A method for producing fast water-absorbing ultra-soft terry fabric and terry fabric
By wrapping low-quantity water-soluble fiber rovings on high-quantity rovings in the spinning wool fabric, and pre-reducing and removing water-soluble fibers during the bleaching process, the high wastewater treatment cost caused by the dissolution of PVA fiber in the hollow core yarn products is solved. The problem has achieved efficient water resource utilization and low-cost production.
Patent Information
- Application Number
- CN202211229111.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-08
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-10-08
AI Technical Summary
The PVA fiber used in the existing hollow core yarn products in the fiber defiber removal process is dissolved in water, resulting in high wastewater treatment cost and water usage, and it is difficult to effectively reduce the proportion of PVA fiber usage.
The fast-absorbing ultra-pliable fabric production method is adopted. When spinning the wool yarn, the low-quantity water-soluble fiber roving is wrapped around the high-quantity roving to form a Sairo spinning structure. The water-soluble fiber is pre-shrinked and removed during the float training process to reduce the The amount of water-soluble fiber is used, and the spinning process is optimized through a special double-hole trumpet and false twisting device, the twist coefficient and terry length are controlled, and the water conduction channel is formed to improve hygroscopicity.
It greatly reduces the amount and water consumption of water soluble fiber, improves the softness and water absorption effect of terry fabrics, reduces the cost of wastewater treatment, and maintains the fluffy and softness of the product and reduces production costs.
Smart Images

Figure CN115538008B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of textiles, in particular to a method for producing a fast-water-absorbing ultra-soft terry fabric and the terry fabric. Background Art
[0002] Hollow yarn products are gradually becoming popular among consumers due to their unique yarn structure and physical properties. In related technologies, hollow yarn products are mainly made of PVA filament or PVA yarn as core yarn and cotton fiber as sheath. After spinning, the soluble PVA fiber is removed through the fiber withdrawal process to obtain hollow yarn products. The PVA fiber content in the core-spun yarn is mostly above 10%.
[0003] PVA fiber, also known as polyvinyl alcohol formal fiber, is dissolved in water through the defibering process. Although it is colorless and odorless, it still dissolves in water to produce tiny substances, and the cost of wastewater treatment is high. my country's textile industry uses more than 10,000 tons of PVA fiber in the form of core-spun yarn and untwisted yarn every year. Therefore, it is urgent to optimize the process of this type of product, while ensuring product performance, gradually reduce the proportion of PVA fiber used, reduce water consumption and wastewater treatment costs. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the prior art or related art.
[0005] To this end, an object of the present invention is to provide a method for producing a fast-absorbing super-soft terry fabric and a terry fabric, in which a low-quantity water-soluble fiber roving is wound around a high-quantity roving to form a siro-spun structure as the terry yarn of the terry fabric, and the water-soluble fiber is pre-shrunk and removed during the scouring and bleaching process. There is no need to remove the water-soluble PVA fiber in a separate step or two, which greatly saves water energy. In addition, the water-soluble fiber shrinks during the pre-shrinking process and drives the cotton fiber to shrink and bend, which is conducive to forming a fluffy and soft terry structure, so that the terry fabric has good softness. After removing the water-soluble fiber, a water guide channel is formed around the terry yarn body, which has good hygroscopicity and ensures the good performance of the terry fabric. At the same time, the method for producing a fast-absorbing super-soft terry fabric greatly reduces the amount of water-soluble fiber used, and the amount of water-soluble fiber used can be as low as 2.5% of the terry yarn.
[0006] In order to achieve the above-mentioned object, the technical solution of the first aspect of the present invention provides a method for producing a fast-absorbing super-soft terry fabric, comprising the following steps:
[0007] (1) Spinning terry yarn: The roving process produces two kinds of rovings with different weights, namely, low-weight water-soluble fiber roving and high-weight roving, and the weight ratio thereof is 1:2 to 1:4. The high-weight roving is pure cotton roving or roving blended with cotton fiber and other fibers, and the low-weight water-soluble fiber roving is roving blended with water-soluble fiber and cotton fiber or roving blended with water-soluble fiber, cotton fiber and other fibers, wherein the water-soluble fiber is contained in the low-weight water-soluble fiber. The content of the water-soluble fiber in the roving is 9%-30%, the roving weight is 8g / 5m-10g / 5m, two rovings with different weights are spun on a Siro compact spinning composite spinning frame or a Siro false twisting composite spinning frame to obtain terry yarn, the spinning count of the terry yarn is: single yarn 21S-8S, the twist coefficient is not higher than 279, the kilometer weight of the yarn is 27.8g-72.8g, and the weight ratio of the water-soluble fiber in the terry yarn is 2.5%-5%;
[0008] (2) Weaving a terry fabric: using the terry yarn obtained in step (1) as the warp, and cooperating with the warp yarn and weft yarn of pure cotton or cotton fiber to weave a terry fabric on a towel loom, wherein the terry fabric has a loop length of 8.5 cm-13.5 cm / 10 loops;
[0009] (3) Desizing the terry fabric: the terry fabric obtained in step (2) is fed into the fabric along the wool direction and desizing is performed on a padding machine;
[0010] (4) Pre-shrinking and scouring: After desizing, the terry fabric enters the overflow machine for pre-shrinking and scouring. After entering the water, the scouring agent is first added, and then the temperature is raised to 70℃~80℃, and the temperature is kept for 10min~20min, and then the temperature is raised to 95℃~105℃, and the temperature is kept for 30min~50min;
[0011] (5) dyeing, polishing, softening, dehydrating, drying and sewing the terry fabric treated in step (4) to obtain a super soft towel product.
[0012] In this technical solution, two kinds of rovings with different quantities are produced in the roving process, and the weight ratio of low-quantity water-soluble fiber roving and high-quantity roving is controlled to be 1:2-1:4. Terry yarn with a siro spinning structure is obtained by spinning yarns such as drawing, twisting, and winding. The water-soluble fiber in the terry yarn can be reduced to 2.5%. At the same time, the content of water-soluble fiber in the low-quantity water-soluble fiber roving is 9%-30%, which is relatively high. After removing the water-soluble fiber, the gaps between cotton fiber or cotton fiber and other fibers are large, and the water conduction speed is fast and the water absorption per unit area is large. This is conducive to reducing the quantity of water-soluble fiber while ensuring the performance of terry fabric, and controlling the twist coefficient of terry yarn to be no higher than 279, which can make the terry fabric fluffy, soft, and more absorbent. By designing the loop length of the terry fabric to be 8.5cm-13.5cm / 10 loops, the beauty, softness and low feather shedding rate of the ultra-soft towel are ensured. Too high a loop length is likely to cause the terry to be messy and pits, affecting the beauty of the towel and having a high feather shedding rate. Too low a loop length will feel hard after shrinking. By feeding the terry fabric along the wool and desizing it in a long-impregnating machine, the pre-setting of the terry fabric is achieved. The terry after long-impregnating machine is smoother, reducing the unevenness of the spiral stress of the terry and reducing the pits of the terry. The terry fabric after desizing is not dried, but loaded into an overflow machine for pre-shrinking and scouring. The pre-shrinking and scouring adopt a two-step method in the same bath. After entering the water, a scouring aid is first added, and then the temperature is raised to 70°C-80°C and kept warm for 10min-20min. During this process, the water-soluble fiber shrinks and drives the cotton fiber to shrink and bend, which is conducive to forming a fluffy and soft terry structure. The temperature is raised to 95°C-105°C and kept warm for 30min-50min, which can remove the water-soluble fiber and fully bleach it. Pre-shrinking and removing the water-soluble fiber during the scouring process does not require a separate step or two steps to remove the water-soluble fiber, which greatly reduces water consumption and water pollution. Moreover, the terry fabric has a high production rate and low cost. In the production method of the fast-absorbent ultra-soft terry fabric, the shrinkage of the water-soluble fiber is controlled before it is dissolved. The shrinkage of the water-soluble fiber drives the cotton fiber blended with the water-soluble fiber to shrink. The cotton fiber bends after shrinking, thereby making the towel fluffy, soft and resilient. The production method uses a small amount of water-soluble fiber to have the same hand feel and water absorption as hollow yarn products using a high content of water-soluble fiber in conventional technology. At the same time, even if the yarn is repeatedly washed, the hollow structure will not be damaged, and the yarn can always remain soft and has a low feather shedding rate.
[0013] Other fibers include various hemp fibers (such as flax, ramie, hemp, etc.), regenerated cellulose fibers (such as viscose, modal, lyocell, etc.), polyester fibers (such as superfine polyester, nylon, acrylic, etc.), regenerated fibers (such as regenerated polyester, regenerated nylon, regenerated acrylic), etc.
[0014] The low-quantity water-soluble fiber roving is prepared by feeding semi-cooked cotton fiber strips or semi-cooked strips mixed with cotton and other fibers into the final drawing and roving process through a bundling device together with the water-soluble fiber pre-drawing strips, with the water-soluble fiber pre-drawing strips in the middle and the semi-cooked cotton fiber strips or semi-cooked strips mixed with cotton and other fibers on the sides of the water-soluble fiber pre-drawing strips, covering the water-soluble fiber pre-drawing strips so that the water-soluble fibers are not exposed and a water guide channel can be formed after the water-soluble fibers are removed, thereby ensuring the water absorption performance of the terry fabric.
[0015] In the above technical scheme, preferably, in step (1), a special double-hole bell mouth is arranged on the siro compact spinning composite spinning machine or the siro false twist composite spinning machine, and the special double-hole bell mouth has an asymmetric double-inlet and single-outlet structure, and high-quantity roving and low-quantity water-soluble fiber roving are fed into the special double-hole bell mouth in parallel, and terry yarn is obtained after drawing, twisting and winding.
[0016] In this technical solution, due to the large difference in the special numbers of the two types of rovings, the feeding of special rovings is formed, which is not easy to form yarn. The special double-hole trumpet with an asymmetric double-inlet and single-outlet structure is adopted to ensure the yarn quality and reduce the machine breakage. The yarn has less hairiness, higher strength, low strength CV value, and obvious ply style.
[0017] In any of the above technical solutions, preferably, the distance between the two inlet holes in the special double-hole bell mouth is 4 mm to 5 mm.
[0018] In this technical solution, the distance between the two inlet holes in the special double-hole bell mouth is 4mm to 5mm, which can further ensure the yarn quality.
[0019] In any of the above technical solutions, preferably, the diameter of the upper roller on the rear roller of the spinning frame for the low-quantity water-soluble fiber roving end is increased by 0.5mm-1.0mm relative to the high-quantity roving end; the spinning frame is provided with a false twist device, through which false twist is added to the sliver output by the front roller, thereby changing the fiber distribution on the yarn surface in the twisting triangle area and controlling the yarn twist coefficient.
[0020] In this technical solution, the diameter of the low-quantity water-soluble fiber roving end is increased by 0.5mm-1.0mm relative to the high-quantity roving end by the top roller of the rear roller of the spinning frame, further ensuring that the two rovings can be spun with good quality when the special numbers are quite different, reducing the decline in drafting efficiency caused by slippery drafting and the problem of "hard head" in roving, and reducing the occurrence of broken ends. The spinning frame is equipped with a false twist device, which adds false twist to the sliver output by the front roller, changes the fiber distribution on the yarn surface in the twisting triangle area, controls the yarn twist coefficient, and makes the twist coefficient not higher than 279, which can make the terry fabric products fluffy, soft, and more absorbent.
[0021] In any of the above technical solutions, preferably, the process parameters for desizing the terry fabric in step (3) are: desizing temperature 50°C to 80°C, desizing time not less than 20 minutes, desizing agent is starch desizing enzyme, and the terry fabric after desizing is not dried.
[0022] In this technical solution, the process parameters of the desizing treatment are further defined to ensure the process effect of desizing. The terry fabric is not dried after desizing, which is conducive to subsequent pre-shrinkage. The terry fabric is pre-shaped during the desizing process, and the terry is smoother. The unevenness of the terry spiral stress and the terry pits are effectively reduced.
[0023] In any of the above technical solutions, preferably, the process parameters for weaving the terry fabric in step (2) are: ground warp density 123 to 160 strands / 10 cm, weft density 150 to 220 strands / 10 cm, and terry length 0.75 to 1.5 cm.
[0024] In this technical solution, the process parameters of weaving the terry fabric are controlled to further improve the production rate of the terry fabric. Further preferably, the ground warp density is 123 to 142 strands / 10 cm, the weft density is 160 to 190 strands / 10 cm, and the terry length is 0.85 to 1.35 cm.
[0025] In any of the above technical solutions, preferably, the scouring aids used in the pre-shrinking and scouring process in step (4) include: 27.5% by mass of hydrogen peroxide: 3g / L-8g / L; caustic soda: 3g / L-8g / L; refining agent JN-98: 1g / L-2.0g / L.
[0026] In this technical solution, the bleaching effect is good by using a scouring and bleaching aid. During the scouring and bleaching process, pre-shrinkage and removal of water-soluble fibers are achieved, saving water consumption.
[0027] In any of the above technical solutions, preferably, before the dyeing process of step (5), washing is performed at 50°C water temperature, the pH value is adjusted to 6.5-7.5, and then deoxidation treatment is performed under the condition of 0.001g / L-0.01g / L deoxidase; the dyeing process of step (5) is carried out under weak alkaline conditions of pH value of 10-13, and then hot water washing and soap washing are performed; the polishing process of step (5) is carried out under the condition of pH value of 4.0-6.5, and glacial acetic acid with a mass fraction of 80% is used for adjustment, and the terry fabric is polished by pure cotton cellulase polishing process; in the softening process of step (5), hydrophilic softener 3C-3 is used in an amount of 2g / L-5g / L; in the drying process of step (5), loose drying or vibration drying is adopted.
[0028] In this technical solution, the dyeing, polishing, softening, dehydration and drying process parameters are further optimized, which further improves the quality of the terry fabric and ensures the manufacturing effect of the terry fabric.
[0029] The technical solution of the second aspect of the present invention provides a fast-water-absorbing super-soft Terry fabric, which is made by the fast-water-absorbing super-soft Terry fabric production method described in any of the above technical solutions. The Terry yarn is a siro ring spun yarn, and a low-quantity water-soluble fiber roving is wound on a high-quantity roving. The weight ratio of the two is 1:2 to 1:4, which greatly reduces the amount of water-soluble fiber used. While ensuring the same performance of the Terry fabric, the water-soluble fiber can be as low as 2.5%, reducing the cost of water pollution treatment, reducing water consumption, saving energy consumption, and reducing production costs.
[0030] In the above technical solution, preferably, a water guide channel is formed around the terry yarn body, which has the effects of fast water guide speed and large water absorption per unit area.
[0031] The fast-absorbing ultra-soft terry fabric production method and the terry fabric proposed by the present invention have the following beneficial technical effects:
[0032] (1) In the method for producing a fast-absorbing ultra-soft terry fabric and the terry fabric proposed in the present invention, a low-quantity water-soluble fiber roving is wound around a high-quantity roving to form a siro-spun structure as the terry yarn of the terry fabric. The water-soluble fiber is pre-shrunk and removed during the scouring and bleaching process. There is no need to remove the water-soluble PVA fiber in a separate step or two, which greatly saves water energy. In addition, the water-soluble fiber shrinks during the pre-shrinking process and drives the cotton fiber to shrink and bend, which is conducive to forming a fluffy and soft terry structure, making the terry fabric soft. After removing the water-soluble fiber, a water guide channel is formed around the main body of the terry yarn, which has good hygroscopicity and ensures the good performance of the terry fabric. At the same time, the method for producing a fast-absorbing ultra-soft terry fabric greatly reduces the amount of water-soluble fiber used. The amount of water-soluble fiber used can be as low as 2.5% of the terry yarn.
[0033] (2) The fast-absorbing ultra-soft terry fabric production method and the terry fabric proposed in the present invention adopt a special double-hole trumpet with an asymmetric double-inlet and single-outlet structure, and the inlet hole spacing is designed to be 4mm-5mm, and the diameter of the low-quantity water-soluble fiber roving end of the upper roller of the rear roller of the spinning machine is increased by 0.5mm-1.0mm relative to the high-quantity roving end, etc., so that two special rovings can be fed into yarn, and the yarn quality is good, the machine is not prone to breakage, the roving is not prone to deviation, the ply style is obvious, the yarn strength is high, the yarn hairiness is less, and the strength CV value is low.
[0034] (3) The terry fabric produced by the method for producing fast-absorbing ultra-soft terry fabric proposed in the present invention is fluffy, soft, elastic, highly water-conductive, and has a low feather shedding rate. It is not only light in weight, but also has high resilience due to its fluffiness. Even if it is washed repeatedly, the hollow structure of the yarn will not be damaged, and the soft style can always be maintained. In addition, since the quantitative amount of the water-soluble fiber roving is low and the relative content of the water-soluble fiber is high, the gaps between the fibers are large after de-fibering, which has the effects of fast water conduction speed and large water absorption per unit area. Compared with the hollow yarn and untwisted yarn in the prior art, the terry fabric has the same softness, water absorption and other properties as the hollow yarn and the untwisted yarn, and at the same time, due to its low content of water-soluble fibers, it has less environmental pollution and low energy consumption cost.
[0035] Additional aspects and advantages of the present invention will be given in part in the following description, and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0037] Figure 1 A schematic structural diagram of terry yarn spun in a method for producing a fast water-absorbing super-soft terry fabric according to an embodiment of the present invention is shown;
[0038] Figure 2 The structure schematic diagram of the double-hole bell mouth in the prior art is shown;
[0039] Figure 3 The structure schematic diagram of a special double-hole bell mouth used in a method for producing a fast-absorbing super-soft terry fabric according to an embodiment of the present invention is shown.
[0040] in, Figures 1 to 3 The corresponding relationship between the reference numerals and the components is as follows:
[0041] 102 high quantitative roving, 104 low quantitative water-soluble fiber roving, 1042 cotton fiber, 1044 water-soluble fiber, 106 terry yarn, 108 double-hole bell mouth. DETAILED DESCRIPTION
[0042] The present invention discloses a method for producing a fast-absorbing ultra-soft terry fabric and a terry fabric. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve the desired effect. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art and are considered to be included in the present invention. The method and application of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the method and application described herein without departing from the content, spirit and scope of the present invention to achieve and apply the technology of the present invention.
[0043] The present invention will be further described below in conjunction with embodiments:
[0044] Example 1
[0045] A method for producing a fast-absorbing ultra-soft terry fabric comprises the following steps:
[0046] S102, selected raw materials: water-soluble fiber specification 1.33dtexX38mm, water-soluble temperature: 90℃, cotton fiber main body length 28.6mm, micronaire value 4.1, short fiber rate 10.22%, raw cotton breaking strength (raw cotton breaking ratio): 31.1cN / tex.
[0047] S104, spinning terry yarn: the water-soluble fiber and cotton fiber are respectively opened and combed into slivers, the semi-cooked cotton fiber sliver and the water-soluble fiber pre-drawing are simultaneously fed into the final drawing through a bundling device, and the roving process is performed to obtain low-weight water-soluble fiber roving with a weight of 2g / 10m; high-weight pure cotton roving with a weight of 8g / 10m and low-weight water-soluble fiber roving are spun on a Siro compact spinning composite spinning frame or a Siro false twisting composite spinning frame, and the Siro yarn is obtained as terry yarn through drawing, twisting, winding, and then winding. Figure 1 As shown, low-weight water-soluble fiber roving 104 is wound on high-weight roving 102 to make terry yarn 106. Low-weight water-soluble fiber roving is obtained by final drawing of cotton fiber 104 and water-soluble fiber 1044. The water-soluble fiber is wrapped inside the cotton fiber and is not exposed. Terry yarn 12S, designed twist 35 twists / 10cm, single yarn breaking strength: 13.9cn / tex, twist direction "Z"; yarn uniformity cv%: 7.44; comprehensive linear density weight deviation %: -0.8%. Among them, water-soluble fiber accounts for 5%, cotton fiber accounts for 95%,
[0048] Specifically, since the two types of roving have a large difference in counts, it is crucial to form roving with different counts, whether it can be made into yarn, and to ensure the quality of the yarn and reduce the number of machine breaks. Figure 2 As shown in FIG. 1 , the conventional symmetrical double-hole bell mouth 108 will cause high-frequency breakage of fine and coarse yarns, directly affecting the yarn quality and the breakage of the machine. After a large number of experimental studies, the double-hole bell mouth is designed, such as Figure 3 As shown, the special double-hole bell mouth 108 with an asymmetric double-inlet and single-outlet structure can significantly improve the yarn quality and reduce the breakage of fine and coarse yarns. The effect is better when the distance between the two inlet holes is 4mm to 5mm. The test results of 36.4tex terry yarn are shown in Table 1 below.
[0049] Table 1 Test results of 36.4tex terry yarn made with different double-hole bell-mouth structures
[0050]
[0051] As can be seen from Table 1, the asymmetric double-inlet and single-outlet structure of the special double-hole bell mouth basically does not cause the roving to break, and can realize the spinning of two rovings with a large difference in count, and the yarn quality is good.
[0052] Due to the large difference in the special rovings, when the special rovings are fed into the yarn drafting zone in parallel, it is easy to cause slippery drafting, which reduces the drafting efficiency, and the rovings have the problem of "hard ends", and the increase of yarn breakage affects the yarn quality. Therefore, after a large number of experiments and studies, the diameter of the roller at the end of the low-quantity water-soluble fiber roving is increased by 0.5mm-1mm relative to the high-quantity roving end, which significantly improves the problem of "hard ends" of the rovings and reduces the yarn breakage.
[0053] The spinning frame is equipped with a false twist device, which adds false twist to the sliver output by the front roller, changes the surface fiber distribution of the yarn in the twisting triangle area, and controls the yarn twist coefficient to be no higher than 272. A set of false twist devices is added to the compact spinning frame, which adds a certain degree of false twist to the sliver output by the front roller, thereby changing the surface fiber distribution of the yarn in the twisting triangle area. When the yarn reaches the strength of normal weaving yarn, the single yarn twist coefficient can be reduced to 200 at the lowest. After multiple tests, the twist coefficient of the yarn is within 279, and the obtained terry fabric has better fluffy, soft and water-absorbent effects.
[0054] S106, weaving a terry fabric: using a 12s ring-spun yarn as a ground warp, a 16s ring-spun yarn as a weft yarn, and the above-mentioned Si-spun yarn as a terry yarn, and weaving according to the following parameters: ground warp density: 132 yarns / 10 cm, wool warp density: 132 yarns / 10 cm, weft density: 160 yarns / 10 cm, and wool height of 1.3 cm, to obtain a terry fabric grey cloth;
[0055] S108, desizing the terry fabric: desizing and terry presetting are performed on a padding long car, the desizing temperature is 50°C-80°C, the desizing time is not less than 20 minutes, and the desizing agent is starch desizing enzyme;
[0056] S110, pre-shrinking and scouring: the terry fabric after desizing is not dried, but directly enters the overflow machine for pre-shrinking and scouring. The scouring agent is first added into the water, and the scouring agent includes: hydrogen peroxide (27.5%): 3g / l, caustic soda: 7g / l, and refining agent JN-98: 1.5g / l. Then the temperature is raised to 70℃~80℃, and the temperature is kept for 10min~20min. After that, the temperature is raised to 95℃~105℃ and kept for 30min-50min to remove the water-soluble fiber and fully bleach.
[0057] S112, performing hot washing, neutralization and deoxidation according to a conventional pure cotton product processing process, specifically, washing at 50° C., adjusting the pH value to 6.5 to 7.5, and then performing deoxidation treatment under the condition of 0.001 g / L to 0.01 g / L of deoxidase;
[0058] S114, dyeing is performed under weak alkaline conditions of pH 10-13, followed by hot water washing and soaping;
[0059] S116, using 80% by mass acetic acid to adjust the pH value to 4.0-6.5, and polishing the terry fabric using a pure cotton cellulase polishing process;
[0060] S118, using hydrophilic softener 3C-3, dosage 3.5g / L, softening finishing at 30℃ for 30min;
[0061] S120, dehydration, opening, loose drying, sewing to obtain the finished terry fabric.
[0062] The terry fabric product prepared in this embodiment is fluffy, soft and has good resilience. According to the AATCC135 method, the feather shedding rate after 5 washes is less than 5‰. The product feels super soft, has good resilience, and has a visual appearance similar to that of conventional untwisted products and super good water absorption. The wastewater pollution in this embodiment is small, the product yield is high, and the production cost is low.
[0063] The finished terry fabric obtained in Example 1 was compared with a conventional untwisted product, and the results are shown in Table 2 below.
[0064] Table 2
[0065]
[0066]
[0067] Example 2
[0068] A method for producing a fast-absorbing ultra-soft terry fabric comprises the following steps:
[0069] S202, selected raw materials: water-soluble fiber specifications: 1.33dtexX32mm, water-soluble temperature: 90℃; cotton fiber main body length: 28.2mm; Micronaire value: 4.2 short lint rate: 10.31%, raw cotton breaking strength (raw cotton breaking ratio): 31.1cN / tex; flax fiber main body length 32mm: fineness: 2200Nm, short lint rate: 12.31%.
[0070] S204, spinning terry yarn: the water-soluble fiber, cotton fiber and flax fiber are respectively opened and carded into slivers, the semi-ripened cotton fiber sliver and the water-soluble fiber pre-drawing are simultaneously fed into the final drawing and roving process through a bundling device to obtain low-weight water-soluble fiber roving with a weight of 2.5g / 10m; high-weight flax-cotton roving with a weight of 5g / 10m and low-weight water-soluble fiber roving are spun on a Siro compact spinning composite spinning frame or a Siro false twisting composite spinning frame, and the Siro yarn is obtained as terry yarn after drawing, twisting and winding, and then winding through a bobbin. Figure 1 As shown, low-weight water-soluble fiber roving 104 is wound on high-weight roving 102 to obtain terry yarn 106. Low-weight water-soluble fiber roving is obtained by final drawing of cotton fiber 104 and water-soluble fiber 1044. The water-soluble fiber is wrapped inside the cotton fiber and is not exposed. Terry yarn 8S, design twist: 25 twists / 10cm, single yarn breaking strength: 14.9cN / tex, twist direction "Z"; yarn uniformity cv%: 5.69; comprehensive linear density weight deviation %: +1.1%, of which water-soluble fiber accounts for 5%, cotton fiber accounts for 75%, and linen fiber accounts for 20%.
[0071] S206, weaving a terry fabric: using a 10s ring-spun yarn as a ground warp, a 12s ring-spun yarn as a weft yarn, and the above-mentioned siro yarn as a terry yarn, and weaving according to the following parameters: a ground warp density of 123 yarns / 10cm, a wool warp density of 132 yarns / 10cm, a weft density of 160 yarns / 10cm, and a wool height of 1.25cm, to obtain a terry fabric grey cloth;
[0072] S208, desizing the terry fabric: desizing and terry presetting are performed on a long padding machine, the desizing temperature is 50°C-80°C, the desizing time is not less than 20 minutes, and the desizing agent is starch desizing enzyme;
[0073] S210, pre-shrinking and scouring: the terry fabric after desizing is not dried, but directly enters the overflow machine for pre-shrinking and scouring. The scouring agent is first added into the water, and the scouring agent includes: hydrogen peroxide (27.5%): 3.5g / l, caustic soda: 6.5g / l, and refining agent JN-98: 1.8g / l. Then the temperature is raised to 70℃~80℃, and the temperature is kept for 10min~20min. After that, the temperature is raised to 95℃~105℃ and kept for 30min-50min to remove the water-soluble fiber and fully bleach.
[0074] S212, performing hot washing, neutralization and deoxidation according to a conventional pure cotton product processing process, specifically, washing at 50° C., adjusting the pH value to 6.5 to 7.5, and then performing deoxidation treatment under the condition of 0.001 g / L to 0.01 g / L of deoxidase;
[0075] S214, dyeing is performed under weak alkaline conditions of pH 10-13, followed by hot water washing and soaping;
[0076] S216, using 80% by mass acetic acid to adjust the pH value to 4.0-6.5, and polishing the terry fabric using a pure cotton cellulase polishing process;
[0077] S218, using hydrophilic softener 3C-3, dosage 2.8g / L, softening finishing at 30℃ for 30min;
[0078] S220, dehydration, opening, loose drying, sewing to obtain the finished terry fabric.
[0079] The terry fabric product prepared in this embodiment has a fluffy and soft feel and is highly resilient. According to the AATCC135 method, the feather shedding rate after 5 washes is less than 5‰. The product has an ultra-soft feel, good resilience, and has a visual appearance similar to that of conventional untwisted products and excellent water absorption. The wastewater pollution in this embodiment is small, the product yield is high, and the production cost is low.
[0080] The finished terry fabric obtained in Example 2 was compared with a conventional untwisted product. The results are shown in Table 3 below.
[0081] Table 3
[0082]
[0083]
[0084] Example 3
[0085] A method for producing a fast-absorbing ultra-soft terry fabric comprises the following steps:
[0086] S302, selected raw materials: water-soluble fiber specifications: 1.33dtexX38mm, water-soluble temperature: 90℃; cotton fiber main body length: 28.8mm; micronaire value: 4.0, short fiber rate: 9.81%, raw cotton breaking strength (raw cotton breaking ratio): 28.1cN / tex; zero-carbon modal fiber specifications: 1.56dtexX38mm, strength: 3.5cN / dtex.
[0087] S304, spinning terry yarn: the water-soluble fiber, cotton fiber and modal fiber are respectively opened and combed into slivers, the semi-ripened cotton fiber sliver and the water-soluble fiber pre-drawing are simultaneously fed into the final drawing and roving process through a bundling device to obtain a low-content water-soluble fiber roving with a basis weight of 2g / 10m; high-basis weight modal cotton roving with a basis weight of 8g / 10m and low-basis weight water-soluble fiber roving are spun on a Siro compact spinning composite spinning frame or a Siro false twisting composite spinning frame, and the Siro yarn is obtained as terry yarn after drawing, twisting and winding, and then winding through a bobbin, such as Figure 1 As shown, low-quantity water-soluble fiber roving 104 is wound on high-quantity roving 102 to make terry yarn 106. Low-quantity water-soluble fiber roving is obtained by final drawing of cotton fiber 104 and water-soluble fiber 1044. The water-soluble fiber is wrapped inside the cotton fiber and is not exposed. Terry yarn 21S, designed single yarn twist: 53 twists / 10cm, single yarn breaking strength: 14.1cn / tex, twist direction "Z"; yarn uniformity cv%: 6.81; comprehensive linear density weight deviation%: +0.5%; ply twist: 18 twists, twist direction "S". Among them, water-soluble fiber accounts for 2.5%, cotton fiber accounts for 67.5%, and zero-carbon modal fiber accounts for 30%.
[0088] S306, weaving a terry fabric: using a 12s ring-spun yarn as a ground warp, a 16s ring-spun yarn as a weft yarn, and the above-mentioned Si-spun yarn as a terry yarn, and weaving according to the following parameters: a ground warp density of 132 yarns / 10 cm, a wool warp density of 132 yarns / 10 cm, a weft density of 168 yarns / 10 cm, and a wool height of 11.5 cm, to obtain a terry fabric grey cloth;
[0089] S308, desizing the terry fabric: desizing and terry presetting are performed on a long padding machine, the desizing temperature is 50°C-80°C, the desizing time is not less than 20 minutes, and the desizing agent is starch desizing enzyme;
[0090] S310, pre-shrinking and scouring: the terry fabric after desizing is not dried, but directly enters the overflow machine for pre-shrinking and scouring. The scouring agent is first added into the water, and the scouring agent includes: hydrogen peroxide (27.5%): 3.8g / l, caustic soda: 6.0 / l, and refining agent JN-98: 1.7g / l. Then the temperature is raised to 70℃~80℃, and the temperature is kept for 10min~20min. After that, the temperature is raised to 95℃~105℃ and kept for 30min-50min to remove the water-soluble fiber and fully bleach.
[0091] S312, performing hot washing, neutralization and deoxidation according to a conventional pure cotton product treatment process, specifically, washing at 50° C., adjusting the pH value to 6.5 to 7.5, and then performing deoxidation treatment under the condition of 0.001 g / L to 0.01 g / L of deoxidase;
[0092] S314, dyeing is carried out under weak alkaline conditions of pH 10-13, followed by hot water washing and soaping;
[0093] S316, using 80% by mass acetic acid to adjust the pH value to 4.0-6.5, and polishing the terry fabric using a pure cotton cellulase polishing process;
[0094] S318, using hydrophilic softener 3C-3, dosage 3.8g / L, softening finishing at 30℃ for 30min;
[0095] S320, dehydration, opening, loose drying, sewing to obtain the finished terry fabric.
[0096] The terry fabric product prepared in this embodiment has a fluffy and soft feel and is highly resilient. According to the AATCC135 method, the feather shedding rate after 5 washes is less than 5‰. The product has an ultra-soft feel, good resilience, and has a visual appearance similar to that of conventional untwisted products and excellent water absorption. The wastewater pollution in this embodiment is small, the product yield is high, and the production cost is low.
[0097] The finished terry fabric obtained in Example 3 was compared with a conventional untwisted product. The results are shown in Table 4 below.
[0098] Table 4
[0099]
[0100]
[0101] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for producing a fast-absorbing ultra-soft terry fabric, characterized in that: The following steps are involved: (1) Spinning terry yarn: The roving process produces two kinds of rovings with different weights, namely, low-weight water-soluble fiber roving and high-weight roving, and the weight ratio thereof is 1:2 to 1:
4. The high-weight roving is pure cotton roving or roving blended with cotton fiber and other fibers, and the low-weight water-soluble fiber roving is roving blended with water-soluble fiber and cotton fiber or roving blended with water-soluble fiber, cotton fiber and other fibers, wherein the water-soluble fiber is contained in the low-weight water-soluble fiber. The content in the roving is 9%-30%, the quantitative roving of the high quantitative roving is 8g / 5m-10g / 5m, and two rovings with different quantitative are spun on a Siro compact spinning composite spinning frame or a Siro false twisting composite spinning frame to obtain terry yarn, the spinning count of the terry yarn is: single yarn 21S-8S, the twist coefficient is not higher than 279, the kilometer weight of the yarn is 27.8g-72.8g, and the weight ratio of the water-soluble fiber in the terry yarn is 2.5%-5%; (2) Weaving terry fabric: using the terry yarn obtained in step (1) as the wool warp, and cooperating with the pure cotton ground warp or the cotton fiber-containing ground warp and weft yarn on a towel loom to weave a terry fabric, wherein the terry length of the terry fabric is 8.5 cm-13.5 cm / 10 terry loops; (3) Desizing the terry fabric: the terry fabric obtained in step (2) is fed into the cloth along the wool direction and desizing is performed on a padding machine; (4) Pre-shrinking and scouring: After desizing, the terry fabric enters the overflow machine for pre-shrinking and scouring. After entering the water, the scouring agent is first added, and then the temperature is raised to 70℃~80℃, and the temperature is kept for 10min~20min, and then the temperature is raised to 95℃~105℃, and the temperature is kept for 30min~50min; (5) The terry fabric treated in step (4) is dyed, polished, softened, dehydrated, dried, and sewn to obtain a super soft towel product.
2. The method for producing fast water-absorbing super-soft terry fabric according to claim 1, characterized in that: In step (1), a special double-hole bell mouth is arranged on the Siro compact spinning composite spinning frame or the Siro false twisting composite spinning frame, and the special double-hole bell mouth presents an asymmetric double-inlet and single-outlet structure. High-quantity roving and low-quantity water-soluble fiber roving are fed into the special double-hole bell mouth in parallel, and terry yarn is obtained after drawing, twisting and winding.
3. The method for producing the fast water-absorbing super-soft terry fabric according to claim 2, characterized in that: The distance between the two inlet holes in the special double-hole bell mouth is 4mm to 5mm.
4. The method for producing fast water-absorbing super-soft terry fabric according to claim 1, characterized in that: The diameter of the top roller of the back roller of the spinning machine at the end of the low-weight water-soluble fiber roving is increased by 0.5mm-1.0mm compared with the end of the high-weight roving; The spinning frame is provided with a false twist device, which adds false twist to the sliver output by the front roller, changes the fiber distribution on the yarn surface in the twisting triangle area, and controls the yarn twist coefficient.
5. The method for producing a fast water-absorbing super-soft terry fabric according to any one of claims 1 to 4, characterized in that: The process parameters for desizing the terry fabric in step (3) are: The desizing temperature is 50°C to 80°C, the desizing time is not less than 20 minutes, the desizing agent is starch desizing enzyme, and the terry fabric is not dried after desizing.
6. The method for producing the fast water-absorbing super-soft terry fabric according to claim 5, characterized in that: The process parameters for weaving the terry fabric in step (2) are as follows: ground warp density 123 to 160 yarns / 10 cm, weft density 150 to 220 yarns / 10 cm, and terry length 0.85 to 1.35 cm.
7. The method for producing fast water-absorbing super-soft terry fabric according to claim 5, characterized in that: The scouring aids used in the pre-shrinking and scouring process in step (4) include: 27.5% by mass hydrogen peroxide: 3 g / L-8 g / L; caustic soda: 3 g / L-8 g / L; refining agent JN-98: 1 g / L-2.0 g / L.
8. The method for producing fast water-absorbing super-soft terry fabric according to claim 5, characterized in that: Before the dyeing process in step (5), washing is performed with water at 50°C, the pH value is adjusted to 6.5 to 7.5, and then deoxidation treatment is performed under the condition of 0.001 g / L to 0.01 g / L of deoxidase; The dyeing process of step (5) is carried out under weak alkaline conditions with a pH value of 10 to 13, followed by hot water washing and soap washing; The polishing process of step (5) is carried out under the condition of pH value of 4.0 to 6.5, and is adjusted by using 80% by mass acetic acid, and the terry fabric is polished by using pure cotton cellulase polishing process; In the softening process of step (5), a hydrophilic softener 3C-3 is used in an amount of 2 g / L to 5 g / L; In the drying process of step (5), loose drying or vibration drying is adopted.
9. A fast-absorbing ultra-soft terry fabric, characterized in that: The fast-absorbing ultra-soft terry fabric is produced by the production method of any one of claims 1 to 8, wherein the terry yarn is a siro ring-spun yarn, and a low-quantity water-soluble fiber roving is wound on a high-quantity roving, and the weight ratio of the two is 1:2 to 1:
4.
10. The fast water-absorbing super-soft terry fabric according to claim 9, characterized in that: A water guide channel is formed around the terry yarn body.