A method for increasing tungsten content and producing calcium sulfate hemihydrate whiskers from scheelite acid decomposition slag
By using hydrochloric acid and sodium sulfate solutions in the decomposition residue of syelitis acid, the tungsten content was successfully improved and high-value calcium sulfate whiskers were produced, which solved the low utilization rate and high cost of tungsten resource in traditional processes. The problem of this achieves efficient recycling of resources and simplification of processes.
Patent Information
- Application Number
- CN202211344113.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-31
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-10-31
AI Technical Summary
When processing low-grade sedative sedative ore, the increase in the tungsten content in the acid decomposition slag leads to a decrease in resource utilization, and the traditional recycling process is costly and complex, making it difficult to effectively improve the tungsten extraction rate.
By stirring the syringogenic acid decomposition residue in hydrochloric acid solution, the tungsten slag and filtrate are separated, the calcium sulfate crystals are cooled down and precipitated, and the calcium sulfate crystals are stirred and aged in the sodium sulfate solution to obtain hemihydrate calcium sulfate whiskers, and tungsten is realized The enrichment and recovery of calcium sulfate reduce raw material costs.
It significantly improves the tungsten content in the acid decomposition slag, simplifies the process flow, reduces costs, and produces high-value calcium sulfate whiskers, with a wide range of industrial application prospects.
Smart Images

Figure CN115595668B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgical waste slag recovery, and in particular to a method for increasing the tungsten content in scheelite acid decomposition slag and simultaneously producing calcium sulfate hemihydrate whiskers and application of the product thereof. Background Art
[0002] The traditional tungsten mineral alkaline decomposition method has high production costs and great environmental pressure. The technology of synergistic treatment of scheelite with sulfuric acid and phosphorus mixed acid came into being. This new technology uses low-cost sulfuric acid as a leaching agent to make tungsten and phosphorus form highly soluble phosphotungstic heteropolyacids that enter the solution, and calcium combines with sulfate to form gypsum slag to achieve the separation of calcium and tungsten. However, due to the influence of tungsten resource endowment, when treating scheelite with low grade and complex composition, the WO3 content in the acid decomposition slag obtained by decomposition increases to more than 1.5%, and the WO3 content in the acid decomposition slag of some difficult-to-treat scheelite even reaches 3%. The substantial increase in tungsten content in the slag significantly reduces the resource utilization rate of valuable metal tungsten. It is difficult to recycle tungsten in the acid decomposition slag by traditional means. Some researchers have used flotation, gravity separation and other means to treat the acid decomposition slag, in order to achieve the recovery and utilization of tungsten resources in the slag through a combination of beneficiation and smelting, but the effect is not obvious and the economic cost is high. Therefore, how to reduce the tungsten content in the acid decomposition slag of such tungsten minerals has become an important issue in the current tungsten extraction metallurgical process.
[0003] Chinese patent CN112899503A discloses a method for treating low-grade scheelite, which comprises adding the low-grade scheelite into dilute hydrochloric acid for pickling to obtain pickling residue and pickling liquid; adding the pickling residue into a hydrochloric acid-phosphoric acid mixed acid solution, stirring and reacting at 70-95°C to obtain a mixed acid decomposition liquid; adding concentrated sulfuric acid into the mixed acid decomposition liquid for reaction, stirring and filtering to obtain high-purity gypsum residue and filtrate, extracting tungsten in the filtrate with a TBP extraction system to obtain a loaded organic phase and a raffinate, and extracting the loaded organic phase with ammonia water to obtain a crude ammonium tungstate solution for subsequent APT production to improve the tungsten extraction rate in the low-grade scheelite; the method requires a large amount of organic solvent, mixed acid and ammonia water, the raw materials are dangerous and consumable, the process is complicated, the cost is high, and only gypsum residue with low market value can be obtained. Summary of the invention
[0004] In order to improve the implementation value of the process of improving the tungsten extraction rate in low-grade scheelite in the prior art and reduce the cost, the present invention provides a method for increasing the tungsten content in the acid decomposition slag of scheelite, which can convert calcium sulfate crystals into calcium sulfate whiskers by a simple process; the present invention also provides a method for increasing the tungsten content from the acid decomposition slag of scheelite and producing hemihydrate calcium sulfate whiskers at the same time, the recovery process is simple, the tungsten content in the acid decomposition slag can be significantly increased for recycling, the raw material cost is low, and hemihydrate calcium sulfate whiskers with high market value can be produced.
[0005] The present invention is achieved by the following technical solutions:
[0006] A method for increasing the tungsten content and producing calcium sulfate hemihydrate whiskers from scheelite acid decomposition slag, comprising the following steps:
[0007] 1) adding the acid decomposition slag of scheelite into a hydrochloric acid solution, stirring for reaction, and then separating the solid and liquid to obtain tungsten slag and filtrate;
[0008] 2) cooling the filtrate prepared in step 1) to precipitate calcium sulfate crystals, and performing solid-liquid separation to obtain the calcium sulfate crystals and mother liquor;
[0009] 3) adding the calcium sulfate crystals prepared in step 2) into a sodium sulfate solution, stirring and aging at 70-95° C., filtering to obtain a filter residue, washing and drying the filter residue to obtain hemihydrate calcium sulfate whiskers.
[0010] The tungsten in the acid decomposition slag of scheelite does not react and remains in the tungsten slag. The hydrochloric acid decomposes the impurities to form metal ions that dissolve in the filtrate. Calcium sulfate has a higher solubility in the filtrate under acidic conditions and at higher temperatures, thereby achieving the enrichment of tungsten in the obtained tungsten slag, which is convenient for the next step of recovery and extraction. The mother liquor separated from the calcium sulfate crystals can be recycled to prepare hydrochloric acid and put back into production, further reducing the cost of raw materials. The obtained hemihydrate calcium sulfate whiskers are fibrous single crystals with many excellent properties such as high strength, high toughness, high insulation, wear resistance, high temperature resistance, acid and alkali resistance, and non-toxicity. It is a new type of inorganic material with a wide application field and broad market prospects. Tungsten slag that can recycle tungsten and high-value calcium sulfate whiskers can be produced simultaneously with a simple process, and the preparation process is more valuable to implement.
[0011] Preferably, the WO3 content in the acid decomposition slag of scheelite in step 1) is 1-3wt%.
[0012] Preferably, in step 1), the mixing ratio of the scheelite acid decomposition slag and the hydrochloric acid solution is 1g:5-10mL, the reaction temperature is 50-95°C, and the time is 1-10h; the concentration of the hydrochloric acid solution is 10-30wt%.
[0013] Preferably, the WO3 content in the tungsten slag in step 1) is 15-25wt%.
[0014] Preferably, in step 2), the filtrate is cooled to 20-25° C. at a cooling rate of 0.5-1° C. / min.
[0015] Preferably, in step 3), the solid-to-liquid ratio of the calcium sulfate crystals to the sodium sulfate solution is 1 g: 1-5 mL.
[0016] Preferably, the concentration of the sodium sulfate solution in step 3) is 100-200 g / L.
[0017] Preferably, the stirring and aging time in step 3) is 5 to 10 hours.
[0018] Preferably, the aspect ratio of the calcium sulfate hemihydrate whiskers in step 3) is greater than or equal to 50.
[0019] The invention discloses an application of tungsten slag prepared by a method of increasing the tungsten content in scheelite acid decomposition slag and producing calcium sulfate hemihydrate whiskers as a tungsten hydrometallurgical raw material.
[0020] Beneficial effects of the present invention:
[0021] (1) The WO3 content in the tungsten slag obtained by soaking the acid decomposition slag of scheelite with hydrochloric acid is increased from 1 to 3 wt% of the original acid decomposition slag of scheelite to 15 to 25 wt% close to the WO3 content in the normal scheelite, and can be used as a raw material for tungsten hydrometallurgy;
[0022] (2) The filtrate obtained by soaking the scheelite acid decomposition slag with hydrochloric acid contains a large amount of calcium sulfate crystals, which are cooled and precipitated and mixed with a sodium sulfate solution to obtain hemihydrate calcium sulfate whiskers, which have high market utilization value. The original scheelite acid decomposition slag can be used to obtain high-value products at a low cost and with a simple process, thus realizing the resource utilization and high-value utilization of the scheelite acid decomposition slag, having a wide range of large-scale industrial promotion value, and having significant economic and ecological benefits;
[0023] (3) The mother liquor from which calcium sulfate crystals are precipitated can be further recycled to prepare a hydrochloric acid solution and put into production again, thereby further reducing the cost of raw materials;
[0024] (4) The aspect ratio of the calcium sulfate hemihydrate whiskers obtained by the present invention is greater than or equal to 50, indicating that the whiskers can still grow smoothly without breaking in the absence of additives to assist crystal growth. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the SEM morphology of calcium sulfate hemihydrate whiskers.
[0026] Figure 2 This is the SEM morphology of the acid decomposition slag of scheelite. DETAILED DESCRIPTION
[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only some embodiments of the present invention, not all. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] Example 1
[0029] A method for recovering tungsten from scheelite acid decomposition slag and producing hemihydrate calcium sulfate whiskers comprises the following steps:
[0030] 1) Adding scheelite acid decomposition slag with a WO3 content of 1.1wt% to a hydrochloric acid solution, stirring for reaction, and then separating the solid and liquid to obtain tungsten slag and filtrate; the mixing ratio of scheelite acid decomposition slag and hydrochloric acid solution is 1g:5mL, the concentration of hydrochloric acid solution is 10wt%, the reaction temperature is 50℃, and the reaction time is 1h;
[0031] 2) cooling the filtrate prepared in step 1) to 20° C. at a rate of 0.5° C. / min to precipitate calcium sulfate crystals, and performing solid-liquid separation to obtain calcium sulfate crystals and mother liquor;
[0032] 3) adding the calcium sulfate crystals prepared in step 2) to the sodium sulfate solution, stirring and aging at 70° C., filtering to obtain a filter residue, washing and drying the filter residue to obtain hemihydrate calcium sulfate whiskers; the solid-liquid ratio of the calcium sulfate crystals to the sodium sulfate solution is 1 g:1 mL, and the concentration of the sodium sulfate solution is 100 g / L.
[0033] Example 2
[0034] A method for recovering tungsten from scheelite acid decomposition slag and producing hemihydrate calcium sulfate whiskers comprises the following steps:
[0035] 1) Adding scheelite acid decomposition slag with a WO3 content of 3wt% into a hydrochloric acid solution, stirring for reaction, and then separating the solid and liquid to obtain tungsten slag and filtrate; the mixing ratio of scheelite acid decomposition slag and hydrochloric acid solution is 1g:10mL, the concentration of hydrochloric acid solution is 30wt%, the reaction temperature is 95℃, and the reaction time is 10h;
[0036] 2) cooling the filtrate prepared in step 1) to 25° C. at a rate of 1° C. / min to precipitate calcium sulfate crystals, and performing solid-liquid separation to obtain calcium sulfate crystals and mother liquor;
[0037] 3) adding the calcium sulfate crystals prepared in step 2) to the sodium sulfate solution, stirring and aging at 95° C., filtering to obtain a filter residue, washing and drying the filter residue to obtain hemihydrate calcium sulfate whiskers; the solid-liquid ratio of the calcium sulfate crystals to the sodium sulfate solution is 1 g:5 mL, and the concentration of the sodium sulfate solution is 200 g / L.
[0038] Example 3
[0039] A method for recovering tungsten from scheelite acid decomposition slag and producing hemihydrate calcium sulfate whiskers comprises the following steps:
[0040] 1) Adding scheelite acid decomposition slag with a WO3 content of 2.4wt% to a hydrochloric acid solution, stirring for reaction, and then separating the solid and liquid to obtain tungsten slag and filtrate; the mixing ratio of scheelite acid decomposition slag and hydrochloric acid solution is 1g:7.5mL, the concentration of hydrochloric acid solution is 20wt%, the reaction temperature is 72.5℃, and the reaction time is 5.5h;
[0041] 2) cooling the filtrate prepared in step 1) to 22.5° C. at a rate of 0.75° C. / min to precipitate calcium sulfate crystals, and performing solid-liquid separation to obtain calcium sulfate crystals and mother liquor;
[0042] 3) adding the calcium sulfate crystals prepared in step 2) to the sodium sulfate solution, stirring and aging at 82.5° C., filtering to obtain a filter residue, washing and drying the filter residue to obtain hemihydrate calcium sulfate whiskers; the solid-liquid ratio of the calcium sulfate crystals to the sodium sulfate solution is 1 g:3 mL, and the concentration of the sodium sulfate solution is 150 g / L.
[0043] Example 4
[0044] A method for recovering tungsten from scheelite acid decomposition slag and producing hemihydrate calcium sulfate whiskers comprises the following steps:
[0045] 1) Adding scheelite acid decomposition slag with a WO3 content of 1.5wt% to a hydrochloric acid solution, stirring for reaction, and then separating the solid and liquid to obtain tungsten slag and filtrate; the mixing ratio of scheelite acid decomposition slag and hydrochloric acid solution is 1g:8mL, the concentration of hydrochloric acid solution is 25wt%, the reaction temperature is 76°C, and the reaction time is 8h;
[0046] 2) cooling the filtrate prepared in step 1) to 21.5° C. at a rate of 0.4° C. / min to precipitate calcium sulfate crystals, and performing solid-liquid separation to obtain calcium sulfate crystals and mother liquor;
[0047] 3) adding the calcium sulfate crystals prepared in step 2) to the sodium sulfate solution, stirring and aging at 87° C., filtering to obtain a filter residue, washing and drying the filter residue to obtain hemihydrate calcium sulfate whiskers; the solid-liquid ratio of the calcium sulfate crystals to the sodium sulfate solution is 1 g:4 mL, and the concentration of the sodium sulfate solution is 175 g / L.
[0048] Example 5
[0049] A method for recovering tungsten from scheelite acid decomposition slag and producing hemihydrate calcium sulfate whiskers comprises the following steps:
[0050] 1) Adding scheelite acid decomposition slag with a WO3 content of 2.1wt% to a hydrochloric acid solution, stirring for reaction, and then separating the solid and liquid to obtain tungsten slag and filtrate; the mixing ratio of scheelite acid decomposition slag and hydrochloric acid solution is 1g:6.5mL, the concentration of hydrochloric acid solution is 28wt%, the reaction temperature is 89°C, and the reaction time is 9h;
[0051] 2) cooling the filtrate prepared in step 1) to 24.5° C. at a rate of 0.4° C. / min to precipitate calcium sulfate crystals, and performing solid-liquid separation to obtain calcium sulfate crystals and mother liquor;
[0052] 3) adding the calcium sulfate crystals prepared in step 2) to the sodium sulfate solution, stirring and aging at 82° C., filtering to obtain a filter residue, washing and drying the filter residue to obtain hemihydrate calcium sulfate whiskers; the solid-liquid ratio of the calcium sulfate crystals to the sodium sulfate solution is 1 g:4 mL, and the concentration of the sodium sulfate solution is 180 g / L.
[0053] Example 6
[0054] A method for recovering tungsten from scheelite acid decomposition slag and producing hemihydrate calcium sulfate whiskers comprises the following steps:
[0055] 1) Adding scheelite acid decomposition slag with a WO3 content of 1.8wt% to a hydrochloric acid solution, stirring for reaction, and then separating the solid and liquid to obtain tungsten slag and filtrate; the mixing ratio of scheelite acid decomposition slag and hydrochloric acid solution is 1g:7mL, the concentration of hydrochloric acid solution is 22wt%, the reaction temperature is 90℃, and the reaction time is 10h;
[0056] 2) cooling the filtrate prepared in step 1) to 23° C. at a rate of 0.6° C. / min to precipitate calcium sulfate crystals, and performing solid-liquid separation to obtain calcium sulfate crystals and mother liquor;
[0057] 3) adding the calcium sulfate crystals prepared in step 2) to the sodium sulfate solution, stirring and aging at 79° C., filtering to obtain a filter residue, washing and drying the filter residue to obtain hemihydrate calcium sulfate whiskers; the solid-liquid ratio of the calcium sulfate crystals to the sodium sulfate solution is 1 g:3.5 mL, and the concentration of the sodium sulfate solution is 170 g / L.
[0058] Comparative Example 1
[0059] The difference from Example 3 is that the hydrochloric acid in step 1) is replaced by sulfuric acid.
[0060] Comparative Example 2
[0061] The difference from Example 3 is that in step 1), the mixing ratio of the scheelite acid decomposition slag and the hydrochloric acid solution is 1 g:1 mL.
[0062] Comparative Example 3
[0063] The difference from Example 3 is that in step 1), the reaction temperature of the scheelite acid decomposition slag and the hydrochloric acid solution is 30°C.
[0064] Comparative Example 4
[0065] The difference from Example 3 is that the cooling rate in step 2) is 5°C / min.
[0066] Comparative Example 5
[0067] The difference from Example 3 is that the sodium sulfate in step 3) is replaced by sodium acetate.
[0068] Comparative Example 6
[0069] The difference from Example 3 is that in step 3), the reaction temperature of the calcium sulfate crystals and the sodium sulfate solution is 55°C.
[0070] Comparative Example 7
[0071] The difference from Example 3 is that in step 3), the mixing ratio of calcium sulfate crystals to sodium sulfate solution is 1 g:0.5 mL.
[0072] Comparative Example 8
[0073] The difference from Example 3 is that the concentration of the sodium sulfate solution in step 3) is 50 g / L.
[0074] Detection Methods
[0075] The tungsten slag obtained in step 1) was analyzed by X-ray fluorescence spectrometry (XRF) to detect the tungsten content, and the morphology of the final product was analyzed by SEM. The mass of the calcium sulfate hemihydrate whiskers was weighed and divided by the mass of the acid decomposition slag of the raw scheelite in step 1) to calculate the yield, and the data in Table 1 and Figure 2 .
[0076] Table 1 Tungsten content in tungsten slag, morphology and yield of calcium sulfate hemihydrate whiskers
[0077]
[0078]
[0079] As shown in Table 1, the tungsten content of the tungsten slag obtained in each embodiment is between 15% and 25%, and hemihydrate calcium sulfate whiskers are obtained with a high yield of 50% to 60%, and the aspect ratio of the whiskers is more than 50; in Comparative Example 1, after the hydrochloric acid in step 1) is replaced by sulfuric acid, the tungsten content of the tungsten slag obtained after the acid decomposition slag is acid-decomposed is reduced by more than 1 / 3. Obviously, sulfuric acid cannot fully dissolve impurities like hydrochloric acid, and there are too many impurities in the tungsten slag, the enrichment degree of tungsten decreases, and the yield of hemihydrate calcium sulfate whiskers is also reduced, but the aspect ratio of the whiskers increases slightly; in Comparative Example 2, the amount of hydrochloric acid is insufficient, the acid decomposition slag cannot be fully dissolved, the impurities in the tungsten slag are too much, the enrichment degree of tungsten decreases, and the yield of hemihydrate calcium sulfate whiskers is seriously reduced, and more calcium sulfate remains in the tungsten slag without dissolving, and the aspect ratio of the whiskers is not affected; in Comparative Example 3, the reaction temperature of the acid decomposition slag and the hydrochloric acid is too low, the dissolution effect of the acid decomposition slag is not good, the impurities in the obtained tungsten slag are too much, the enrichment degree of tungsten decreases, and the hemihydrate calcium sulfate whiskers The yield is seriously reduced, the temperature is not enough to dissolve more calcium sulfate, and more calcium sulfate remains in the tungsten slag, and the aspect ratio of the whiskers is not affected; the cooling rate in step 2) in comparative example 4 is too high, and the tungsten content in the tungsten slag is not affected, but because the supersaturation of calcium sulfate changes too much, the directional growth of the crystals cannot be controlled. After the calcium sulfate crystals are precipitated, they are mixed with the sodium sulfate solution, and whiskers with a qualified aspect ratio cannot be generated; the sodium sulfate in step 3) in comparative example 5 is replaced by sodium acetate, which will reduce the solubility of the calcium sulfate crystals in the solution, and whiskers with a qualified aspect ratio cannot be generated, and the whisker yield is low; the reaction temperature of the calcium sulfate crystals and the sodium sulfate solution in comparative example 6 is low, and the conditions for whisker growth cannot be achieved, and no hemihydrate calcium sulfate whiskers can be obtained; in comparative example 7, there is too little sodium sulfate solution, and some calcium sulfate crystals cannot be converted into whiskers, and the product is a mixture of block crystals and whiskers; the concentration of the sodium sulfate solution in comparative example 8 is too low, and the conditions for whisker growth cannot be achieved, and no hemihydrate calcium sulfate whiskers can be obtained.
[0080] like Figure 2 As shown in the figure, the acid decomposition slag of the raw scheelite is in block shape under SEM. Figure 1 SEM images of calcium sulfate hemihydrate whiskers show that they have a longer aspect ratio.
[0081] It should be noted that, for those skilled in the art, several modifications and improvements can be made without departing from the concept of the present invention, and these modifications and improvements all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for increasing the tungsten content and producing calcium sulfate hemihydrate whiskers from the acid decomposition slag of scheelite, It is characterized in that The following steps are involved: 1) adding the acid decomposition slag of scheelite into a hydrochloric acid solution, stirring for reaction, and then separating the solid and liquid to obtain tungsten slag and filtrate; 2) cooling the filtrate prepared in step 1) to precipitate calcium sulfate crystals, and performing solid-liquid separation to obtain the calcium sulfate crystals and mother liquor; 3) adding the calcium sulfate crystals prepared in step 2) to a sodium sulfate solution, stirring and aging at 70-82.5° C., filtering to obtain a filter residue, washing and drying the filter residue to obtain hemihydrate calcium sulfate whiskers; the concentration of the sodium sulfate solution is 100-200 g / L; the solid-liquid ratio of the calcium sulfate crystals to the sodium sulfate solution is 1 g:1-5 mL; the aspect ratio of the hemihydrate calcium sulfate whiskers is greater than or equal to 50; the filtrate in step 2) is cooled to 20-25° C., and the cooling rate is 0.5-1° C. / min.
2. A method for increasing the tungsten content and producing calcium sulfate hemihydrate whiskers from scheelite acid decomposition slag according to claim 1, It is characterized in that The WO in the scheelite acid decomposition slag in step 1) 3 The content is 1 to 3 wt%.
3. A method for increasing the tungsten content and producing calcium sulfate hemihydrate whiskers from scheelite acid decomposition slag according to claim 1, It is characterized in that In step 1), the mixing ratio of the scheelite acid decomposition slag and the hydrochloric acid solution is 1g:5-10mL, the reaction temperature is 50-95°C, and the time is 1-10h; the concentration of the hydrochloric acid solution is 10-30wt%.
4. A method for increasing the tungsten content and producing calcium sulfate hemihydrate whiskers from the acid decomposition slag of scheelite according to any one of claims 1 to 2, It is characterized in that WO in the tungsten slag in step 1) 3 The content is 15-25wt%.
5. A method for increasing the tungsten content and producing calcium sulfate hemihydrate whiskers from the acid decomposition slag of scheelite according to any one of claims 1 to 2, It is characterized in that The stirring and aging time in step 3) is 5 to 10 hours.