An anti-aging additive package and preparation method thereof and application in epoxy electronic coating adhesive

By adding a liquid anti-aging additive package to epoxy electronic coating adhesive, the poor weather resistance and yellowing problems of bisphenol A type epoxy resin were solved, achieving high-efficiency anti-aging performance and color retention of epoxy adhesive, and reducing production costs and complexity.

CN115537146BActive Publication Date: 2024-11-29JIANGMEN YANEN CHEM TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202211184330.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-27
Publication Date
2024-11-29
Estimated Expiration
2042-09-27

AI Technical Summary

Technical Problem

Bisphenol A type epoxy resin has poor weather resistance under ultraviolet radiation and is prone to yellowing. Existing solutions are costly or have complex processes, and there is a lack of economical and effective anti-aging technologies.

Method used

An anti-aging additive package consisting of a liquid hindered phenolic primary antioxidant, a liquid phosphite secondary antioxidant, an alkyl radical scavenger, a liquid ultraviolet absorber, a liquid HALS light stabilizer, and a liquid reinforcing agent is prepared by uniform mixing and filtration, and then added to epoxy electronic coating adhesive to improve weather resistance and anti-yellowing properties.

Benefits of technology

It effectively solves the problems of photoaging and thermo-oxidative aging of epoxy resin, maintains the color stability of epoxy adhesive, significantly improves weather resistance and anti-yellowing performance, and is simple to process and economical in cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The present invention belongs to the technical field of special additives, and discloses an anti-aging additive package, a preparation method and an application in epoxy electronic coating adhesive. The anti-aging additive package is a light yellow uniform transparent liquid, and is composed of the following components in percentage by mass: liquid hindered phenol main antioxidant: 10-20%, liquid phosphite auxiliary antioxidant: 0-20%, alkyl free radical scavenger 0-5%, liquid ultraviolet absorber 20-40%, liquid HALS light stabilizer 20-40%. The present invention is applied to the anti-aging additive package product of epoxy electronic coating adhesive, which not only effectively solves the problem that ordinary bisphenol A type epoxy resin is not resistant to light aging, but also solves the problem of thermal oxidation aging of epoxy resin during high temperature curing (temperature resistance can reach up to 200°C), and also has many advantages such as little effect on epoxy resin base color, and is economical in cost, simple in processing process, stable in performance and easy to use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of special additives, and specifically relates to an anti-aging additive package, a preparation method thereof, and application in epoxy electronic coating adhesive. Background Art

[0002] Electronic products are increasingly integrated into our lives, bringing great value to people. With the advancement of electronic technology, people pay more and more attention to the reliability and service life of electronic products. In order to prevent the erosion of electronic components by the natural environment, people begin to use electronic coating glue to coat or spray electronic components to achieve moisture-proof, salt spray-proof and anti-static effects. Electronic coating glue will form a layer of insulation and moisture-proof glue on the surface of electronic components, which can effectively isolate dust in the atmosphere, improve the insulation between internal components and circuits, and reduce the occurrence of short circuits.

[0003] Electronic coating adhesive is a protective coating that is applied or sprayed on electronic components. It is generally about 30μm to 210μm thick and can prevent odor, dirt, and dust for electronic components. It has excellent weather resistance and anti-aging capabilities. Applying it on electronic components can prevent solder joints and conductors from being directly exposed to the air. It can also shield and eliminate certain electromagnetic interference to ensure the stability of electronic products. Due to its many advantages, it is often used in electronic products that work in harsh environments. It is very useful for protecting circuits and maintaining a low-stress environment for components and lines.

[0004] Common electronic coating adhesives on the market are composed of various base resins. There are acrylic system, polyurethane system, epoxy system and other different types of products are widely used in the field of electronic coating adhesives. Among the many base resin systems, bisphenol A epoxy resin is widely used in the field of electronic coating adhesives because of its low price, excellent chemical stability, high coating strength and toughness and many other advantages. However, since bisphenol A epoxy resin contains active groups such as benzene rings and bisphenol A groups, it is easy to break and form free radicals under ultraviolet light. Therefore, epoxy resin is not resistant to ultraviolet rays, has poor weather resistance, is easy to yellow, and is easy to powder in application scenarios.

[0005] In view of the problem of poor weather resistance and yellowing of bisphenol A epoxy resin during application, the current solutions of the anti-aging additive industry are: (1) Selecting aliphatic epoxy resin or alicyclic epoxy resin with good weather resistance; (2) Modifying epoxy resin with other resins with good weather resistance; (3) Adding anti-aging additive products to epoxy resin to improve the weather resistance of epoxy resin.

[0006] The above idea (1) is not cost-effective due to its high price; idea (2) involves many materials in the process of epoxy resin modification, the process is complicated, and the cost is not advantageous. Idea (3) is currently the most cost-effective technical solution to improve the weather resistance of epoxy resin, but the anti-aging technical solution of epoxy resin has always been one of the difficult problems in the industry, and the selection of a suitable anti-aging formula for epoxy resin has a high technical threshold. Summary of the invention

[0007] In view of the shortcomings and deficiencies of the above prior art, the primary purpose of the present invention is to provide an anti-aging auxiliary agent package.

[0008] Another object of the present invention is to provide a method for preparing the anti-aging aid package.

[0009] Another object of the present invention is to provide the use of the above-mentioned anti-aging additive package in epoxy electronic coating adhesive.

[0010] The present invention is applied to the anti-aging additive package product of epoxy electronic coating adhesive, which not only effectively solves the problem that ordinary bisphenol A epoxy resin is not resistant to light aging, but also can solve the problem of thermal oxidation aging of epoxy resin during high-temperature curing (the temperature resistance can reach up to 200°C), and also has many advantages such as little effect on the base color of epoxy resin, is cost-effective, has a simple processing process, stable performance, and is easy to use.

[0011] The purpose of the present invention is achieved through the following technical solutions:

[0012] The invention discloses an anti-aging auxiliary agent package, which is in the form of a light yellow uniform transparent liquid and is composed of the following components in percentage by mass: 10-20% of a liquid hindered phenol main antioxidant, 0-20% of a liquid phosphite auxiliary antioxidant, 0-5% of an alkyl free radical scavenger, 20-40% of a liquid ultraviolet absorber, and 20-40% of a liquid HALS light stabilizer.

[0013] Preferably, the liquid hindered phenol main antioxidant is one or more of antioxidant 5057 (Tianjin Lianlong New Materials Co., Ltd., no repeated description below), antioxidant 1135 (Tianjin Lianlong New Materials Co., Ltd., no repeated description below), and antioxidant 245 emulsion (Tianjin Lianlong New Materials Co., Ltd., no repeated description below).

[0014] Preferably, the liquid phosphite auxiliary antioxidant is one or more of antioxidant W705 (US SI Company, no further description below), antioxidant 2190 (Guangzhou Zhiyi Chemical Co., Ltd., no further description below), and antioxidant PL-706 (Jiangsu Evergreen New Materials Technology Co., Ltd., no further description below).

[0015] Preferably, the alkyl radical scavenger is REVONOX U-5035 (produced by Taiwan Chi Tai Technology Co., Ltd., which will not be described again below).

[0016] Preferably, the liquid UV absorber is one or more of the liquid triazine UV absorber UV-400 (Tianjin Lianlong New Materials Co., Ltd., no repeated description below), the liquid benzotriazole UV absorber UV384-2 (Tianjin Lianlong New Materials Co., Ltd., no repeated description below), and the liquid phenylmethylenediamine UV absorber UV-101 (Guangzhou Zhiyi Chemical Co., Ltd., no repeated description below).

[0017] Preferably, the liquid HALS light stabilizer is light stabilizer UV-292 (Tianjin Lianlong New Materials Co., Ltd., which will not be described again below).

[0018] Preferably, 2-5% of a liquid enhancer is further added to the anti-aging aid package, and the liquid enhancer is an aminopolysiloxane with a number average molecular weight of 500-5000.

[0019] The preparation method of the above-mentioned anti-aging auxiliary agent package comprises the following preparation steps:

[0020] (1) weighing a liquid hindered phenol primary antioxidant, a liquid phosphite auxiliary antioxidant and an alkyl free radical scavenger according to a ratio, stirring and mixing them evenly for later use;

[0021] (2) The liquid UV absorber, the liquid HALS light stabilizer and the liquid enhancer are weighed according to the proportion and added to the liquid mixture of step (1), stirred thoroughly, filtered, and cooled to room temperature to obtain a clear and transparent anti-aging additive package product.

[0022] Furthermore, the stirring and mixing in step (1) refers to stirring at a speed of 400 to 600 rpm for 10 to 20 minutes.

[0023] Furthermore, the stirring in step (2) refers to stirring at a speed of 500 to 700 rpm for 10 to 30 min.

[0024] Furthermore, the filtering in step (2) refers to filtering through a 400-mesh stainless steel filter.

[0025] The application of the above anti-aging additive package in epoxy electronic coating adhesive.

[0026] Furthermore, the application process is: adding the anti-aging additive package into the epoxy electronic coating adhesive at a mass percentage of 1-3%, and then using it in the protective adhesive curing process of electronic components.

[0027] Further preferably, the epoxy electronic coating adhesive is bisphenol A type epoxy resin.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] (1) We were one of the first in the industry to propose a technical solution for the polymer chain breakage and free radicals generated by epoxy resin in the early stage of oxidation induction. This solution uses a suitable alkyl free radical scavenger to quickly capture the free radicals generated by the chain breakage of epoxy molecules, thereby slowing down the chain reaction. This is a theoretical innovation in the anti-aging of epoxy systems.

[0030] (2) For the first time, liquid phosphite-based auxiliary antioxidants are used in epoxy adhesive anti-aging technology solutions, which can give epoxy adhesive better color retention and partially reduce the unstable color-developing groups formed during the aging process of epoxy adhesive, thereby improving the anti-yellowing properties of epoxy adhesive and also improving the initial color of epoxy adhesive.

[0031] (3) The entire formula adopts a liquid anti-aging additive formula, which is convenient for addition to the epoxy adhesive and is more conducive to the dispersion of the anti-aging additive package in the epoxy adhesive, thereby improving the stability of the quality of the epoxy adhesive product and facilitating the processing and production of the epoxy adhesive. The overall formula has an obvious anti-aging synergistic effect during application.

[0032] (4) By further adding liquid aminopolysiloxane as a reinforcing agent, it has good compatibility with the liquid anti-aging agent package of a specific composition, and can obtain a uniform transparent liquid product; and the reinforcing agent can produce a cross-linking effect with the epoxy resin. On the one hand, the introduction of polysiloxane chains improves weather resistance, and on the other hand, its cross-linking effect also helps to improve the color stability of the remaining components in the anti-aging agent package, and the anti-yellowing performance of the epoxy electronic coating adhesive is further significantly improved. DETAILED DESCRIPTION

[0033] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto.

[0034] Example 1

[0035] An anti-aging additive package product for epoxy electronic coating adhesive of this embodiment includes the following components in percentage by mass:

[0036]

[0037]

[0038] The anti-aging aid package product is prepared by the following method:

[0039] (1) After weighing the liquid hindered phenol primary antioxidant 1135, the liquid phosphite auxiliary antioxidant 2190 and the alkyl free radical scavenger U-5035 according to the proportion, the mixture was placed in a 304 stainless steel barrel and stirred at 500 rpm for 15 minutes for later use;

[0040] (2) Liquid methyl methacrylate UV absorber UV-101 and HALS light stabilizer UV-292 were weighed according to the ratio and added into the liquid mixture of step (1), stirred at 600 rpm for 20 min to fully mix, filtered through a 400-mesh stainless steel filter, and cooled to room temperature to obtain a clear and transparent anti-aging additive package product.

[0041] Example 2

[0042] An anti-aging additive package product for epoxy electronic coating adhesive of this embodiment includes the following components in percentage by mass:

[0043]

[0044] The anti-aging aid package product is prepared by the following method:

[0045] (1) After weighing the liquid hindered phenol primary antioxidant 245 emulsion, the liquid phosphite auxiliary antioxidant W-705 and the alkyl free radical scavenger U-5035 according to the proportion, the mixture was placed in a 304 stainless steel barrel and stirred at 500 rpm for 15 minutes for later use;

[0046] (2) Liquid triazine ultraviolet absorber UV-400 and HALS light stabilizer UV-292 are weighed according to the ratio and added into the liquid mixture of step (1), stirred at a speed of 600 rpm for 20 min to fully mix, filtered through a 400-mesh stainless steel filter, and cooled to room temperature to obtain a clear and transparent anti-aging additive package product.

[0047] Example 3

[0048] An anti-aging additive package product for epoxy electronic coating adhesive of this embodiment includes the following components in percentage by mass:

[0049]

[0050] The anti-aging aid package product is prepared by the following method:

[0051] (1) After weighing the liquid hindered phenol primary antioxidant 5057, the liquid phosphite auxiliary antioxidant PL-706 and the alkyl free radical scavenger U-5035 according to the ratio, put them in a 304 stainless steel barrel and stir them with a stirrer at 500 rpm for 15 minutes for use;

[0052] (2) Liquid benzotriazole UV absorber UV384-2 and HALS light stabilizer UV-292 are weighed according to the ratio and added into the liquid mixture of step (1), stirred at a speed of 600 rpm for 20 min to fully mix, filtered through a 400-mesh stainless steel filter, and cooled to room temperature to obtain a clear and transparent anti-aging additive package product.

[0053] Example 4

[0054] An anti-aging additive package product for epoxy electronic coating adhesive of this embodiment includes the following components in percentage by mass:

[0055]

[0056] The anti-aging aid package product is prepared by the following method:

[0057] (1) After weighing the liquid hindered phenol primary antioxidant 245 emulsion, the liquid phosphite auxiliary antioxidant 2190 and the alkyl free radical scavenger U-5035 according to the proportion, the mixture was placed in a 304 stainless steel barrel and stirred at 500 rpm for 15 minutes before use;

[0058] (2) Liquid phenylmethylamine ultraviolet absorber UV-101 and HALS light stabilizer UV-292 are weighed according to the ratio and added into the liquid mixture of step (1), stirred at a speed of 600 rpm for 20 min to fully mix, filtered through a 400-mesh stainless steel filter, and cooled to room temperature to obtain a clear and transparent anti-aging additive package product.

[0059] Example 5

[0060] The anti-aging additive package product for epoxy electronic coating adhesive of this embodiment, compared with Example 3, further adds 4% aminopolysiloxane with a number average molecular weight of 2000, and includes the following components in percentage by weight:

[0061]

[0062] The anti-aging aid package product is prepared by the following method:

[0063] (1) After weighing the liquid hindered phenol primary antioxidant 5057, the liquid phosphite auxiliary antioxidant PL-706 and the alkyl free radical scavenger U-5035 according to the ratio, put them in a 304 stainless steel barrel and stir them with a stirrer at 500 rpm for 15 minutes for use;

[0064] (2) Liquid benzotriazole UV absorber UV384-2, HALS light stabilizer UV-292 and liquid enhancer aminopolysiloxane are weighed according to the ratio and added into the liquid mixture of step (1), stirred at a speed of 600 rpm for 20 min to fully mix, filtered through a 400-mesh stainless steel filter, and cooled to room temperature to obtain a clear and transparent anti-aging additive package product.

[0065] Comparative Example 1

[0066] Compared with Example 1, in this comparative example, no liquid hindered phenolic primary antioxidant 1135 is added to the anti-aging additive package product, and the remaining components are supplemented to 100% in the same ratio as the raw materials in Example 1.

[0067] Comparative Example 2

[0068] Compared with Example 1, in this comparative example, the liquid phosphite auxiliary antioxidant 2190 is not added to the anti-aging auxiliary agent package product, and the remaining components are supplemented to 100% in the same ratio between the raw materials as in Example 1.

[0069] Comparative Example 3

[0070] Compared with Example 1, in this comparative example, no liquid alkyl radical scavenger U-5035 is added to the anti-aging additive package product, and the remaining components are supplemented to 100% in the same ratio as the raw materials in Example 1.

[0071] Comparative Example 4

[0072] Compared with Example 1, in this comparative example, liquid phenylmethylimidazole ultraviolet absorber UV-101 is not added to the anti-aging auxiliary agent package product, and the remaining components are supplemented to 100% in the same ratio between the raw materials as in Example 1.

[0073] Comparative Example 5

[0074] Compared with Example 1, in this comparative example, no liquid light stabilizer UV-292 is added to the anti-aging additive package product, and the remaining components are supplemented to 100% in the same ratio between the raw materials as in Example 1.

[0075] The anti-aging additive package for epoxy resin prepared in the above embodiments and comparative examples was added to the epoxy electronic coating glue (the present invention uses DOW 331 standard bisphenol A epoxy resin) at a mass percentage of 1.5%, and after stirring evenly, a 20 μm adhesive film was applied to the natural color epoxy test board, and an accelerated aging test was performed using a Q-Lab aging tester, with an irradiation energy of 0.51 W / m 2 The lamp test wavelength is 340nm. After the test, the color difference of the square plate is tested using a colorimeter under a D65 light source (10° angle). The results are shown in Table 1 below:

[0076] Table 1

[0077]

[0078]

[0079] It can be seen from the above results that the anti-aging aid package product of the present invention applied to epoxy electronic batch coating adhesive can give epoxy adhesive good anti-aging performance. The QUV test was carried out using Q-LAB for 1000 hours. Compared with the initial color, the color was still well maintained. It can be seen that the addition of the anti-aging aid package of the present invention can effectively improve the weather resistance of epoxy electronic coating adhesive and can well give the anti-yellowing performance of epoxy electronic batch coating adhesive. It can be seen from the comparison results of Example 3 and Example 5 that by further adding liquid aminopolysiloxane as a reinforcing agent, a uniform transparent liquid product can be obtained, and the anti-yellowing performance of the anti-aging aid package in the application of epoxy electronic batch coating adhesive can be further improved. It can be seen from the comparison results of Example 1 and Comparative Examples 1 to 5 that the raw materials in the anti-aging aid package of the present invention have obvious synergistic effects, and the lack of any component will lead to a significant reduction in the anti-aging and yellowing performance during application.

[0080] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. Application of an anti-aging additive package in epoxy electronic coating adhesive, It is characterized in that The application process is: adding the anti-aging additive package to the epoxy electronic coating adhesive at a weight percentage of 1-3%, and then using it in the curing process of the protective adhesive of the electronic components; The anti-aging additive package is a light yellow uniform transparent liquid, and is composed of the following components in percentage by weight: liquid hindered phenol main antioxidant: 10-20%, liquid phosphite auxiliary antioxidant: 0-20%, alkyl free radical scavenger 0-5%, liquid ultraviolet absorber 20-40%, liquid HALS light stabilizer 20-40%, liquid enhancer 2-5%; The liquid hindered phenol main antioxidant is one or more of antioxidant 1135 and antioxidant 245 emulsions; the liquid phosphite auxiliary antioxidant is one or more of antioxidant W705, antioxidant 2190, and antioxidant PL-706; the alkyl free radical scavenger is REVONOX U-5035; the liquid ultraviolet absorber is one or more of liquid triazine ultraviolet absorber UV-400, liquid benzotriazole ultraviolet absorber UV384-2, and liquid phenylmethylamine ultraviolet absorber UV-101; the liquid HALS light stabilizer is light stabilizer UV-292; and the liquid enhancer is aminopolysiloxane with a number average molecular weight of 500 to 5000.

2. The use of an anti-aging additive package according to claim 1 in epoxy electronic coating adhesive, It is characterized in that The anti-aging aid package is prepared by the following method: (1) weighing a liquid hindered phenol primary antioxidant, a liquid phosphite auxiliary antioxidant and an alkyl free radical scavenger according to a ratio, stirring and mixing them evenly for later use; (2) The liquid UV absorber, the liquid HALS light stabilizer and the liquid enhancer are weighed according to the proportion and added to the liquid mixture of step (1), stirred thoroughly, filtered and cooled to room temperature to obtain a clear and transparent anti-aging additive package product.

3. Application of an anti-aging additive package according to claim 2 in epoxy electronic coating adhesive, It is characterized in that The stirring and mixing in step (1) refers to stirring at a speed of 400-600 rpm for 10-20 min; the stirring in step (2) refers to stirring at a speed of 500-700 rpm for 10-30 min; the filtering in step (2) refers to filtering through a 400-mesh stainless steel filter.

4. Application of an anti-aging additive package according to claim 1 in epoxy electronic coating adhesive, It is characterized in that The epoxy electronic coating adhesive is bisphenol A type epoxy resin.

Citation Information

Patent Citations

  • Fiber reinforced resin matrix composite weatherability improvement composition and application thereof

    CN105440580A