activation. The specific process is: electrochemical polymerization is carried out at a constant potential of 0.75V in a three-electrode system, and the electrodeposition time is 3000s. After immersing in 1mol / L hydrochloric acid solution for 24h, the electrode is reduced and activated in deionized water at a constant potential of -0.2V for 1000s to remove the doped Cl - Finally, the product with Cl was dried under vacuum at 80 °C for 12 h. - The anode is vacant, and the rest is the same as in Example 1.

[0098] Example 5

[0099] The difference between this embodiment and embodiment 1 is that the anode is prepared as follows: 0.01mol / L sodium chloride solution and 0.05mol / L hydrochloric acid solution are mixed, and 0.1mol / L pyrrole monomer is added in an ice bath to form electrolyte solution A, and then the carbon nanofiber membrane is immersed in electrolyte solution A for electrodeposition and activation. The specific process is: electrochemical polymerization is carried out at a constant potential of -0.8V in a three-electrode system, the scanning rate is 5mV / s, and the electrodeposition time is 17min. After soaking in 1mol / L hydrochloric acid solution for 24h, the electrode is reduced and activated in deionized water at a constant potential of -0.2V for 500s to remove the doped Cl - Finally, the product with Cl was dried under vacuum at 80 °C for 12 h. - Vacant anode;

[0100] The cathode was prepared as follows: 0.01 mol / L DBSNa solution and 0.05 mol / L HDBS solution were mixed, and 0.1 mol / L pyrrole monomer was added in an ice bath to form electrolyte solution B, and then the carbon nanofiber membrane was immersed in electrolyte solution B for electrodeposition and activation. The specific process is: electrochemical polymerization was carried out at a constant potential of -0.8 V under a three-electrode system, the scan rate was 5 mV / s, and the electrodeposition time was 17 min. After soaking in 1 mol / L HDBS solution for 24 h, the electrode was reduced and activated in deionized water at a constant potential of -0.2 V for 500 s to remove the doped DBS. - Finally, vacuum drying was performed at 80° C. for 12 h to obtain a cathode with cation vacancies. The other steps were the same as those in Example 1.

[0101] Example 6

[0102] The difference between this embodiment and embodiment 1 is that the anode is prepared as follows: 0.1mol / L sodium chloride solution and 0.2mol / L hydrochloric acid solution are mixed, and 1mol / L pyrrole monomer is added in an ice bath to form electrolyte solution A, and then the carbon nanofiber membrane is immersed in electrolyte solution A for electrodeposition and activation. The specific process is: electrochemical polymerization is carried out at a constant potential of 2.5V in a three-electrode system, the scanning rate is 50mV / s, and the electrodeposition time is 50min. After soaking in 1mol / L hydrochloric acid solution for 24h, the electrode is reduced and activated in deionized water at a constant potential of -0.2V for 1000s to remove the doped Cl - Finally, the product with Cl was dried under vacuum at 80 °C for 12 h. - Vacant anode;

[0103] The cathode was prepared as follows: 0.1 mol / L DBSNa solution and 0.2 mol / L HDBS solution were mixed, and 1 mol / L pyrrole monomer was added in an ice bath to form electrolyte solution B, and then the carbon nanofiber membrane was immersed in electrolyte solution B for electrodeposition and activation. The specific process is: electrochemical polymerization was carried out at a constant potential of 2.5V under a three-electrode system, the scan rate was 50mV / s, and the electrodeposition time was 50min. After soaking in 1 mol / L HDBS solution for 24h, the electrode was reduced and activated in deionized water at a constant potential of -0.2V for 1000s to remove the doped DBS. - Finally, vacuum drying was performed at 80° C. for 12 h to obtain a cathode with cation vacancies. The other steps were the same as those in Example 1.

[0104] Example 7

[0105] The difference between this embodiment and embodiment 1 is that the preparation of the anode is as follows: 0.005 mol / L sodium chloride solution and 0.025 mol / L hydrochloric acid solution are mixed; the preparation of the cathode is as follows: 0.005 mol / L DBSNa solution and 0.025 mol / L HDBS solution are mixed, and the rest are the same as embodiment 1.

[0106] Example 8

[0107] The difference between this embodiment and embodiment 1 is that the preparation of the anode is as follows: 0.2 mol / L sodium chloride solution and 0.4 mol / L hydrochloric acid solution are mixed; the preparation of the cathode is as follows: 0.2 mol / L DBSNa solution and 0.4 mol / L HDBS solution are mixed, and the rest are the same as embodiment 1.

[0108] Example 9

[0109] The difference between this embodiment and embodiment 1 is that 0.05 mol / L pyrrole monomer is added during the preparation of the anode and the cathode, and the rest is the same as embodiment 1.

[0110] Example 10

[0111] The difference between this embodiment and embodiment 1 is that 2 mol / L pyrrole monomer is added during the preparation of the anode and the cathode, and the rest is the same as embodiment 1.

[0112] Comparative Example 1

[0113] The difference between this comparative example and Example 1 is that during the preparation process, the carbon nanofibers are replaced by graphite paper, and only steps (1) to (3) are performed, and step (4) is not performed, and the prepared electrode is used as both an anode and a cathode, and the rest is the same as Example 1.

[0114] Fig.10 This indicates that the electrode prepared in Comparative Example 1 has an agglomerated spherical structure.

[0115] Comparative Example 2

[0116] The difference between this comparative example and Example 1 is that, during the preparation process, only steps (1), (2) and (4) are performed, and step (3) is not performed, and the prepared electrode is used as both an anode and a cathode, and the rest is the same as Example 1.

[0117] Comparative Example 3

[0118] This comparative example provides a membrane capacitor deionization and desalination module, which includes an anode, a cathode and an ion exchange membrane. The anode and the cathode are both made of activated carbon electrode materials.

[0119] Comparative Example 4

[0120] This comparative example provides a membrane capacitor deionization and desalination module, which includes an anode, a cathode and an ion exchange membrane. The anode includes a carbon nanofiber membrane and a conductive polymer doped with sodium ions deposited in the carbon nanofiber membrane; the cathode includes a carbon nanofiber membrane and a conductive polymer doped with chloride ions deposited in the carbon nanofiber membrane.

[0121] Application Examples 1 to 10 and Comparative Application Examples 1 to 4

[0122] The membrane capacitor deionization and desalination modules provided in Examples 1 to 10 and Comparative Examples 1 to 4 are assembled into a membrane capacitor deionization and desalination device, and the assembly method is as follows:

[0123] The end plates are arranged on both sides of the membrane capacitor deionization and desalination module, and the edges of the end plates are sealed and fixed to each other using sealing materials; the electrodes are located between the end plates and the ion exchange membranes; the two oppositely arranged ion exchange membranes, the anion and cation exchange membranes are respectively arranged between the electrodes and the partitions, and are respectively in contact with the anode and cathode electrodes.

[0124] Test conditions

[0125] The electrodes provided in Examples 1 to 10 and Comparative Examples 1 to 4 were subjected to performance tests, and the test methods were as follows:

[0126] (1) AC impedance test: The electrochemical test was performed using a three-electrode electrochemical workstation, with a platinum sheet as the counter electrode, Ag / AgCl as the reference electrode, and 1 mol / L sodium chloride solution as the electrolyte. The interference voltage was 5 mV and the range was 0.1-10 5 AC impedance test is performed within the frequency range of Hz;

[0127] (2) Cyclic voltammetry test: Using Ag / AgCl as the reference electrode, cyclic voltammetry test was performed in the electrochemical window of -0.4V-0.6V at a scan rate of 1mV / s, wherein the specific capacitance C (F / g) is calculated as follows:

[0128]

[0129] Where V1(V) and V2(V) are the starting potential and ending potential respectively, i(A) is the response current, m(g) is the effective electrode mass, v(V / s) is the scanning speed, and ΔV(V) is the voltage change.

[0130] (3) Constant current charge and discharge test: The electrode was cycled at a current density of 1 A / g. The corresponding specific capacitance C (F / g) can be calculated based on the corresponding charge and discharge curve and the following formula:

[0131]

[0132] Among them, I (A) is the response current, Δt (s) is the discharge time, m (g) is the electrode mass, and ΔV (V) is the voltage change value.

[0133] Figure 6 This indicates that the electrode prepared in Example 1 has a higher specific capacitance; Figure 7 It is shown that the impedance of the electrode prepared in Example 1 is relatively small, which is mainly due to the continuous fiber framework and the conductive polymer coating layer with high pseudocapacitive properties, which greatly promotes the rapid transfer of charges in the electrolyte solution; Figure 8 It shows that the electrode prepared in Example 1 has a high specific capacitance and good cycle stability, which lays a foundation for the high adsorption capacity and good cycle stability of the subsequent asymmetric membrane capacitor deionization and desalination device.

[0134] The test results are shown in Table 1:

[0135] Table 1

[0136]

[0137]

[0138] It can be seen from the data in Table 1 that within the appropriate deposition conditions (Application Examples 1-6), based on the pseudocapacitive mechanism of the conductive polymer, the electrodes coated with the conductive polymer all exhibit excellent conductivity and high electrode capacity. Due to the difference in the deposition liquid system (organic and inorganic), the capacity of the cation-doped conductive polymer composite electrode is slightly smaller than that of the anion-doped composite electrode under the same conditions, but the cation-doped conductive polymer composite electrode is more stable after 250 cycles at a current density of 1A / g. However, when the concentration of the dopant and the coordination acid, as well as the concentration of the conductive polymer to be deposited are too low (Application Example 7, Application Example 9), the conductive polymer cannot be coordinated and undergo polymerization reaction, resulting in polymerization failure, and no product is generated, so it cannot be detected. On the contrary, when the concentration of the dopant and the coordination acid is too high (Application Example 8), due to the low relative concentration of the conductive polymer monomer to be deposited, only a few monomers can be polymerized, resulting in poor conductivity and low electrode capacity of the obtained composite electrode; and when the concentration of the conductive polymer monomer to be deposited is high (Application Example 10), it can fully polymerize and coordinate with the coordination ions in the solution during the electrodeposition process, and the obtained composite electrode has the characteristics of high conductivity and high electrode capacitance. However, due to the high monomer concentration, the formation morphology of the conductive polymer and the polymer chain during the deposition process have many defects, resulting in poor electrode cycle stability. The base material of the electrode obtained in Comparative Examples 1 and 2 and Example 1 is graphite paper, which is smooth and non-porous throughout. The conductive polymer obtained by electrodeposition shows the characteristics of irregular spherical agglomeration, thereby affecting the transmission channel of ions and electrons, and the insertion and removal of ions during the charge and discharge process aggravates the volume expansion of the conductive polymer, resulting in poor cycle stability. The electrode used in Comparative Example 3 is a traditional activated carbon electrode. During the electrochemical test of the electrolyte solution, no redox reaction occurs, and double-layer adsorption is performed only by its own specific surface area. Therefore, the electrode capacity is relatively low, but since no ion insertion and extraction occurs during charging and discharging, it still has high stability after cycling. The electrode used in Comparative Example 4 does not undergo any activation treatment, resulting in the deposited conductive polymer having no specific ion vacancies, so the conductivity and electrode capacity are lower than the electrode prepared in Example 1. The comprehensive parameters of the above electrodes are compared. Thanks to the regular fiber network framework, the electrode prepared in Example 1 has the advantages of faster ion and electron transmission rate, higher electrode capacity and stable electrode cycle. In summary, the method in Example 1 is the best.

[0139] The membrane capacitor deionization and desalination devices provided in Application Examples 1 to 10 and Comparative Application Examples 1 to 4 were subjected to desalination tests:

[0140] (1) Electrochemical desalination test: The membrane capacitor deionization module is connected to a DC voltage circuit to form a closed loop. The voltage range of the DC voltage circuit to the positive and negative electrodes is 1.2V. A peristaltic pump is used to send the saline solution to be treated from the water reservoir to the capacitor deionization module, and finally flows back to the water reservoir. The concentration of the saline solution is 500mg / L, and the flow rate of the saline solution is 15mL / min. First, a 1.2V voltage is applied to the module using a DC voltage circuit, and then an opposite voltage is applied to the two electrodes of the module for desorption. A conductivity meter is used to detect the conductivity of the salt solution to be adsorbed at the outlet of the membrane capacitor deionization module in real time to determine the adsorption amount. The adsorption time is 20min. After the electrode reaches adsorption saturation, an opposite voltage is applied for desorption. The desorption time is 20min. Repeat steps (1)-(3) to proceed to the next desalination process.

[0141] (2) Salt water desalination test: During the charge and discharge process of the membrane capacitor deionization desalination device, a DC power supply was used to operate in a constant potential mode (1.2V). A peristaltic pump was used to pump a sodium chloride solution (volume 50mL, concentration 500mg / L) into the above device at an injection rate of 15mL / min, and the conductivity of the solution was recorded online using a handheld conductivity meter. The desalination capacity of the electrode can be evaluated by the saturated sodium chloride adsorption capacity (SAC, mg / g), and the average desalination rate (SAR, mg -1 min -1 ) is calculated by the following formula:

[0142]

[0143]

[0144] Where C0 (mg / L) and C1 (mg / L) are the concentrations of sodium chloride salt solution before and after seawater desalination, V (L) is the volume of sodium chloride salt solution, m (g) is the mass of the electrode, and t (s) is the adsorption time.

[0145] Fig. 9 It shows that the membrane capacitor deionization and desalination device provided in Application Example 1 has no significant loss in desalination capacity after repeated adsorption / desorption cycles. After repeated operation for 5 days under 50 adsorption and desorption cycles, the average desalination capacity of MCNF@PPy remained at 64 mg / g, with no significant performance degradation and no electrode contamination. This is in stark contrast to the phenomenon that when using polypyrrole electrodes alone, repeated insertion / deinsertion of ions leads to electrode expansion and fragmentation, as well as lower actual desalination and poor electrode stability. The energy consumption of the system at a voltage of 1.2 V is only 0.41 ± 0.007 kWh kg NaCl -1 Therefore, the hybridization of the conductive polymer with the carbon nanofiber membrane skeleton greatly improves the overall stability of the electrode. Fig.11 It shows that the electrode prepared in Comparative Example 1 induces a volume swelling effect during multiple charge and discharge cycles, and an oxidation reaction occurs, resulting in a decrease in electrical activity and an increase in ion transfer resistance, thereby resulting in extremely poor cycle stability.

[0146] The test results are shown in Table 2:

[0147] Table 2

[0148]

[0149] From the data in Table 2, we can see that thanks to the specific anion (Cl - ) and cations (Na + ) vacancies, Application Examples 1, 3, 4, 6 and 10 and Comparative Application Example 1 all show high sodium chloride adsorption in electrochemical desalination and desalination solutions. Among them, thanks to the asymmetric electrode setting, Application Example 1 has both adsorbable anion and cation vacancies, and therefore shows extremely excellent adsorption capacity. Not only that, the highly conductive fiber framework provided by the MCNF fiber electrode provides an ordered nucleation channel when depositing polymerized conductive polymers, prevents the occurrence of agglomeration, and enhances the stability of the composite electrode; increases the ion transmission rate during the desalination process, so compared with Comparative Examples 1 and 2 using graphite paper as the substrate, Application Examples 1, Application Example 3, Application Example 4 and Application Example 6 using fiber electrodes as the substrate have more excellent desalination capacity. Since the anion vacancies generated in Example 2 are 1 - , and the electrolyte solution tested was a sodium chloride solution, which did not contain I - , which results in limited salt capacity adsorbed by Example 2. The electrode used in Comparative Application Example 3 is a traditional activated carbon electrode, which only relies on its own specific surface area to undergo physical adsorption of double-layer capacitance during the adsorption process, so the desalination capacity is relatively low. Since the electrode used in Comparative Example 4 does not undergo any activation treatment, the deposited conductive polymer has no specific ion vacancies, and the ion embedding capacity is limited during the desalination process, so the desalination amount is significantly lower than that of Example 1. The comprehensive parameters of the above-mentioned electrodes are compared. Thanks to the regular fiber network framework, the electrode prepared in Example 1 has a faster transmission rate of ions and electrons, and the synergistic adsorption of anions and cations unique to the asymmetric electrode produces an ultra-high adsorption amount. In summary, the method of Example 1 is the best in sodium chloride solution.

[0150] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A membrane capacitor deionization and desalination module, characterized in that: The membrane capacitor deionization and desalination module comprises an anode, a cathode and an ion exchange membrane; The anode includes a carbon material matrix and a conductive polymer doped with anions A deposited in the carbon material matrix; The cathode comprises a carbon material matrix and a conductive polymer doped with anions B deposited in the carbon material matrix; The ionic radius of the anion A is smaller than the ionic radius of the anion B; The membrane capacitor deionization and desalination module is prepared by the following method, which comprises the following steps: (1) mixing a precursor containing anion A and an optional solvent, and adding a monomer to form an electrolyte solution A, then immersing a carbon material substrate in the electrolyte solution A for electrodeposition and activation, and drying to obtain the anode; (2) mixing a precursor containing anions B and an optional solvent, and adding a monomer to form an electrolyte solution B, and then immersing a carbon material substrate in the electrolyte solution B for electrodeposition, and drying to obtain the cathode; (3) Assembling the anode obtained in step (1), the cathode obtained in step (2) and the ion exchange membrane to obtain the membrane capacitor deionization and desalination module; Wherein, the precursor containing anion A in step (1) comprises at least two of a coordination acid solution containing anion A, a coordination salt solution containing anion A, or a single substance; The activation in step (1) is carried out in deionized water at a constant potential; The precursor containing anion B in step (2) includes at least two of a coordination acid solution containing anion B, a coordination salt solution containing anion B, or a single substance.

2. The membrane capacitor deionization and desalination module according to claim 1, characterized in that: The anion A includes Cl - ,I - 、ClO4 - or NO3 - Any one or a combination of at least two of the following.

3. The membrane capacitor deionization and desalination module according to claim 1, characterized in that: The anion B includes DBS - , TsO - , m-nitrobenzenesulfonate anion, 3-carboxybenzenesulfonate anion or PSS - Any one or a combination of at least two of the following.

4. The membrane capacitor deionization and desalination module according to claim 1, characterized in that: The carbon material matrix includes any one of carbon nanofibers, activated carbon or carbon aerogel, or a combination of at least two of them.

5. The membrane capacitor deionization and desalination module according to claim 1, characterized in that: The conductive polymer includes any one of polypyrrole, polyaniline or polythiophene, or a combination of at least two of them.

6. A method for preparing a membrane capacitor deionization and desalination module according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: (1) mixing a precursor containing anion A and an optional solvent, and adding a monomer to form an electrolyte solution A, then immersing a carbon material substrate in the electrolyte solution A for electrodeposition and activation, and drying to obtain the anode; (2) mixing a precursor containing anions B and an optional solvent, and adding a monomer to form an electrolyte solution B, and then immersing a carbon material substrate in the electrolyte solution B for electrodeposition, and drying to obtain the cathode; (3) Assembling the anode obtained in step (1), the cathode obtained in step (2) and the ion exchange membrane to obtain the membrane capacitor deionization and desalination module; Wherein, the precursor containing anion A in step (1) comprises at least two of a coordination acid solution containing anion A, a coordination salt solution containing anion A, or a single substance; The activation in step (1) is carried out in deionized water at a constant potential; The precursor containing anion B in step (2) includes at least two of a coordination acid solution containing anion B, a coordination salt solution containing anion B, or a single substance.

7. The method according to claim 6, characterized in that The coordination acid solution containing anion A includes any one of hydrochloric acid solution, hydroiodic acid solution, perchloric acid solution or nitric acid solution, or a combination of at least two of them.

8. The method according to claim 6, characterized in that The concentration of the coordination acid solution containing anion A is 0.05-0.2 mol / L.

9. The method according to claim 6, characterized in that The coordination salt solution containing anion A includes a sodium salt solution and a potassium salt solution.

10. The method according to claim 6, characterized in that The concentration of the coordination salt solution containing anion A is 0.01-0.1 mol / L.

11. The method according to claim 6, characterized in that The solvent in step (1) is deionized water.

12. The method according to claim 6, characterized in that The temperature of addition in step (1) is -2-0°C.

13. The method according to claim 6, characterized in that The monomer in step (1) includes any one of pyrrole, aniline or thiophene, or a combination of at least two of them.

14. The method according to claim 6, characterized in that The concentration of the monomer in step (1) is 0.1-1.0 mol / L.

15. The method according to claim 6, characterized in that The voltage of the electrodeposition in step (1) is -0.8-2.5V.

16. The method according to claim 6, characterized in that The scanning rate of the electrodeposition in step (1) is 5-50 mV / s.

17. The method according to claim 6, characterized in that The electrodeposition time in step (1) is 17-50 minutes.

18. The method according to claim 6, characterized in that The activation in step (1) includes soaking in a coordination acid solution containing anion A.

19. The method according to claim 6, characterized in that The activation time in step (1) is 500-3600s.

20. The method according to claim 6, characterized in that The coordination acid solution containing anion B includes any one of dodecylbenzenesulfonic acid solution, p-toluenesulfonic acid solution, m-nitrobenzenesulfonic acid solution, 3-carboxybenzenesulfonic acid solution or polystyrenesulfonic acid solution, or a combination of at least two thereof.

21. The method according to claim 6, characterized in that The concentration of the coordination acid solution containing anion B is 0.05-0.2 mol / L.

22. The method according to claim 6, characterized in that The coordination salt solution containing anion B includes sodium salt solution and potassium salt solution.

23. The method according to claim 6, characterized in that The concentration of the coordination salt solution containing anion B is 0.01-0.1 mol / L.

24. The method according to claim 6, characterized in that The solvent in step (2) is deionized water.

25. The method according to claim 6, characterized in that The temperature of addition in step (2) is -2-0°C.

26. The method according to claim 6, characterized in that The monomer in step (2) includes any one of pyrrole, aniline or thiophene, or a combination of at least two of them.

27. The method according to claim 6, characterized in that The concentration of the monomer in step (2) is 0.1-1.0 mol / L.

28. The method according to claim 6, characterized in that The voltage of the electrodeposition in step (2) is -0.8-2.5V.

29. The method according to claim 6, characterized in that The scanning rate of the electrodeposition in step (2) is 5-50 mV / s.

30. The method according to claim 6, characterized in that The time of the electrodeposition in step (2) is 17-50 minutes.

31. A membrane capacitor deionization and desalination device, characterized in that: The membrane capacitor deionization and desalination device comprises an end plate and a membrane capacitor deionization and desalination module according to any one of claims 1 to 5.

32. The membrane capacitor deionization and desalination device according to claim 31, characterized in that: The end plates are arranged on both sides of the membrane capacitor deionization and desalination module.