A temperature-responsive particle gel and preparation method thereof
Through the particle gel with hydrophilic shell and temperature-sensitive core layer structure, the blockage problem caused by the increase in hydrophobic interaction force of traditional temperature-sensitive particle gels at high temperatures is solved, and the fluidity increases with the increase of temperature. It also provides easy-to-modify features, improving its application potential in the field of biomedical science.
Patent Information
- Application Number
- CN202211284951.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-20
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-10-20
AI Technical Summary
Traditional temperature-sensitive particle gels are blocked due to increased hydrophobic interaction force at high temperatures, and the fluidity changes are complex, making them unable to effectively match the actual printing process.
The particle gel adopts hydrophilic shell and thermosensitive core layer structure, and copolymerizes branched polyvinyl macromolecules and thermosensitive polymers to form a temperature-responsive particle gel with volume shrinkage and increased fluidity at high temperatures to avoid The blockage problem of excessive hydrophobic interaction force is conveniently modified through Michael addition reaction.
It effectively improves the fluidity of the granular gel, avoids blockage problems during printing, and provides active double bonds that are easy to modify, enhancing the application value in the fields of tissue engineering and drug delivery.
Smart Images

Figure CN115558133B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a biological particle gel and a preparation method thereof, and in particular to a temperature-responsive particle gel and a preparation method thereof. Background Art
[0002] Granular gel refers to a type of viscoelastic material composed of micron-sized hydrogel particles. Compared with traditional hydrogel block materials, granular gel has the basic characteristics of high water content and good biocompatibility, as well as unique advantages such as shear thinning, high specific surface area, large porosity, and injectability. The volume fraction of hydrogel particles in granular gel materials exceeds 58%, so the hydrogel particles are in close contact and a physical jamming effect occurs. This jamming effect causes the granular gel to appear in a solid form when the external shear force is small; when the external force exceeds a certain threshold, slippage will occur between the hydrogel particles and they begin to show flow characteristics. Based on this principle, a series of granular gel bio-inks have been developed one after another and applied in the fields of tissue engineering and biomedicine.
[0003] The interaction between hydrogel particles in the particle gel has an important influence on the stability of the bioprinting process. When the interaction between particles is too large, the extrusion resistance will be greatly increased and the filament cannot be produced; when the interaction between particles is too small, the particle gel modulus is too low, resulting in collapse or distortion of the printed structure. To solve this problem, researchers have proposed a strategy of printing first and then "welding". For example, microsphere "binders" such as active polymers and metal ions are introduced into the printed structure to further "cross-link" the microsphere particles to improve the mechanical properties of the printed part. In recent years, researchers have also tried to adjust the rheological properties of particle gels by introducing temperature-sensitive materials (Angew. Chem. Int. Ed. 2022, 61, 202114602). This type of thermosensitive particle will shrink in volume at high temperature, reducing its volume fraction in the particle gel. In theory, it can effectively reduce the friction effect and improve the fluidity of the particle gel; however, since the particles are hydrophobic at high temperatures, the hydrophobic interaction force between particles will increase, and even phase separation will occur in extreme cases. Therefore, these two completely opposite effects cause the rheological properties of the particle gel to vary in a complex manner with temperature, which cannot effectively match the actual printing process. Summary of the invention
[0004] Purpose of the invention: The first purpose of the present invention is to provide a temperature-responsive particle gel having a simple positive temperature-sensitive characteristic, and its fluidity increases with increasing temperature, effectively avoiding the problem of hydrophobic-hydrophobic interaction or phase separation between traditional temperature-sensitive hydrogel particles at high temperatures causing clogging of the printing nozzle; The second purpose of the present invention is to provide a method for preparing the temperature-responsive particle gel.
[0005] Technical solution: The temperature-responsive particle gel described in the present invention comprises a hydrophilic shell layer and a thermosensitive core layer, wherein the hydrophilic shell layer is a branched polyvinyl macromolecule; and the thermosensitive core layer is a thermosensitive polymer.
[0006] Preferably, the branched polyvinyl macromolecule is obtained by copolymerization of ethylene glycol polyvinyl monomers or low molecular weight polymers, wherein the ethylene glycol polyvinyl monomers or low molecular weight polymers are one or more of ethylene glycol dimethacrylate, ethylene glycol diacrylate, polyethylene glycol diacrylate, polypropylene glycol diacrylate and polyethylene glycol dimethacrylate. The molecular weight of the branched polyvinyl macromolecule is 10 kDa to 30 kDa.
[0007] The polymerization reaction is atom transfer free radical polymerization, reversible addition / fragmentation chain transfer polymerization or chain transfer termination polymerization, preferably reversible addition / fragmentation chain transfer polymerization.
[0008] Preferably, the thermosensitive polymer is obtained by copolymerization of a monomer or a low molecular weight polymer, and the monomer or the low molecular weight polymer is at least one of isopropyl acrylamide, polyether F127 diacrylate, maleimide-terminated poly (N-isopropyl acrylamide), and N-hydroxysuccinimide ester-terminated poly (N-isopropyl acrylamide).
[0009] Preferably, the average particle size of the constituent units of the granular gel is 5 to 300 μm.
[0010] The method for preparing the temperature-responsive particle gel of the present invention comprises the following steps:
[0011] (1) dissolving the branched polyvinyl macromolecule, the thermosensitive polymer monomer or the low molecular weight polymer, and the initiator in water as the aqueous phase;
[0012] (2) dispersing the water phase in the oil phase to prepare W / O water-in-oil droplets;
[0013] (3) inducing a polymerization reaction of the W / O oil-in-water droplets by heating, irradiation or redox reaction to obtain hydrogel particles;
[0014] (4) The prepared hydrogel particles are concentrated and dispersed in deionized water to obtain a temperature-responsive particle gel.
[0015] Preferably, the initiator is a photoinitiator, a thermal initiator or a redox initiator, the photoinitiator is 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone or phenyl (2,4,6-trimethylbenzoyl) phosphate lithium salt; the thermal initiator is azobisisobutyramidine hydrochloride, ammonium persulfate, potassium persulfate or sodium persulfate; the redox initiator is composed of persulfate and tetramethylethylenediamine.
[0016] Preferably, the oil phase comprises one of vegetable oil, mineral oil, fluorinated oil and silicone oil.
[0017] Preferably, the W / O water-in-oil droplets are prepared by microfluidics, membrane emulsification or mechanical stirring.
[0018] Preferably, the volume fraction of the hydrogel particles in the particle gel is 58%-100%.
[0019] Invention mechanism: The particle gel described in the present invention is obtained by copolymerization with W / O oil-in-water droplets as templates and branched polyvinyl macromolecules and polymer monomers or low molecular weight polymers with thermosensitive properties as main raw materials. Since the branched polyvinyl macromolecules are amphiphilic, they will be enriched on the surface of the W / O oil-in-water droplets, thereby forming a particle gel with a hydrophilic shell layer and a thermosensitive core layer structure. Due to the hydrophilic shell layer and thermosensitive core layer structural characteristics, the particle gel shrinks in volume when it is higher than the critical phase transition temperature of its core layer, the volume fraction of the particle gel decreases, and the jamming effect between particles is weakened; at the same time, the hydrophilic shell layer of the particle gel effectively avoids the occurrence of hydrophobic-hydrophobic interactions between particles. Therefore, the fluidity of the particle gel increases with increasing temperature and decreases with decreasing temperature, and effectively avoids the phase separation caused by excessive hydrophobic effects of traditional thermosensitive particles. In addition, since the branched polyvinyl macromolecules on the surface of the particle gel contain a large number of active double bonds, they can also be conveniently modified by Michael addition reactions.
[0020] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: (1) The particle gel is wrapped with a hydrophilic shell layer outside the thermosensitive core layer, and its fluidity increases with increasing temperature and decreases with decreasing temperature, effectively avoiding the phase separation and clogging problems of traditional thermosensitive particles caused by excessive hydrophobic effect during the printing process; (2) The branched polyvinyl macromolecules on the surface of the particle gel contain a large number of active double bonds, which are easy to modify and convenient for various protein or drug modifications, and have important value in the field of tissue engineering or drug delivery. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a schematic diagram of the preparation principle of the temperature-responsive particle gel of the present invention;
[0022] Figure 2 The chemical structural formula and H-NMR spectrum of the branched polyvinyl macromolecule prepared in Example 1 of the present invention;
[0023] Figure 3 The chemical structural formula and H-NMR spectrum of polyether F127 diacrylate in Example 3;
[0024] Figure 4Microscope images of the particle gel prepared in Example 1 under different temperature conditions;
[0025] Figure 5 This is a macroscopic physical state diagram of the particle gel prepared in Example 1 under different temperature conditions;
[0026] Figure 6 Microscope images of the particle gel prepared in Example 3 under different temperature conditions;
[0027] Figure 7 This is a macroscopic physical state diagram of the particle gel prepared in Example 3 under different temperature conditions;
[0028] Figure 8 This is a test diagram of the hydrophobic-hydrophobic force effect of the particle gel prepared in Example 1 at 45°C;
[0029] Fig. 9 This is a test diagram of the hydrophobic-hydrophobic force effect of the particle gel prepared in Comparative Example 1 at 45°C;
[0030] Fig.10 This is a physical picture of the particle gel extrusion and biological scaffold prepared in Example 2 of the present invention;
[0031] Fig.11 The fluorescence images and fluorescence intensity images of the particle gel prepared in Example 1 of the present invention before and after the reaction with thiolated rhodamine. DETAILED DESCRIPTION
[0032] The technical solution of the present invention is further described below in conjunction with embodiments.
[0033] Example 1
[0034] The temperature-responsive particle gel of the present invention comprises the following steps:
[0035] (1) Preparation of branched polyvinyl macromolecules (HB-PEGDA)
[0036] Add 13.625g of poly(ethylene glycol) diacrylate (PEGDA) monomer into a 250mL three-necked flask, then add 62.5mL of butanone solution, turn on the magnetic stirrer, and rotate at 300rpm until completely dissolved. Then, continue to add 0.296g of tetraethylthiuram disulfide (DS) and 0.295g of 2,2-azobisisobutyronitrile (AIBN). Bubble argon for 1h. After the oxygen is removed, react the solution in the three-necked flask at 70℃ for 10h, and then introduce air to terminate the reaction.
[0037] The structure and NMR results of the synthesized branched polyvinyl macromolecules are shown in Figure 11H NMR (400MHz, Deuterium Oxide) δ4.34–4.28 (m, 1H), 4.25 (s, 1H), 4.13 (s, 8H), 3.82–3.75 (m, 1H), 3.70–3.63 (m, 10H), 1.73 (s, 1H).
[0038] (2) Preparation of precursor solution
[0039] 60 mg of ammonium persulfate (NH4)2S2O8 and 120 mg of branched polyvinyl macromolecule (HB-PEGDA) were dissolved in 2 mL 1×PBS at pH = 7.4 to prepare a dispersed phase A1 with a concentration of 6% (w / v); 280 mg of N-isopropylacrylamide (NIPAAm) was dissolved in 2 mL 1×PBS at pH = 7.4, and 20 μL of tetramethylethylenediamine (TEMED) was added to prepare a dispersed phase A2 with a concentration of 14% (w / v).
[0040] (3) Preparation of temperature-responsive particle gel
[0041] The surfactant (FE-surf) was dissolved in fluorinated oil to prepare a mass fraction of 2%, which was recorded as the continuous phase B1 (oil phase). The solutions A1 and A2 prepared in step (2) were connected to the microfluidic chip through pipes respectively; the flow rate of the oil phase B1 was adjusted to 40 μL / min, the flow rate of the water phase A1 was 4 μL / min, and the flow rate of the water phase A2 was 4 μL / min, and monodispersed droplets were prepared through the microfluidic chip, and the free radical reaction was allowed to occur for 1 hour to solidify the droplets to form hydrogel particles, and the hydrogel particles were washed out and concentrated and dispersed in deionized water to obtain a particle gel with a particle size distribution of 150 to 170 μm (such as Figure 4 a) as shown).
[0042] Example 2
[0043] The temperature-responsive particle gel of the present invention comprises the following steps:
[0044] (1) The preparation of branched polyvinyl macromolecule (HB-PEGDA) was the same as in Example 1.
[0045] (2) Preparation of precursor solution
[0046] 10 mg of phenyl (2,4,6-trimethylbenzoyl) lithium phosphate and 100 mg of branched polyvinyl macromolecule (HB-PEGDA) were dissolved in 1 mL 1×PBS at pH = 7.4 to prepare a dispersed phase A1 with a concentration of 10% (w / v); 280 mg of N-isopropylacrylamide (NIPAAm) was dissolved in 2 mL 1×PBS at pH = 7.4 to prepare a dispersed phase A2 with a concentration of 14% (w / v).
[0047] (3) Preparation of temperature-responsive particle gel
[0048] The surfactant (DOWSIL RSN-0749) was dissolved in dimethyl silicone oil to prepare a mass fraction of 5%, which was recorded as the continuous phase B1 (oil phase). The solutions A1 and A2 prepared in step (2) were connected to the microfluidic chip through pipelines respectively; the flow rate of the oil phase B1 was adjusted to 30 μL / min, the flow rate of the water phase A1 was adjusted to 2 μL / min, and the flow rate of the water phase A2 was adjusted to 2 μL / min, and monodisperse droplets were prepared through the microfluidic chip, and were solidified by blue light irradiation for 30 minutes to form hydrogel particles, and the hydrogel particles were washed out and concentrated and dispersed in deionized water to obtain a particle gel with a particle size distribution of 150 to 170 μm.
[0049] Example 3
[0050] The temperature-responsive particle gel of the present invention comprises the following steps:
[0051] (1) The preparation of branched polyvinyl macromolecule (HB-PEGDA) was the same as in Example 1.
[0052] (2) Preparation of precursor solution
[0053] 120 mg of branched polyvinyl macromolecule (HB-PEGDA) was dissolved in 2 mL of 1×PBS at pH = 7.4 to prepare dispersed phase A1 with a concentration of 6% (w / v), and 60 mg of ammonium persulfate ((NH4)2S2O8) was added; 280 mg of F127-DA) was dissolved in 2 mL of 1×PBS at pH = 7.4, and 20 μL of tetramethylethylenediamine (TEMED) was added to prepare dispersed phase A2 with a concentration of 14% (w / v);
[0054] The NMR images of F127-DA are as follows Figure 3 As shown, 1H NMR (400MHz, Deuterium Oxide) δ3.63 (s, 34H), 3.59–3.46 (m, 3H), 3.39 (ddt, J = 10.4, 5.1, 2.7 Hz, 2H), 3.09 (qd, J = 7.3, 4.8 Hz, 1H), 1.40 (t, J = 7.3 Hz, 2H), 1.25 (s, 2H), 1.23 (t, J = 7.0 Hz, 1H), 1.12 (dd, J = 6.1, 3.3 Hz, 8H). The NMR graph shows that there are peaks at chemical shifts 5-7, which can be judged as chemical shifts of olefins, thereby confirming the existence of double bonds.
[0055] (3) Preparation of temperature-responsive particle gel
[0056] The surfactant (DOWSIL RSN-0749) was dissolved in dimethyl silicone oil to a mass fraction of 5%, which was recorded as the continuous phase B1 (oil phase). The solutions A1 and A2 prepared in step (2) were connected to the microfluidic chip through pipes respectively; the flow rate of the oil phase B1 was adjusted to 40 μL / min, the flow rate of the water phase A1 was 4 μL / min, and the flow rate of the water phase A2 was 4 μL / min to prepare monodisperse droplets, which were solidified for 1 hour to form hydrogel particles, and the hydrogel particles were washed out and dispersed in deionized water to obtain a particle gel with a particle size distribution of 150 to 170 μm. Figure 6 shown.
[0057] Example 4
[0058] The temperature-responsive particle gel of the present invention comprises the following steps:
[0059] (1) Preparation of branched polyvinyl macromolecules (HB-EGDMA)
[0060] Add 4.955g of polyethylene glycol diacrylate (EGDMA) to a 250mL three-necked flask, then add 62.5mL of butanone solution, turn on the magnetic stirrer, and stir at 300rpm until it is completely dissolved. Then, add 0.296g of tetraethylthiuram disulfide (DS) and 0.295g of 2,2-azobisisobutyronitrile (AIBN) to the flask in sequence. Bubble argon for 1h. After the oxygen is removed, react the solution in the three-necked flask at 70℃ for 10h, and then introduce air to terminate the reaction.
[0061] (2) Preparation of precursor solution
[0062] 60 mg of ammonium persulfate (NH4)2S2O8 and 120 mg of branched polyvinyl macromolecule (HB-EGDMA) were dissolved in 2 mL 1×PBS at pH = 7.4 to prepare a dispersed phase A1 with a concentration of 6% (w / v); 20 μL of tetramethylethylenediamine (TEMED) and 280 mg of N-isopropylacrylamide (NIPAAm) were dissolved in 2 mL 1×PBS at pH = 7.4 to prepare a dispersed phase A2 with a concentration of 14% (w / v).
[0063] (3) Preparation of temperature-responsive particle gel
[0064] The fluorinated surfactant (FE-surf) was dissolved in fluorinated oil to prepare a mass fraction of 2%, which was recorded as the continuous phase B1 (oil phase). The solutions A1 and A2 prepared above were connected to the microfluidic chip through pipes respectively; the flow rate of the oil phase B1 was adjusted to 40 μL / min, the flow rate of the water phase A1 was 4 μL / min, and the flow rate of the water phase A2 was 4 μL / min, and monodisperse droplets were prepared through the microfluidic chip, and the free radical reaction was allowed to occur for 1 hour to solidify the droplets to form hydrogel particles, and the hydrogel particles were washed out and dispersed in deionized water to obtain a particle gel with a particle size distribution of 150 to 170 μm.
[0065] Comparative Example 1
[0066] 1. Preparation of particle gel composed of poly (N-isopropylacrylamide) hydrogel microspheres
[0067] On the basis of Example 1, the branched polyvinyl macromolecule was replaced with a cross-linking agent, N,N'-methylenebisacrylamide (MBA).
[0068] Performance Characterization
[0069] (1) Test of the thermosensitive properties of particle gel
[0070] The particle gels with a volume fraction of 58% prepared in Examples 1 and 3 were placed at 25°C and 45°C respectively, and the changes in the particle size of the gel particles were observed under a microscope. Then, the volume fraction of the gel was reduced to 70% by centrifugation, and the state of the gel was observed. The results are as follows: Figures 4 to 7 shown.
[0071] Depend on Figure 4 It can be seen that the particle size of the hydrogel particles prepared in Example 1 shrinks by about 10% at 45°C. The macroscopic physical state of the particle gel at 25°C and 45°C is as follows: Figure 5 As shown, it is further proved that the particle size of hydrogel particles will decrease with increasing temperature.
[0072] Depend on Figure 6 It can be seen that the particle size of the hydrogel particles prepared in Example 3 shrinks by about 10% at 45°C. The macroscopic physical state of the particle gel at 25°C and 45°C is as follows: Figure 7 As shown, it is further proved that the particle size of hydrogel particles will decrease with increasing temperature.
[0073] (2) Test of the hydrophobic-hydrophobic interaction effect of particle gel
[0074] The particle gels with a volume fraction of 58% prepared in Example 1 and Comparative Example 1 were placed at 45°C. The hydrophobic-hydrophobic interaction results of the particle gels were as follows: Figure 8 and 9 shown.
[0075] Depend on Figure 8It can be seen that the particle gel composed of poly (N-isopropylacrylamide) hydrogel microspheres synthesized in Comparative Example 1 undergoes phase separation at 45°C due to the strong hydrophobic-hydrophobic interaction.
[0076] Depend on Fig. 9 It can be seen that the hydrogel particles with a hydrophilic shell prepared in Example 1 can still be well dispersed at 45° C. due to the presence of the hydrophilic shell, and the occurrence of phase separation is effectively suppressed.
[0077] (3) Bioprinting
[0078] The particle gel with a volume fraction of 58% in Example 2 was centrifuged to obtain a particle gel with a volume fraction of 70%, and printed using an extrusion bioprinter, with the printing speed set at 400 mm / min and the extrusion pressure set at 20 psi; then the particle gel in Example 2 was filled into a barrel, and the barrel temperature was increased, and extruded through a 21G needle to construct a biological scaffold. Fig.10 As shown, the particle gel prepared in this embodiment can be smoothly and continuously extruded through an extrusion 3D printer, and can construct a biological scaffold at the same time.
[0079] (4) Testing of double bonds on the particle gel surface
[0080] 2 mg of SH-PEG-Rhodamine was dissolved in 1 mL of PBS, which was recorded as aqueous solution B. 1 mL of PBS was taken as a control group, which was recorded as aqueous solution A. The pH was adjusted to 7.4. 100 mg of the particle gel prepared in Example 1 was placed in the above aqueous solutions (A, B) and incubated for 20 minutes. After the incubation, the excess SH-PEG-Rhodamine solution was washed off with PBS and observed under a fluorescence microscope. The results are as follows Fig.11 shown.
[0081] Depend on Fig.11 It can be seen that the surface of the particle gel in solution A is fluorescent, indicating that SH-PEG-Rhodamine is successfully grafted onto the surface of the particle gel, indicating that the surface of the particle gel contains a large number of active double bonds, which is convenient for subsequent functional modification applications.
Claims
1. A temperature-responsive particle gel, characterized in that: It comprises a hydrophilic shell layer and a thermosensitive core layer, wherein the hydrophilic shell layer is a branched polyvinyl macromolecule, and the thermosensitive core layer is a thermosensitive polymer; the branched polyvinyl macromolecule is obtained by copolymerization of ethylene glycol polyvinyl monomers or low molecular weight polymers, and the ethylene glycol polyvinyl monomers or low molecular weight polymers are one or more of ethylene glycol dimethacrylate, ethylene glycol diacrylate, polyethylene glycol diacrylate, polypropylene glycol diacrylate and polyethylene glycol dimethacrylate; The thermosensitive polymer is obtained by copolymerization of a monomer or a low molecular weight polymer, wherein the monomer or the low molecular weight polymer is at least one of isopropyl acrylamide, polyether F127 diacrylate, maleimide-terminated poly(N-isopropyl acrylamide), and N-hydroxysuccinimide ester-terminated poly(N-isopropyl acrylamide); The preparation method comprises the following steps: (1) dissolving the branched polyvinyl macromolecule, the thermosensitive polymer monomer or the low molecular weight polymer, and the initiator in water as the aqueous phase; (2) dispersing the water phase in the oil phase to prepare W / O water-in-oil droplets; (3) inducing a polymerization reaction of the W / O oil-in-water droplets by heating, irradiation or redox reaction to obtain hydrogel particles; (4) The hydrogel particles are concentrated and dispersed in deionized water to obtain a temperature-responsive particle gel.
2. The temperature-responsive particle gel according to claim 1, characterized in that: The average particle size of the constituent units of the particle gel is 5 to 300 μm.
3. A method for preparing the temperature-responsive particle gel according to claim 1 or 2, characterized in that: The following steps are involved: (1) dissolving the branched polyvinyl macromolecule, the thermosensitive polymer monomer or the low molecular weight polymer, and the initiator in water as the aqueous phase; (2) dispersing the water phase in the oil phase to prepare W / O water-in-oil droplets; (3) inducing a polymerization reaction of the W / O oil-in-water droplets by heating, irradiation or redox reaction to obtain hydrogel particles; (4) The hydrogel particles are concentrated and dispersed in deionized water to obtain a temperature-responsive particle gel.
4. The method for preparing the temperature-responsive particle gel according to claim 3, characterized in that: The initiator is a photoinitiator, a thermal initiator or a redox initiator. The photoinitiator is 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone or phenyl (2,4,6-trimethylbenzoyl) lithium phosphate; the thermal initiator is azobisisobutyramidine hydrochloride, ammonium persulfate, potassium persulfate or sodium persulfate; and the redox initiator is composed of persulfate and tetramethylethylenediamine.
5. The method for preparing the temperature-responsive particle gel according to claim 3, characterized in that: The oil phase includes one of vegetable oil, mineral oil, fluorinated oil and silicone oil.
6. The method for preparing the temperature-responsive particle gel according to claim 3, characterized in that: The W / O water-in-oil droplets are prepared by microfluidics, membrane emulsification or mechanical stirring.
7. The method for preparing the temperature-responsive particle gel according to claim 3, characterized in that: The volume fraction of hydrogel particles in the particle gel is 58% to 100%.